Water-based UPR emulsion applied to asphalt pavement pothole interface bonding and preparation method of water-based UPR emulsion

Through the application of aqueous UPR emulsion, the use of unsaturated polyester resin and emulsifier components, the problem of low interface bonding strength of asphalt pavement pit grooves in the prior art is solved, and high strength and durability interface bonding is achieved. Prevent cracking of the interface after pits and grooves are repaired.

CN118956316APending Publication Date: 2024-11-15SHAANXI TRAFFIC CONTROL OPERATION MANAGEMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410830272.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-25
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

When the prior art uses the cold repair method to repair asphalt pavement pits, the emulsified asphalt interface bonding material has a slow strength and low bonding force, which can easily lead to cracking of the pit and groove interface and affect the stability and durability of the pavement.

Method used

A water-based UPR emulsion is prepared by unsaturated polyester resin, emulsifier and initiator, and has excellent bonding properties and is used for the interface bonding of asphalt pavement pit grooves, including components A, components B and The emulsifier is compounded with sodium dodecyl sulfate and alkylphenol polyoxyethylene ether, the initiator is benzoyl peroxide, the accelerator is N,N dimethylaniline, the component ratio is 100:(1.5~2.5):(0.75~1.25).

Benefits of technology

It significantly improves the interface bonding strength and durability after pit and groove repair, prevents interface cracking, and is simple in preparation, low in cost, good emulsion stability, can penetrate and cover the pit and groove interface quickly, and the pulling strength reaches more than 0.6MPa , the shear strength reaches 1.0MPa or above.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118956316A_ABST
    Figure CN118956316A_ABST
Patent Text Reader

Abstract

The invention discloses a water-based UPR emulsion applied to asphalt pavement pit interface bonding and a preparation method thereof.The water-based UPR emulsion is prepared from a component A, a component B and a component C. The component A comprises unsaturated polyester resin, an emulsifier and water; the component B is an initiator; the component C is an accelerant; the mass ratio of the component A to the component B to the component C is 100: (1.5-2.5): (0.75-1.25); the mass ratio of the unsaturated polyester resin to the emulsifier to the water is 100: (5-9): (50-100); the emulsifying agent is an emulsifying agent formed by compounding lauryl sodium sulfate (SDS) and alkylphenol polyoxyethylene ether (TX-10); according to the present invention, the compounding mass ratio of SDS to TX-10 is 1: (10-17), the aqueous UPR emulsion has excellent adhesion performance, can enhance the interface adhesion between the pit slot repair material and the original pavement, and can effectively prevent the cracking of the interface after the pit slot repair, and the preparation method is simple.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of road construction materials for highway engineering, and relates to an aqueous UPR emulsion used for bonding the interface of a pothole on an asphalt road surface and a preparation method thereof. Background Art

[0002] In recent years, with the improvement of my country's social and economic level, the traffic volume has increased. Under the influence of repeated traffic loads and external climate environment, the diseases of asphalt pavement have become increasingly prominent. Potholes, as one of the main diseases, are a major problem in highway maintenance. Due to their existence, surface water on the road can seep down, which not only weakens the adhesion between asphalt and aggregate, but also seriously reduces the bearing capacity of the road surface, affecting the overall stability and durability of the highway. In addition, potholes will directly affect the flatness of the road surface, reduce the service level of the road surface, and even endanger the driving safety of drivers. Therefore, it is very necessary to repair potholes on the road surface in a timely manner.

[0003] Cold patching is widely used in pothole repair because it can be constructed all day, is less affected by temperature and weather, is simple to construct, and is energy-saving and environmentally friendly. However, in actual projects, cold patching mostly uses emulsified asphalt interface adhesives to bond the new and old interfaces of potholes, which has slow strength formation and low bonding force. Under the influence of vehicle loads and the environment, it is very easy to cause cracks in the pothole interface. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide an aqueous UPR emulsion used for bonding the interface of potholes in asphalt pavements and a preparation method thereof. The aqueous UPR emulsion has excellent bonding properties, can strengthen the interface bonding between the pothole repair material and the original road surface, effectively prevent cracking of the interface after pothole repair, and the preparation method is relatively simple.

[0005] To achieve the above-mentioned purpose, the present invention discloses an aqueous UPR emulsion used for bonding the interface of potholes in asphalt pavement, which is prepared by component A, component B and component C, wherein component A includes unsaturated polyester resin, emulsifier and water; component B is an initiator; and component C is a accelerator.

[0006] The mass ratio of component A, component B and component C is 100:(1.5-2.5):(0.75-1.25).

[0007] The mass ratio of unsaturated polyester resin, emulsifier and water is 100:(5-9):(50-100).

[0008] The emulsifier is a compound emulsifier of sodium dodecyl sulfate (SDS) and alkylphenol polyoxyethylene ether (TX-10).

[0009] The mass ratio of SDS to TX-10 is 1:(10~17).

[0010] The initiator is benzoyl peroxide (BPO).

[0011] The accelerator is N,N dimethylaniline (DMA).

[0012] The invention discloses a method for preparing an aqueous UPR emulsion used for bonding an asphalt pavement pothole interface, comprising the following steps:

[0013] 1) heating the emulsifier and the unsaturated polyester resin to make them easy to flow, and then mixing the unsaturated polyester resin and the emulsifier and stirring them to obtain a mixture;

[0014] 2) heating the mixture obtained in step 1) and continuing stirring, and adding water within a preset emulsification time to obtain component A;

[0015] 3) Component A, component B and component C are mixed and stirred evenly to obtain a water-based UPR emulsion for bonding the interface of potholes in asphalt pavement.

[0016] The heating temperature in step 2) is 40°C to 70°C;

[0017] The stirring speed is 500r / min~1000r / min.

[0018] The preset emulsification time in step 2) is 20 min to 40 min.

[0019] The present invention has the following beneficial effects:

[0020] The aqueous UPR emulsion and preparation method thereof applied to the asphalt pavement pothole interface bonding of the present invention are in specific operation, and the unsaturated polyester resin has excellent mechanical properties, heat resistance and chemical corrosion resistance such as water, acid and alkali. The unsaturated polyester resin is used as the raw material to prepare the emulsion, and the mechanical properties such as bonding performance and durability of the pothole interface bonding material can be obtained. In addition, the emulsifier has a better resin emulsification effect, the emulsion has good stability, a long shelf life, and good fluidity, and can better cover the pothole interface and penetrate into the inside of the pothole interface more quickly. After testing, the pull-out strength of the aqueous UPR emulsion obtained by the present invention and the Marshall asphalt mixture specimen reaches more than 0.6MPa, and the shear strength of the Marshall asphalt mixture specimen reaches more than 1.0MPa. In addition, when preparing, basically adopt more conventional means, i.e. heating, stirring and mixing, the preparation method is relatively simple, low cost, and in actual operation, the heating temperature, stirring rate and stirring time can be adjusted to better emulsify the resin, and the obtained emulsion storage stability is longer. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1a This is the particle size distribution diagram of the aqueous UPR emulsion obtained in Example 1;

[0022] Figure 1b This is the particle size distribution diagram of the aqueous UPR emulsion obtained in Example 2;

[0023] Figure 1c This is the particle size distribution diagram of the aqueous UPR emulsion obtained in Example 3;

[0024] Figure 2 This is the structural diagram of the Marshall composite specimen;

[0025] Figure 3 This is the structural diagram of the shear composite specimen. DETAILED DESCRIPTION

[0026] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiment of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiment of the present invention. Obviously, the described embodiment is only an embodiment of a part of the present invention, not all embodiments, and is not intended to limit the scope of the present invention. In addition, in the following description, the description of well-known structures and technologies is omitted to avoid unnecessary confusion of the concepts disclosed in the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work should fall within the scope of protection of the present invention.

[0027] The accompanying drawings show schematic diagrams of structures according to embodiments disclosed in the present invention. These figures are not drawn to scale, and some details are magnified and some details may be omitted for the purpose of clear expression. The shapes of various regions and layers shown in the figures and the relative sizes and positional relationships therebetween are only exemplary, and may deviate in practice due to manufacturing tolerances or technical limitations, and those skilled in the art may additionally design regions / layers with different shapes, sizes, and relative positions according to actual needs.

[0028] Embodiment 1

[0029] The preparation method of the aqueous UPR emulsion used for bonding the pothole interface of asphalt pavement described in this embodiment comprises the following steps:

[0030] 1) Heat the emulsifier and unsaturated polyester resin in an oven to reduce the viscosity and make it easy to flow, then dissolve SDS in TX-10 according to the mass ratio of SDS:TX-10=1:13 to obtain the emulsifier; weigh the unsaturated polyester resin and emulsifier according to the mass ratio of 100:7 and put them into a three-necked flask, start the stirrer and stir at a low speed to fully mix the two;

[0031] 2) Raise the heating temperature to 50° C. and increase the stirring rate to 800 r / min. Add water dropwise to the flask at a mass ratio of unsaturated polyester resin to water of 100:80 within 30 minutes of emulsification to obtain component A.

[0032] 3) Component A, component B and component C are mixed in a mass ratio of 100:2:1, and the agitator is started to stir and mix evenly to obtain a water-based UPR emulsion for bonding the interface of potholes in asphalt pavement.

[0033] Embodiment 2

[0034] The difference between Example 2 and Example 1 is that the mass ratio of SDS to TX-10 is 1:10.

[0035] Embodiment 3

[0036] The difference between Example 3 and Example 1 is that the mass ratio of SDS to TX-10 is 1:17.

[0037] Embodiment 4

[0038] The difference between Example 4 and Example 1 is that the mass ratio of unsaturated polyester resin to emulsifier is 100:5.

[0039] Embodiment 5

[0040] The difference between Example 5 and Example 1 is that the mass ratio of unsaturated polyester resin to emulsifier is 100:9.

[0041] Embodiment 6

[0042] The difference between Example 6 and Example 1 is that the mass ratio of unsaturated polyester resin to water is 100:50.

[0043] Embodiment 7

[0044] The difference between Example 7 and Example 1 is that the mass ratio of unsaturated polyester resin to water is 100:100.

[0045] Embodiment 8

[0046] The difference between Example 8 and Example 1 is that the mass ratio of component A, component B and component C is 100:1:0.75.

[0047] Embodiment 9

[0048] The difference between Example 9 and Example 1 is that the mass ratio of component A, component B and component C is 100:1.5:0.75.

[0049] Embodiment 10

[0050] The difference between Example 1 and Example 1 is that the mass ratio of component A, component B and component C is 100:2.5:1.25.

[0051] Embodiment 11

[0052] The difference between Example 1 and Example 1 is that the stirring rate is 500 r / min.

[0053] Embodiment 12

[0054] The difference between Example 1 and Example 1 is that the stirring rate is 1000 r / min.

[0055] Embodiment 13

[0056] The difference between the thirteenth embodiment and the first embodiment is that the heating temperature is 40°C.

[0057] Embodiment 14

[0058] The difference between Example 14 and Example 1 is that the stirring rate is 60°C.

[0059] Embodiment 15

[0060] The difference between Example 1 and Example 1 is that the stirring rate is 70°C.

[0061] Embodiment 16

[0062] The difference between Example 1 and Example 1 is that the time for uniformly adding water to the flask is 20 minutes.

[0063] Embodiment 17

[0064] The difference between Example 1 and Example 1 is that the time for uniformly adding water to the flask is 40 minutes.

[0065] Comparative Example 1

[0066] The difference between Comparative Example 1 and Example 1 is that the emulsifier is an emulsifier prepared by compounding sodium dodecyl sulfate (hereinafter referred to as SDBS) and TX-10, and the mass ratio is SDBS:TX-10=1:1.

[0067] Comparative Example 2

[0068] The difference between Comparative Example 2 and Comparative Example 1 is that the mass ratio of the emulsifiers SDBS and TX-10 is SDBS:TX-10=1:2.

[0069] Comparative Example 3

[0070] The difference between Comparative Example 3 and Comparative Example 1 is that the mass ratio of the emulsifiers SDBS and TX-10 is SDBS:TX-10=1:3.

[0071] Comparative Example 4

[0072] Comparative Example 4 is ordinary emulsified asphalt, and its technical indicators are shown in Table 1.

[0073] Table 1

[0074]

[0075] Comparative Example 5

[0076] Comparative Example 5 is SBS emulsified asphalt, and its technical indicators are shown in Table 2.

[0077] Table 2

[0078]

[0079]

[0080] The aqueous UPR emulsions prepared in Examples 1 to 5 and Comparative Examples 1 to 3 were subjected to a phase volume ratio test to measure the dispersion uniformity and performance stability of the emulsions.

[0081] Test method: prepare two 25ml measuring cylinders, a medical syringe and a 20% calcium sulfate solution, number the prepared aqueous UPR emulsions in sequence, and then place them in a constant temperature water bath at 35°C for 1h, and then take them out for use; use a syringe to take out 20g from the upper and lower layers of the emulsion in sequence, and then inject them into the two prepared 25ml measuring cylinders respectively, and add 8ml of 20wt% calcium sulfate solution, then put them back into the constant temperature water bath, heat them to 90°C, and heat until the oil phase and the water phase are completely separated; according to the scale value of the measuring cylinder, read the oil phase volume of the two parts of the sample in sequence, and record them as V 上 、V 下 , calculate the relative volume ratio V of the oil phase in the upper and lower parts of the sample 上 / V 下 .

[0082] The phase volume ratio test results of the aqueous UPR emulsions prepared in Examples 1 to 5 and Comparative Examples 1 to 3 are shown in Table 3.

[0083] Table 3 shows the phase volume ratio test results of the aqueous UPR emulsions prepared in Examples 1 to 5 and Comparative Examples 1 to 3.

[0084] Table 3

[0085]

[0086] By comparing the test results of Example 1 to Example 3 and Comparative Example 1 to Comparative Example 3, it can be seen that the emulsification effect of the SDS / TX-10 compound emulsifier is significantly better than that of the SDBS / TX-10 compound emulsifier, the stability of the aqueous UPR emulsion emulsified by the SDS / TX-10 compound emulsifier is better, and the storage stability of the emulsion is longer. Therefore, the present invention selects the SDS / TX-10 compound emulsifier as the emulsifier of the aqueous UPR emulsion; at the same time, it can also be found that with the increase of the content of TX-10 emulsifier in the SDS / TX-10 compound emulsifier, the emulsification stability of the emulsion shows a trend of first increasing and then decreasing, and the optimal ratio is SDS:TX-10=1:13. Therefore, the optimal ratio of the SDS / TX-10 compound emulsifier selected by the present invention is SDS:TX-10=1:13.

[0087] By comparing the test results of Example 1, Example 4 and Example 5, it can be seen that with the increase of the emulsifier content, the emulsification effect of the emulsion first improves and then deteriorates, and the optimal emulsifier dosage is 7%. Therefore, the present invention selects the optimal ratio of unsaturated polyester resin to emulsifier in the emulsion as 100:7.

[0088] Laser particle size analysis was performed on the aqueous UPR emulsions prepared in Example 1, Example 6 and Example 7 to measure the effect of the amount of water in the emulsion on the dispersed particle size of the emulsion.

[0089] Test method: According to the “Particle Size Distribution Laser Diffraction Method” (GB / T 19077-2016), Beckman Coulter LS13 320 micro-nano laser particle size analyzer was used for testing. Deionized water was used as the dispersant, ultrasonic dispersion was performed for 1 minute, and then the prepared aqueous UPR emulsion was tested.

[0090] The particle size distribution of the aqueous UPR emulsion prepared in Example 1, Example 6 and Example 7 is as follows: Figure 1a , Figure 1b and Figure 1c shown.

[0091] from Figure 1a , Figure 1b and Figure 1c It can be seen that as the water content in the emulsion increases, the emulsion particle size changes from large to small and then to large. When the water content is 80%, the emulsion particle size is the smallest and the dispersion effect is the best. Therefore, the present invention determines that the optimal mass ratio of unsaturated polyester resin to water in the aqueous UPR emulsion is 100:80.

[0092] The aqueous UPR emulsions prepared in Example 1 and Example 8 to Example 10 were subjected to a pull-out test to measure the effect of the ratio of components A, B and C in the emulsion on the bonding properties of the emulsion.

[0093] Test method: Add the emulsion at 0.5kg / m 2 Sprinkle the amount of the coating evenly on the drawing head and stick it on a 10cm×10cm×0.5cm steel plate. The drawing specimen is placed at room temperature for curing for 24 hours, and then its pulling strength is measured.

[0094] The pull-out test results of the aqueous UPR emulsions prepared in Example 1 and Example 8 to Example 10 are shown in Table 4.

[0095] Table 4

[0096] Test indicators Embodiment 1 Embodiment 8 Embodiment 9 Embodiment 10 Tensile strength (MPa) 1.2 0.8 1.0 1.2

[0097] It can be seen from Table 4 that with the increase of the content of component B and component C, the pull-out strength of the emulsion gradually increases and then tends to be stable. When the dosage of component B and component C reaches 2% and 1% respectively, the pull-out strength of the emulsion tends to the maximum value of 1.2MPa. Therefore, the present invention determines that the optimal ratio of each component in the emulsion is the mass ratio of component A, component B and component C = 100:2:0.75.

[0098] The aqueous UPR emulsions prepared in Example 1, Example 11 and Example 12 were subjected to a storage stability test to measure the effect of the emulsion preparation parameter stirring rate on the emulsion dispersion effect.

[0099] Test method: The storage stability of the emulsion is determined according to the test method for emulsion storage stability in "Test method for properties of medium and high viscosity emulsions of surfactants and evaluation method for their emulsification ability" (GB / T 11543-2008).

[0100] The storage stability test results of the aqueous UPR emulsions prepared in Example 1, Example 11 and Example 12 are shown in Table 5.

[0101] Table 5

[0102] Test indicators Embodiment 1 Embodiment 11 Embodiment 12 Appearance Unstratified Layering Layering Storage stability (d) >6 5 6

[0103] As can be seen from Table 5, at stirring rates of 500 r / min and 1000 r / min, the aqueous UPR emulsions prepared in Example 11 and Example 12 showed stratification within 5 to 6 days, while at a stirring rate of 800 r / min, the aqueous UPR emulsion prepared in Example 1 did not show stratification within 6 days, indicating that with the increase of the stirring rate, the stability of the prepared emulsion first gradually improved and then deteriorated. Therefore, the present invention determines that the optimal stirring rate for emulsion preparation is 800 r / min.

[0104] The aqueous UPR emulsions prepared in Example 1 and Example 13 to Example 15 were subjected to a storage stability test to measure the effect of the emulsion preparation parameter heating temperature on the emulsion dispersion effect.

[0105] Test method: The storage stability of the emulsion is determined according to the test method for emulsion storage stability in "Test method for properties of medium and high viscosity emulsions of surfactants and evaluation method for their emulsification ability" (GB / T 11543-2008).

[0106] The storage stability test results of the aqueous UPR emulsions prepared in Example 1 and Example 13 to Example 15 are shown in Table 6.

[0107] Table 6

[0108] Test indicators Embodiment 1 Embodiment 13 Embodiment 14 Embodiment 15 Appearance Unstratified Layering Layering Layering Storage stability (d) >4 1 4 1

[0109] It can be seen from Table 6 that with the increase of heating temperature, the storage stability of the prepared emulsion first improves and then deteriorates, and the optimal heating temperature is 50°C. Therefore, the present invention determines that the optimal heating emulsification temperature for emulsion preparation is 50°C.

[0110] The aqueous UPR emulsions prepared in Example 1, Example 16 and Example 17 were subjected to a storage stability test to measure the effect of the emulsification time, a parameter of the emulsion preparation, on the dispersion effect of the emulsion.

[0111] Test method: The storage stability of the emulsion is determined according to the test method for emulsion storage stability in "Test method for properties of medium and high viscosity emulsions of surfactants and evaluation method for their emulsification ability" (GB / T 11543-2008).

[0112] The storage stability test results of the aqueous UPR emulsions prepared in Example 1, Example 16 and Example 17 are shown in Table 7.

[0113] Table 7

[0114] Test indicators Embodiment 1 Embodiment 16 Embodiment 17 Appearance Unstratified Layering Layering Storage stability (d) >8 7 8

[0115] It can be seen from Table 7 that as the emulsification time increases, the storage stability of the prepared emulsion first improves and then deteriorates, and the optimal emulsification time is 30 min. Therefore, the present invention determines that the optimal emulsification time for emulsion preparation is 30 min.

[0116] Marshall composite specimen pulling and shearing tests were performed on Example 1, Comparative Example 4 and Comparative Example 5 to compare the bonding performance of the aqueous UPR emulsion with other interface adhesives.

[0117] Marshall composite specimen pull-out test method: AC-13 Marshall asphalt mixture specimens and rutting plates are molded according to the "Test Procedures for Asphalt and Asphalt Mixtures in Highway Engineering" (JTGE20-2011). Figure 2Assemble the composite specimen; then perform the Marshall composite specimen pull-out test according to the following steps: (1) Take out the prepared composite core specimen, apply AB glue on the top and bottom surfaces of the core specimen respectively, then fix one end to the rutting plate and connect the other end to the metal pulling head. (2) Take out the pulling instrument, connect the pulling instrument and the pulling head, start the pulling instrument, start the pulling test, and record the maximum pulling force F (kN) when the specimen is destroyed. (3) Calculate the pull-out strength σ according to the formula σ = F / S, where S is the force-bearing area, mm 2 .

[0118] Marshall composite specimen shear test method: AC-13 Marshall asphalt mixture specimens were formed according to the "Test Procedures for Asphalt and Asphalt Mixtures in Highway Engineering" (JTGE20-2011). Figure 3 Combine the composite shear specimens; then perform the Marshall composite specimen shear test according to the following steps: (1) Take out the composite specimen, fix the composite specimen with a clamp, start the instrument, start the oblique shear test, and record the maximum shear force P (kN) at the time of test failure. (2) Calculate the shear strength τ according to the formula τ = Psinα / A, where α is the angle between the vertical axis of the specimen and the horizontal plane, °; A is the stress area of ​​the specimen, mm 2 .

[0119] The Marshall composite specimen pulling and shearing test results of Example 1, Comparative Example 4 and Comparative Example 5 are shown in Table 8.

[0120] Table 8

[0121] Test indicators Embodiment 1 Comparative Example 4 Comparative Example 5 Tensile strength (MPa) 0.62 0.18 0.21 Shear strength(MPa) 1.0 0.3 0.4

[0122] It can be seen from Table 8 that the pull-out and shear strengths of the aqueous UPR emulsion prepared in the present invention and the Marshall composite specimen are significantly higher than those of the currently commonly used emulsified asphalt and SBS modified emulsified asphalt interface binders, and the present invention has excellent bonding properties, can more effectively bond the pit interface, and prevent cracking after the pit is repaired.

[0123] Water immersion and freeze-thaw Marshall composite specimen shear tests were performed on Example 1, Comparative Example 4 and Comparative Example 5 to compare the durability of the water-based UPR emulsion and other interface adhesives.

[0124] Immersed Marshall composite specimen shear test method: According to the "Highway Engineering Asphalt and Asphalt Mixture Test Code" (JTG E20-2011), AC-13 Marshall asphalt mixture specimens were formed. Figure 3Combine composite specimens; then perform a Marshall shear test on the immersed composite specimens according to the following steps: (1) Place the composite specimen in a 45°C constant temperature water bath and soak for 3 days. (2) Take out the composite specimen, fix the composite specimen with a clamp, start the instrument, start the oblique shear test, and record the maximum shear force P (kN) at the time of test failure. (3) Calculate the shear strength τ according to the formula τ = Psinα / A, where α is the angle between the vertical axis of the specimen and the horizontal plane, °; A is the stress-bearing area of ​​the specimen, mm 2 (4) The shear strength τ of the immersed composite specimen 浸 Divided by the shear strength τ of the original composite specimen 原 , and obtain the intensity ratio R (%).

[0125] Freeze-thaw Marshall composite specimen shear test method: AC-13 Marshall asphalt mixture specimens were formed according to the "Test Procedures for Asphalt and Asphalt Mixtures in Highway Engineering" (JTG E20-2011). Figure 3 Assemble the composite specimens; then conduct the immersed Marshall composite specimen shear test according to the following steps: (1) Place the specimen in a constant temperature water bath at 25°C and soak for 8 hours, then take it out and place it in a freezer at -10°C for 8 hours, and finally place it in a constant temperature water bath at 25°C and soak it for 8 hours. This is one freeze-thaw cycle, and perform three freeze-thaw cycles. (2) Take out the composite specimen, fix the composite specimen with a clamp, start the instrument, start the oblique shear test, and record the maximum shear force P (kN) at the time of test failure. (3) Calculate the shear strength τ according to the formula τ = Psina / A, where α is the angle between the vertical axis of the specimen and the horizontal plane, °; A is the force-bearing area of ​​the specimen, mm 2 (4) The shear strength τ of the composite specimen after freeze-thaw 冻融 Divided by the shear strength τ of the original composite specimen 原 , and obtain the intensity ratio R (%).

[0126] The results of the immersion and freeze-thaw Marshall composite specimen shear tests of Example 1, Comparative Example 4 and Comparative Example 5 are shown in Table 9.

[0127] Table 9

[0128] Test indicators Embodiment 1 Comparative Example 4 Comparative Example 5 Strength ratio of immersed specimens (%) 90 80 82 Freeze-thaw specimen strength ratio (%) 82 64 68

[0129] As can be seen from Table 9, the water-based UPR emulsion prepared by the present invention has significantly higher water damage resistance and freeze-thaw resistance than the currently commonly used emulsified asphalt and SBS modified emulsified asphalt interface binders, and its bonding performance is less affected by the environment, has excellent durability, and can bond the pit interface for a longer time to prevent cracking after the pit is repaired.

[0130] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the specific implementation methods of the present invention can still be modified or replaced by equivalents. Any modification or equivalent replacement that does not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.

Claims

1. A water-based UPR emulsion used for bonding the interface of asphalt road potholes. It is characterized in that It is prepared by component A, component B and component C, wherein component A includes unsaturated polyester resin, emulsifier and water; component B is an initiator; and component C is an accelerator.

2. The aqueous UPR emulsion for bonding the pothole interface of asphalt pavement according to claim 1, It is characterized in that The mass ratio of component A, component B and component C is 100:(1.5-2.5):(0.75-1.25).

3. The aqueous UPR emulsion for bonding the pothole interface of asphalt pavement according to claim 1, It is characterized in that The mass ratio of unsaturated polyester resin, emulsifier and water is 100:(5-9):(50-100).

4. The aqueous UPR emulsion for bonding the pothole interface of asphalt pavement according to claim 1, It is characterized in that The emulsifier is a compound emulsifier of sodium dodecyl sulfate (SDS) and alkylphenol polyoxyethylene ether (TX-10).

5. The aqueous UPR emulsion for bonding the pothole interface of asphalt pavement according to claim 4, It is characterized in that The mass ratio of SDS to TX-10 is 1:(10~17).

6. The aqueous UPR emulsion for bonding the pothole interface of asphalt pavement according to claim 1, It is characterized in that The initiator is benzoyl peroxide (BPO).

7. The aqueous UPR emulsion for bonding the pothole interface of asphalt pavement according to claim 1, It is characterized in that The accelerator is N,N dimethylaniline (DMA).

8. A method for preparing the aqueous UPR emulsion for bonding the pothole interface of asphalt pavement according to claim 1, It is characterized in that The following steps are involved: 1) heating the emulsifier and the unsaturated polyester resin to make them easy to flow, and then mixing the unsaturated polyester resin and the emulsifier and stirring them to obtain a mixture; 2) heating the mixture obtained in step 1) and continuing stirring, and adding water within a preset emulsification time to obtain component A; 3) Component A, component B and component C are mixed and stirred evenly to obtain a water-based UPR emulsion for bonding the interface of potholes in asphalt pavement.

9. The method for preparing the aqueous UPR emulsion for bonding the pothole interface of asphalt pavement according to claim 8, It is characterized in that The heating temperature in step 2) is 40°C to 70°C; The stirring speed is 500r / min~1000r / min.

10. The method for preparing the aqueous UPR emulsion for bonding the pothole interface of asphalt pavement according to claim 8, It is characterized in that The preset emulsification time in step 2) is 20 min to 40 min.