MOF in-situ derived oxide semiconductor material, gas sensor and preparation method of MOF in-situ derived oxide semiconductor material
By using MOF in-situ derived oxide semiconductor material ZnO/In2O3 composite material, a heterostructure with a matching band structure is constructed, which solves the problem of the reduction in sensitivity of NO2 gas-sensitive sensors under ultraviolet light irradiation, and achieves high sensitivity and low detection Extreme NO2 detection performance, suitable for low concentration NO2 detection in room temperature environment.
Patent Information
- Application Number
- CN202411021861.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-15
AI Technical Summary
The sensitivity of existing NO2 gas-sensitive sensors is significantly reduced under ultraviolet light irradiation, making it difficult to effectively detect low-concentration NO2 gases.
The MOF in-situ derived oxide semiconductor material ZnO/In2O3 composite material is used as the sensitive layer. By constructing a heterostructure that matches the energy band structure, ultraviolet light excitation is used to form rich photogenerated carriers and effectively separate them, improving sensing performance.
It realizes high sensitivity, low detection limit and fast response NO2 detection, has good long-term stability and moisture resistance, and is suitable for low concentration NO2 detection in room temperature environments.
Smart Images

Figure CN118961815A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of gas sensors and relates to a semiconductor material, a gas sensitive sensor and a preparation method thereof, and in particular to a MOF in-situ derived oxide semiconductor material, a gas sensitive sensor and a preparation method thereof. Background Art
[0002] Gas sensors are considered to be one of the most effective detection strategies due to their high sensitivity, fast response speed, simple preparation, good stability and good reproducibility. They are widely used in industrial safety, environmental monitoring, food safety, medical diagnosis and other fields, especially for detecting explosive, flammable and toxic gases. The World Health Organization (WMO) database in April 2022 showed that billions of people still breathe unhealthy air, among which NO2 gas is associated with decreased lung function, increased respiratory symptoms, asthma and premature death. The health and safety rule alert mentioned that the human body cannot stay in an environment with 3ppm NO2 for more than 8 hours. At the same time, long-term exposure to NO2 concentrations above 0.1ppm can damage the respiratory and cardiovascular systems and even pose a risk of cancer. Therefore, the development of excellent NO2 gas sensors plays a key role in industrial waste gas monitoring. Under ultraviolet light irradiation, single-component indium oxide generates photogenerated carriers, but most photogenerated electrons and holes tend to recombine rapidly, resulting in a significant decrease in the sensitivity of pure indium oxide NO2 gas sensors. In order to improve this problem, constructing semiconductor heterostructures with matching band structures is an effective way to improve carrier separation. Among them, ZnO not only has a band structure that matches that of In2O3, but also has excellent ultraviolet absorption properties. Therefore, constructing an In2O3 / ZnO heterojunction may be a feasible solution to effectively separate UV-excited electron-hole pairs and greatly improve the sensing performance under UV light irradiation. Summary of the invention
[0003] To solve the above problems, the present invention provides a MOF in-situ derived oxide semiconductor material, a gas sensor and a preparation method thereof. The sensor of the present invention is based on a ZnO / In2O3 composite material, has high sensitivity and selectivity, a low detection limit, a fast response, good long-term stability, and moisture-resistant gas-sensitive properties, and is expected to be used for low-concentration NO2 detection in room temperature environments.
[0004] The technical solution adopted by the present invention is as follows:
[0005] A method for preparing a MOF in-situ derived oxide semiconductor material comprises the following steps:
[0006] (1) dispersing indium nitrate hydrate in dimethylformamide, stirring, adding terephthalic acid, further stirring evenly, heating, washing and drying the obtained product after the reaction is completed to obtain MOF-In;
[0007] (2) adding MOF-In to methanol, ultrasonically dispersing, then adding zinc nitrate hexahydrate and dimethylimidazole, stirring evenly, and after the reaction is completed, washing and drying the obtained product to obtain a MOF-In / MOF-Zn composite material;
[0008] (3) Grinding the obtained MOF-In / MOF-Zn composite material into powder, and calcining to obtain the MOF in-situ derived oxide semiconductor material.
[0009] Furthermore, in step (1), the mass volume ratio of the indium nitrate hydrate to dimethylformamide is 2:1 to 3:1 mg / mL; and the mass ratio of the indium nitrate hydrate to terephthalic acid is 1:1.
[0010] Furthermore, in step (1), the heating method is an oil bath method, the temperature is 100-120° C., and the time is 1-2 h.
[0011] Furthermore, in step (1), the washing is performed by centrifugal washing three times with ethanol; and the drying is performed by vacuum drying.
[0012] Furthermore, in step (2), the atomic ratio of indium to zinc is 1:1 to 1:3; the concentration of zinc nitrate hexahydrate after stirring is 1:1 to 3:1 mg / mL; the volume ratio of the amount of dimethylimidazole to methanol is 1:1 to 1:2 mmol / mL, and this concentration can ensure that MOF-Zn can better adhere to the surface of MOF-In.
[0013] Furthermore, in step (2), the washing is performed by centrifugation three times with methanol to remove unnecessary organic and inorganic impurity ions; and the drying is performed by vacuum drying.
[0014] Furthermore, in step (2), the reaction temperature is room temperature and the reaction time is 1 to 3 hours.
[0015] Furthermore, in step (3), the calcination parameters are: heating rate 1°C / min, calcination time 1 to 3 hours, and calcination temperature 350 to 450°C. This temperature can ensure that after the MOF is calcined, the remaining ZnO / In2O3 composite material retains its original complete structure.
[0016] A MOF in-situ derived oxide semiconductor material is prepared by the above method, wherein the MOF is MOF-In (MIL-68) / MOF-Zn (ZIF-8), the oxide semiconductor material is indium oxide composite zinc oxide, the indium oxide is a microrod structure, that is, a rod-shaped structure with a diameter and a length both in the micrometer order, the zinc oxide is a nanoparticle structure, and the zinc oxide nanoparticles are attached to the surface of the indium oxide microrod structure.
[0017] A gas sensor uses the above MOF in-situ derived oxide semiconductor material as a sensitive layer material, and the gas sensor can be used for NO2 detection in room temperature environment.
[0018] Preparation of gas sensors and gas detection:
[0019] The MOF in-situ derived oxide semiconductor material was dispersed in a small amount of anhydrous ethanol to form a paste slurry in agate mortar, which was subsequently deposited on an Au ceramic interdigital electrode to construct a sensor. The obtained samples were subjected to gas-sensitive measurements and detected using the intelligent gas-sensitive analysis system CGS-MT. A certain amount of NO2 or dry air was alternately filled in the test chamber, and a gas-liquid distribution system DGL-V with automatic humidity control was used. In a typical test, the humidity was dynamically controlled by a dual-flow dynamic humidity generator DHD-Ⅱ. The response value is defined as the resistance R of the gas sensor in the target gas NO2 environment. g Resistor R against air background a Experiments have shown that the MOF in-situ derived oxide semiconductor material is used for selective detection of NO2 at room temperature, with a response value of 79.5 for 5 ppm NO2 and a response time of 20 s.
[0020] The beneficial effects of the present invention are as follows:
[0021] (1) The MOF in-situ derived oxide semiconductor material proposed in the present invention is used as a gas-sensitive material with a high surface area and abundant oxygen vacancies. Its unique nanostructure can effectively shorten the gas diffusion path and induce more reversible active adsorption / reaction sites, making an important contribution to accelerating the redox reaction and achieving ultra-sensitive response to NO2. At the same time, through ultraviolet light excitation, abundant photogenerated carriers (i.e., holes and electrons) are formed inside the In2O3 / ZnO sensitive layer. The photogenerated holes and electrons can be effectively separated by the internal electric field, thereby improving the room temperature gas-sensitive performance.
[0022] (2) The preparation method of the present invention is simple and controllable, with mild process conditions, low energy consumption, short production cycle, low equipment requirements, and no pollution to the environment. The preparation method is simple and low in cost, and is suitable for large-scale preparation.
[0023] (3) The gas sensor made of MOF in-situ derived oxide semiconductor material provided by the present invention can test low concentration NO2 gas at room temperature. The response value of the synthesized heterostructure ZnO / In2O3 sensor to NO2 gas is as high as (S=79.5,5ppm), which is about 8 times higher than that of the pure In2O3 sensor, and the response speed is 20s. In addition, the sensor based on ZnO / In2O3 has good selectivity and long-term stability of more than 60 days. The sensor based on ZnO / In2O3 has a high response value and a low detection limit (5.2ppb) at low concentrations, and can be used for room temperature NO2 detection.
[0024] (4) The MOF in-situ derived oxide semiconductor material provided by the present invention is expected to be used for low-concentration NO2 detection in room temperature environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a schematic diagram of the preparation process of the NO2 detection composite material in an embodiment of the present invention.
[0026] Figure 2 It is the XRD diffraction pattern of pure In2O3, pure ZnO and ZnO / In2O3 composite material in the embodiment of the present invention.
[0027] Figure 3 3 and 4 are SEM images of pure In2O3 (a), pure ZnO (b) and ZnO / In2O3 composite material (c) in the embodiments of the present invention.
[0028] Figure 4 The following are transmission electron microscope photograph (a), high-resolution transmission microscope photograph (b), selected area electron diffraction pattern (c), and energy dispersion spectrum elemental diagram (d) of the ZnO / In2O3 composite material in the embodiment of the present invention.
[0029] Figure 5 The following are the dynamic response curves of the ZnO / In2O3 sensor to 5ppm NO2 with (without) ultraviolet light irradiation at room temperature in an embodiment of the present invention (a), the response / recovery curve of the ZnO / In2O3 sensor to 5ppm NO2 under the condition of ultraviolet light (b), the dynamic response curve of the ZnO / In2O3 sensor to 0.3-5ppm NO2 gas at room temperature (c), and the curve of the change of response value with NO2 concentration (d).
[0030] Figure 6 The repeatability curve of the ZnO / In2O3 based sensor in the embodiment of the present invention at 25% RH at room temperature in a 5ppm NO2 environment (a) and the selectivity of the ZnO / In2O3 based sensor to 5ppm NO2 and various interfering gases (b). DETAILED DESCRIPTION
[0031] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and specific embodiments.
[0032] Example 1
[0033] Synthesis of sensitive layer materials and preparation of gas sensors:
[0034] (1) Dissolve 0.2 g In(NO3)3·4.5H2O and 0.2 g terephthalic acid in 80 mL dimethylformamide (DMF) and stir evenly for 30 min.
[0035] (2) Transfer the above solution to an oil bath, seal the beaker, and heat at 120°C for 1 hour.
[0036] (3) The mixture was cooled naturally, washed with ethanol three times, the white precipitate was collected by centrifugation, and dried in an oven at 70°C for 10 h to obtain MIL-In powder.
[0037] (4) Add 0.27 mmol of MIL-68 to 30 ml of methanol and stir vigorously for 30 min.
[0038] (5) Disperse 0.5 mmol Zn(NO3)2·6H2O and 2 mmol 2-methylimidazole in the above methanol solution, stir vigorously for 20 min, and leave at room temperature for 4 h.
[0039] (6) After the reaction is completed, the supernatant is separated by centrifugation. The precipitate is then washed three times with methanol to remove residual organic and inorganic impurity ions. The washed product is vacuum dried at 70° C. for at least 24 hours to obtain a MOF-In / MOF-Zn composite material.
[0040] (7) The MOF-In / MOF-Zn composite material was ground into a uniform powder in an agate mortar, placed in a tube furnace, and calcined at 400 °C for 2 h at a heating rate of 1 °C / min to obtain a ZnO / In2O3 composite material, i.e., a MOF in-situ derived oxide semiconductor material. The preparation process is as follows: Figure 1 shown.
[0041] (8) The ZnO / In2O3 composite material and the calcined pure In2O3 were dispersed in a small amount of anhydrous ethanol, respectively, and slurried by ultrasonic grinding, and then coated on the interdigital electrodes and dried to prepare a sensor.
[0042] (9) Finally, the prepared sensor was heated at 70 °C for 12 h to age the sensor.
[0043] Gas Sensitivity Test:
[0044] The obtained samples were subjected to gas-sensitive measurements using an intelligent gas-sensitive analysis system: a micro-multifunctional detection station CGS-MT for detection. A certain amount of NO2 or dry air was alternately filled into the cavity, as well as a gas-liquid distribution system DGL-V that automatically controls humidity. During operation, the test device is first placed in the center of the heating table to stabilize its resistance under air atmosphere. In a typical test, nitrogen is first introduced into the pneumatic valve to open the valve in the device. Humidity is dynamically controlled by a dual-flow dynamic humidity generator DHD-Ⅱ. The response value is defined as the resistance R of the gas sensor in the target gas NO2 environment. g With the resistance R against the air background a The response time and recovery time are defined as the time required for the resistance value to change by 90% during the response and recovery processes.
[0045] Result analysis:
[0046] (1) XRD analysis: The crystal structures of pure In2O3, ZnO and ZnO / In2O3 composite materials were studied by XRD. Figure 2 As shown, there is a weak XRD peak of ZnO in the ZnO / In2O3 composite material, which corresponds to the (101) lattice plane of ZnO, which is consistent with the standard card (PDF#75-0576). The diffraction peaks of pure In2O3 and ZnO / In2O3 composite materials correspond to the (211), (222), (400), (440) and (622) lattice planes of cubic In2O3, respectively, which are consistent with the standard card (PDF#71-2194).
[0047] (2) SEM and TEM analysis: Analyze the morphology, composition and element types of In2O3, ZnO and ZnO / In2O3 composite materials. Figure 3 (a) SEM image of In2O3 shows that the shape of In2O3 microrods is hexagonal, with a length of about 3.5μm and a width of 1μm. After calcination, the hexagonal structure is well preserved. Figure 3 (b) is the SEM image of ZnO particles. The morphology and size of pure ZnO nanoparticles are uniform. After calcination, the structure is well preserved. The particles are poorly dispersed and agglomerated, which may be detrimental to the diffusion and transmission of gas molecules. Figure 3 (c)) and TEM images ( Figure 4 a) shows that MOF-derived ZnO is well attached to In2O3 microrods. The structure does not show any obvious collapse during the sintering process. Figure 4The high-resolution TEM image of ZnO / In2O3 in (b) shows that there are two highly crystalline structures with interplanar spacings of 0.292nm and 0.247nm, corresponding to the lattice planes (222) of In2O3 and (101) of ZnO, respectively. It is worth noting that in the ZnO / In2O3 SEM, it can be seen that a large number of nanoparticles of ZnO are uniformly grown on the surface of the In2O3 microrods. There are many pores between the particles formed by the fracture of the metal organic framework, which provide channels for gas transport and adsorption sites for gas adsorption. In addition, the selected area electron diffraction pattern ( Figure 4 (c)) shows multiple diffraction rings, corresponding to the lattice planes (222) of In2O3 and (101) of ZnO. Combining the SAED pattern and EDX mapping image ( Figure 4 (d)), it can be found that In, Zn and O are uniformly distributed in the ZnO / In2O3 composite material.
[0048] (3) Gas-sensing properties: Figure 5 As shown in (a), the ZnO / In2O3 sensor shows an immediate increase in resistance when exposed to an environment containing NO2; when the sensor enters the air environment, the resistance value decreases and gradually recovers. The sensor has a low response under natural light and a negligible recovery time, which may seriously affect the practical application of these sensors. At room temperature, the ZnO / In2O3 sensor has a response value of 79.5 for 5ppm NO2. Figure 5 As shown in (b), at room temperature, the response time and recovery time of the ZnO / In2O3 sensor to 5 ppm NO2 are 20 / 40s. Figure 5 (c) shows the dynamic response curve of the sensor prepared at room temperature to 0.3-5ppm NO2 gas. The response values of the ZnO / In2O3-based sensor to 0.3, 0.5, 0.8, 1, 3 and 5ppm NO2 concentrations are 4.53, 7.73, 13.07, 18.40, 53.60 and 79.5, respectively. Figure 5 (d) shows the function fit of NO2 concentration and response value at the optimal working temperature, indicating that there is a linear relationship at low concentrations. According to the formula LOD = 3RMS noise / m is used to evaluate the detection limit (LOD) of the sensor in practical applications, where m is the slope of the calibration curve, RMS noise is the rms noise. The LOD of the ZnO / In2O3 based sensor is 5.2ppb.
[0049] Figure 6(a) Shows the repeatability of the ZnO / In2O3 sensor at 5ppm NO2 concentration during six cycles of air-NO2-air exposure process at room temperature. It can be observed that the response to NO2 gas remains consistent, the response of the fabricated sensor remains constant and exhibits reversible and stable characteristics during each cyclic exposure, and the changes over the six cycles are small for high and low NO2 concentrations, indicating that the sensor has good repeatability. The gas selectivity of the ZnO / In2O3 based sensor was studied by exposure to 5ppm NO2 or interfering gases such as hydrogen, methane, hydrogen sulfide, acetone, ammonia, triethylamine, ethanol, and toluene. Figure 6 As shown in (b), the sensor based on ZnO / In2O3 has the best response to NO2, which is 25 times that of other interfering gases. Figure 6 (c) shows the long-term stability of the ZnO / In2O3-based sensor to 5 ppm NO2 at room temperature. The response of the sensor did not change significantly over 30 days and remained in a stable range. The response changed very slightly over the following 30 days, which may be due to changes in the environment (temperature or air).
[0050] The embodiments described above provide a detailed description of the technical solutions and beneficial effects of the present invention. It should be understood that the above are only specific embodiments of the present invention and are not intended to limit the present invention. Any modifications, supplements and equivalent substitutions made within the scope of the principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a MOF in-situ derived oxide semiconductor material, It is characterized in that The following steps are involved: (1) dispersing indium nitrate hydrate and terephthalic acid in dimethylformamide, stirring for a period of time, heating, and washing and drying the obtained product after the reaction is completed to obtain MOF-In; (2) adding MOF-In to methanol, ultrasonically dispersing, then adding zinc nitrate hexahydrate and dimethylimidazole, stirring evenly, and after the reaction is completed, washing and drying the obtained product to obtain a MOF-In / MOF-Zn composite material; (3) Grinding the obtained MOF-In / MOF-Zn composite material into powder, and calcining to obtain the MOF in-situ derived oxide semiconductor material.
2. The preparation method according to claim 1, It is characterized in that In step (1), the mass volume ratio of the indium nitrate hydrate to dimethylformamide is 2:1 to 3:1 mg / mL; the mass ratio of the indium nitrate hydrate to terephthalic acid is 1:
1.
3. The preparation method according to claim 1, It is characterized in that In step (1), the heating method is an oil bath method, the temperature is 100-120° C., and the time is 1-2 hours.
4. The preparation method according to claim 1, It is characterized in that In step (1), the washing is performed by centrifugal washing three times with ethanol; and the drying is performed by vacuum drying.
5. The preparation method according to claim 1, It is characterized in that In step (2), the atomic ratio of indium to zinc is 1:1 to 1:3; the concentration of zinc nitrate hexahydrate after stirring is 1:1 to 3:1 mg / mL; and the volume ratio of the amount of dimethylimidazole to methanol is 1:1 to 1:2 mmol / mL.
6. The preparation method according to claim 1, It is characterized in that In step (2), the washing is performed by centrifugal washing three times with methanol; and the drying is performed by vacuum drying.
7. The preparation method according to claim 1, It is characterized in that In step (2), the reaction temperature is room temperature and the reaction time is 1 to 3 hours.
8. The preparation method according to claim 1, It is characterized in that In step (3), the calcination parameters are: heating rate 1°C / min, calcination time 1 to 3 hours, and calcination temperature 350 to 450°C.
9. A MOF in-situ derived oxide semiconductor material, It is characterized in that The method according to any one of claims 1 to 8 is used to prepare the MOF in-situ derived oxide semiconductor material, wherein the MOF in-situ derived oxide semiconductor material is indium oxide composite zinc oxide, the indium oxide is a microrod structure, and the zinc oxide is a nanoparticle structure.
10. A gas sensor, It is characterized in that The MOF in-situ derived oxide semiconductor material as claimed in claim 9 is used as a sensitive layer material.
Citation Information
Cited By
Preparation and use method of MOF-derived AuRu-In2O3 gas-sensitive material with UV-assisted sensitization
CN119534561A
MOF-derived In2O3-CeO2 composite material based on adsorption cotton template, gas sensor, preparation and application
CN122187117A