Resistive random access memory based on strontium stannate resistive film and preparation method and packaging method thereof

By using strontium stannate as a resistive film material and polydimethylsiloxane packaging technology, the problem of perovskite resistive film material being easily dehydrated is solved, the stability and performance of the resistive memory are improved, and the higher storage density and read and write speed.

CN118973373APending Publication Date: 2024-11-15GUANGDONG UNIV OF TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411183260.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the prior art, perovskite resistance film materials are prone to dehydration, resulting in poor stability of resistance memory, which limits its application.

Method used

Strontium stannate (SrSnO3) is used as the resist film material, and a strontium stannate resist film is prepared by spin-coating the strontium stannate precursor solution on the surface of FTO or ITO conductive glass and annealing, and depositing gold, platinum or silver electrodes on its surface. , combined with the packaging method of polydimethylsiloxane, improve the stability of the memory.

Benefits of technology

Strontium stannate resistive film materials show higher stability, can quickly switch between low-resistance state and high-resistance state, and maintain the state for a long time, with a concentrated switch ratio, reducing the impact of the external environment on the memory, and improving Memory performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118973373A_ABST
    Figure CN118973373A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of memory devices, and particularly relates to a resistive random access memory based on a strontium stannate resistive thin film, a preparation method and a packaging method. The resistive random access memory comprises a top electrode, a bottom electrode and a strontium stannate resistive thin film, the strontium stannate resistive thin film is arranged between the top electrode and the bottom electrode, the strontium stannate resistive thin film is an oxide of a perovskite structure, and compared with a traditional resistive thin film of the perovskite structure, the stability is better, and deliquescence is not likely to happen; meanwhile, after the resistive random access memory based on the strontium stannate resistive random access film is packaged by using polydimethylsiloxane, the adverse effect of the external environment on the resistive random access memory can be reduced, and the performance of the resistive random access memory is improved, so that the technical problem that the stability of the resistive random access memory is relatively poor due to the fact that a perovskite resistive random access film material is easy to deliquesce in the prior art is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of memory devices, and in particular relates to a resistive memory based on a strontium stannate resistive film, and a preparation method and a packaging method thereof. Background Art

[0002] With the exponential growth of Internet big data and the vigorous development of artificial intelligence technology, the reading, writing and running speed of the memory and central processing unit of the traditional von Neumann system may not keep up with the development speed of information technology in the era of data explosion in the future due to the barrier limitation of the "storage wall"; the huge amount of data requires the next generation of non-volatile memory technology to have a larger storage space and speed. Among them, resistive random access memory (RRAM) is regarded as a potential non-volatile memory technology. Compared with traditional memory, resistive random access memory (RRAM) can provide higher storage density, faster reading and writing speed and lower power consumption. Resistive random access memory (RRAM) has sub-nanosecond switching speed, low programming energy consumption and long write / erase endurance, and is expected to solve key problems in traditional computer architecture.

[0003] Resistive random access memory (RRAM) is usually based on resistive random access thin film materials. According to the filament model, its working mechanism can be seen as that under the condition of an applied voltage, the resistive random access thin film material located between the two electrodes forms and breaks a conductive filament, switching back and forth between a high resistance state and a low resistance state. Placing the resistive random access thin film material between the two electrodes is the basic structure of resistive random access memory (RRAM); perovskite film is a potential material for resistive random access thin film materials in resistive random access memory (RRAM), with advantages such as high switching ratio, fast high-low resistance switching speed and low turn-on voltage, showing great research and application potential.

[0004] However, conventional perovskite resistive switching thin film materials currently have the defect of easy deliquesce, which may lead to the degradation or loss of non-volatile performance, seriously affecting the reliability and durability of information stored in resistive random access memory (RRAM). The stability of resistive random access memory (RRAM) is poor, which limits the application of resistive random access memory (RRAM). Summary of the invention

[0005] In view of this, the present application provides a resistive memory based on strontium stannate resistive film, and a preparation method and a packaging method, which are used to solve the technical problem in the prior art that the perovskite resistive film material is easy to deliquesce, resulting in poor stability of the resistive memory.

[0006] In a first aspect, the present application provides a resistive memory based on a strontium stannate resistive film, which comprises a top electrode, a bottom electrode, and a strontium stannate resistive film;

[0007] A strontium stannate resistive film is arranged between the top electrode and the bottom electrode.

[0008] Preferably, the top electrode is selected from any one of gold, platinum and silver;

[0009] The bottom electrode is selected from any one of FTO conductive glass and ITO conductive glass.

[0010] Preferably, the size of the bottom electrode is 25×20×5 mm;

[0011] The size of the strontium stannate resistive film is 15×10×0.5 mm;

[0012] The top electrode is a cylindrical top electrode with a radius of 1 mm and a height of 1 mm.

[0013] The second aspect of the present application provides a method for preparing a resistive random access memory based on a strontium stannate resistive random access film, which can prepare the resistive random access memory based on a strontium stannate resistive random access film described in the first aspect, and the preparation method comprises the steps of:

[0014] Step A1, spin coating a strontium stannate precursor solution on the surface of FTO conductive glass or ITO conductive glass to obtain a strontium stannate precursor film covering the surface of the FTO conductive glass or ITO conductive glass;

[0015] Step A2, annealing the strontium stannate precursor film covering the surface of the FTO conductive glass or the ITO conductive glass to obtain a strontium stannate resistive switching film covering the surface of the FTO conductive glass or the ITO conductive glass;

[0016] Step A3: depositing gold, platinum or silver on the surface of the strontium stannate resistive variable film to obtain a resistive variable memory of the strontium stannate resistive variable film.

[0017] Preferably, in step A1, the spin coating speed is 1000-3000 rpm, and the time is 10-20 s;

[0018] In step A2, the annealing temperature is 600-700° C. and the time is 2-4 hours.

[0019] In step A3, the deposition is to deposit gold, platinum or silver on the surface of the strontium stannate resistive film by magnetron sputtering.

[0020] The third aspect of the present application provides another method for preparing a resistive random access memory based on a strontium stannate resistive random access film, which can prepare the resistive random access memory based on a strontium stannate resistive random access film described in the first aspect, and the preparation method comprises the steps of:

[0021] Step B1, placing a T-shaped barrier on the surface of the FTO conductive glass or the ITO conductive glass to obtain the FTO conductive glass or the ITO conductive glass covered with the T-shaped barrier;

[0022] Step B2, spin coating a strontium stannate precursor solution on the surface of the FTO conductive glass or the ITO conductive glass covering the T-shaped barrier to obtain a strontium stannate precursor film covering the surface of the FTO conductive glass or the ITO conductive glass;

[0023] Step B3, annealing the strontium stannate precursor film covering the surface of the FTO conductive glass or the ITO conductive glass to obtain a strontium stannate resistive switching film covering the surface of the FTO conductive glass or the ITO conductive glass;

[0024] Step B4: depositing gold, platinum or silver on the surface of the strontium stannate resistive variable film, removing the T-shaped blocking area to obtain a resistive variable memory of the strontium stannate resistive variable film.

[0025] Preferably, in step B1, the T-shaped barrier is selected from T-shaped PI glue or T-shaped waterproof insulation glue;

[0026] In step B2, the spin coating speed is 1000-3000 rpm, and the time is 10-20 s;

[0027] In step B3, the annealing temperature is 600-700° C. and the time is 2-4 hours.

[0028] In step B4, the deposition is to deposit gold, platinum or silver on the surface of the strontium stannate resistive film by magnetron sputtering.

[0029] The fourth aspect of the present application provides a packaging method for a resistive random access memory based on a strontium stannate resistive random access film, which can encapsulate a resistive random access memory based on a strontium stannate resistive random access film described in the second aspect or the third aspect, comprising the steps of: spin coating a n-hexane solution of polydimethylsiloxane on the surface of the resistive random access memory based on the strontium stannate resistive random access film, and obtaining a packaged resistive random access memory based on the strontium stannate resistive random access film after drying.

[0030] The fifth aspect of the present application provides a packaging method for a resistive random access memory based on a strontium stannate resistive random access film, which can encapsulate a resistive random access memory based on a strontium stannate resistive random access film described in the second aspect or the third aspect, comprising the steps of spraying a n-hexane solution of polydimethylsiloxane on the surface of the resistive random access memory based on the strontium stannate resistive random access film, and obtaining a packaged resistive random access memory based on the strontium stannate resistive random access film after drying.

[0031] The fifth aspect of the present application provides an application of a resistive random access memory based on a strontium stannate resistive random access film as described in the first to fourth aspects in the preparation of an integrated circuit.

[0032] In summary, the present application provides a resistive memory based on a strontium stannate resistive variable film, and a preparation method and a packaging method. The resistive variable memory provided by the present application includes a top electrode, a bottom electrode, and a strontium stannate resistive variable film arranged between the top electrode / bottom electrode. The strontium stannate resistive variable film is an oxide with a perovskite structure. Compared with the conventional perovskite resistive variable film, the strontium stannate resistive variable film has better stability and is not easy to deliquesce. Moreover, after the resistive variable memory based on the strontium stannate resistive variable film is encapsulated with polydimethylsiloxane, the adverse effect of the external environment on the resistive variable memory can be reduced, thereby greatly improving the performance of the resistive variable memory. The turn-on voltage / reset voltage of the resistive variable memory is concentrated, and the resistance state mode is similar after multiple cycles, and the switching ratio is concentrated. At the same time, when the working voltage is applied, the low resistance state / high resistance state can be maintained for a long time, and the resistive variable memory has good stability. Therefore, the technical problem that the perovskite resistive variable film material is easy to deliquesce in the prior art, resulting in poor stability of the resistive variable memory can be solved. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to more clearly illustrate the specific implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0034] Figure 1 A schematic diagram of the structure of a resistive random access memory based on a strontium stannate resistive random access film provided in Example 1 of the present application;

[0035] Figure 2 A schematic diagram of the structure of a resistive memory based on a strontium stannate resistive switching film provided in Example 2 of the present application before and after being encapsulated with polydimethylsiloxane;

[0036] Figure 3 Scanning electron microscope images of a resistive random access memory based on a strontium stannate resistive random access film provided in Example 2 of the present application before and after being encapsulated with polydimethylsiloxane;

[0037] Figure 4 XRD analysis diagram of the SrSnO3 film provided in the embodiment of the present application;

[0038] Figure 5 A schematic diagram of the working principle of a resistive memory based on a strontium stannate resistive switching film provided in Example 1 or 2 of the present application when a voltage is applied;

[0039] Figure 6 An IV curve diagram of a resistive random access memory based on a strontium stannate resistive random access film provided in an embodiment of the present application;

[0040] Figure 7The switching voltage of the resistive random access memory based on the strontium stannate resistive random access film provided in the embodiment of the present application;

[0041] Figure 8 A switching ratio curve diagram of a resistive random access memory based on a strontium stannate resistive random access film provided in an embodiment of the present application;

[0042] Fig. 9 A resistance retention time diagram of a resistive memory based on a strontium stannate resistive switching film provided in an embodiment of the present application in a high resistance state and a low resistance state;

[0043] Fig.10 An IV curve diagram of the resistive random access memory based on the strontium stannate resistive random access film provided in an embodiment of the present application after multiple cycles;

[0044] Fig.11 Schematic diagram of thermal simulation performed using Comsol on a resistive random access memory based on a strontium stannate resistive random access film provided in an embodiment of the present application. DETAILED DESCRIPTION

[0045] The present application provides a resistive memory based on a strontium stannate resistive film, and a preparation method and a packaging method, which are used to solve the technical problem in the prior art that the perovskite resistive film material is easy to deliquesce, resulting in poor stability of the resistive memory.

[0046] The technical solution of the present application will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.

[0047] In view of the defect that conventional perovskite resistive variable film materials are easy to deliquesce, resulting in poor stability of resistive random access memory (RRAM), the present application provides a resistive random access memory based on a strontium stannate resistive variable film, and the resistive random access memory provided comprises a top electrode, a bottom electrode, and a strontium stannate resistive variable film arranged between the top electrode and the bottom electrode; when the resistive random access memory provided by the present application is in operation, a working voltage is applied to the strontium stannate resistive variable film through the top electrode and the bottom electrode, and the conductivity of the defective region (such as oxygen vacancies) in the strontium stannate resistive variable film can undergo a reversible change, forming a reversible conductive channel or disconnecting the conductive channel, thereby realizing a reversible low resistance state and a high resistance state; at the same time, it can quickly switch between the low resistance state and the high resistance state, and maintain the state after power failure, so it can be used as a non-volatile memory;

[0048] In addition, the resistive variable film material in the resistive random access memory provided by the present application is strontium stannate (SrSnO3), which is an oxide with a perovskite structure. Different from the resistive random access film material with a perovskite structure, strontium stannate as a resistive random access film material can exhibit better stability, which is reflected in that when the resistive random access memory provided by the present application adopts strontium stannate as the resistive random access film material, the turn-on voltage of the resistive random access memory is concentrated at about 0.65V, the reset voltage is concentrated at about -5V, the switching ratio range is in the range of 10 to 20, and the high resistance and low resistance are kept stable within 10,000s, and a stable resistive state mode can be maintained after 50 cycles. This shows that the resistive random access memory provided by the present application adopts strontium stannate as the resistive random access film material to improve the stability of the resistive random access memory, thereby overcoming the defect that the conventional perovskite resistive random access film material in the prior art is easy to deliquesce, resulting in poor stability of the resistive random access memory (RRAM).

[0049] Meanwhile, for the materials of the top electrode and the bottom electrode in this patent application, the top electrode is selected from any one of gold, platinum, and silver, and the bottom electrode is selected from FTO conductive glass / ITO conductive glass having a FTO film / ITO film on the surface.

[0050] Correspondingly, the present application also provides a corresponding preparation method for a resistive memory based on a strontium stannate resistive thin film, the preparation method comprising directly annealing a strontium stannate precursor solution on the surface of FTO conductive glass / ITO conductive glass, and depositing a top electrode by magnetron sputtering or the like to obtain a resistive memory, or pre-covering the surface of the FTO conductive glass / ITO conductive glass with a T-shaped barrier, and then annealing a strontium stannate precursor solution on the surface of the FTO conductive glass / ITO conductive glass, and depositing a top electrode by magnetron sputtering or the like to obtain a resistive memory.

[0051] Preferably, the present application also provides a method for packaging a resistive memory based on a strontium stannate resistive film, wherein the packaging method uses 20% polydimethylsiloxane (20% PDMS), which is spin-coated or sprayed on the resistive memory based on the strontium stannate resistive film; since polydimethylsiloxane has excellent mechanical properties, good chemical inertness and chemical corrosion resistance, these properties enable it to effectively protect electronic devices from external impact and friction, and can protect the electronic components packaged therein from the influence of corrosive substances that may exist in the external environment.

[0052] At the same time, the present application has conducted experiments on the electrical and thermal properties of the resistive memory based on the strontium stannate resistive film. The resistive memory based on the strontium stannate resistive film provided by the present application will be specifically described below in combination with embodiments and experimental examples.

[0053] Example 1

[0054] Embodiment 1 of the present application provides a method for preparing a resistive memory based on a strontium stannate resistive memory film, the structure of which is as follows: Figure 1 As shown, the preparation method includes: the steps of preparing a strontium stannate precursor solution, preparing a strontium stannate resistive film on the surface of a bottom electrode, and preparing a top electrode on the surface of the strontium stannate resistive film.

[0055] The step of preparing a strontium stannate precursor solution comprises: dissolving 0.004 mol of strontium acetate in 4 ml of deionized water and stirring at 60° C. for 30 min to obtain a strontium acetate aqueous solution, dissolving 0.004 mol of tin tetrachloride pentahydrate in 16 ml of ethanol and stirring at 60° C. for 30 min to obtain a tin tetrachloride ethanol solution; stirring the two solutions to obtain a clear and transparent solution, mixing the strontium acetate aqueous solution and the tin tetrachloride ethanol solution together and adding 2 g of citric acid, heating to 80° C. and stirring to obtain a clear and transparent solution to obtain a strontium stannate precursor solution.

[0056] The steps of preparing a strontium stannate resistive film on the surface of the bottom electrode include: first placing FTO conductive glass (25×20×5mm) on a spin coater, and dropping 100μL of a strontium stannate precursor solution on the FTO conductive glass; then spin coating at a rotation speed of 2000rpm and an acceleration of 200rpm for 15s to obtain a transparent strontium stannate precursor film; then heating to 600~700℃ at a heating rate of 10℃ / min, annealing for 3h, and preparing a strontium stannate resistive film (15×10×0.5mm) on the surface of the FTO conductive glass.

[0057] The steps of preparing the top electrode on the surface of the strontium stannate resistive film include: placing a mask with four top electrode shapes on the strontium stannate resistive film, and then sputtering four top electrodes (R=1mm, H=1mm) on the top of the strontium stannate resistive film using a magnetron sputtering process.

[0058] Example 2

[0059] Embodiment 2 of the present application provides a method for preparing a resistive memory based on a strontium stannate resistive thin film, the structure of which is as follows: Figure 2 As shown in Figure a, the preparation method includes: the steps of preparing a strontium stannate precursor solution, preparing a strontium stannate resistive film on the surface of a bottom electrode, and preparing a top electrode on the surface of the strontium stannate resistive film.

[0060] The step of preparing a strontium stannate precursor solution comprises: dissolving 0.004 mol of strontium acetate in 4 ml of deionized water and stirring at 60° C. for 30 min to obtain a strontium acetate aqueous solution, dissolving 0.004 mol of tin tetrachloride pentahydrate in 16 ml of ethanol and stirring at 60° C. for 30 min to obtain a tin tetrachloride ethanol solution; stirring the two solutions to obtain a clear and transparent solution, mixing the strontium acetate aqueous solution and the tin tetrachloride ethanol solution together and adding 2 g of citric acid, heating to 80° C. and stirring to obtain a clear and transparent solution to obtain a strontium stannate precursor solution.

[0061] The steps of preparing a strontium stannate resistive variable film on the surface of the bottom electrode include: first placing FTO conductive glass (25×20×5mm) on a spin coater, and then covering the surface of the FTO conductive glass with a T-shaped PI glue; and dropping 100μL of a strontium stannate precursor solution on the FTO conductive glass; then spin coating at a rotation speed of 2000rpm and an acceleration of 200rpm for 15s to obtain a transparent strontium stannate precursor film; then heating to 600~700℃ at a heating rate of 10℃ / min, annealing for 3h, and preparing a strontium stannate resistive variable film (10×4×0.5mm / 10×4×0.5mm) on the surface of the FTO conductive glass.

[0062] The steps of preparing the top electrode on the surface of the strontium stannate resistive film include: placing a mask with two top electrode shapes above the strontium stannate resistive film, and then sputtering four top electrodes (R=1mm, H=1mm) on the top of the strontium stannate resistive film using a magnetron sputtering process.

[0063] Example 3

[0064] Embodiment 3 of the present application provides a method for preparing a resistive memory device based on a strontium stannate resistive film, which can encapsulate the resistive memory device based on the strontium stannate resistive film described in Embodiment 1 or Embodiment 2, wherein the schematic diagram of the resistive memory device based on the strontium stannate resistive film described in Embodiment 2 after encapsulation is as shown in FIG. Figure 2 As shown in Figure b; the encapsulation method includes the steps of preparing a polydimethylsiloxane (PDMS) solution and the step of encapsulating.

[0065] The step of preparing a polydimethylsiloxane (PDMS) solution includes: weighing 2 ml of polydimethylsiloxane (PDMS) and 8 ml of n-hexane in a volume ratio of 20:80 and mixing them evenly to obtain a polydimethylsiloxane solution (with a concentration of 20%).

[0066] The encapsulation step includes: taking 50 μL of the prepared polydimethylsiloxane solution and dropping it on the surface of the resistive memory based on the strontium stannate resistive film, spinning it at a rotation speed of 5000 rpm and an acceleration of 200 rpm for 30 seconds, and obtaining the encapsulated resistive memory based on the strontium stannate resistive film after drying; or taking 50 μL of the prepared polydimethylsiloxane solution and filling it into a spray bottle, and then placing it 30 cm above the center of the resistive memory based on the strontium stannate resistive film for spraying, and obtaining the encapsulated resistive memory based on the strontium stannate resistive film after drying.

[0067] Experimental Example 1

[0068] Experimental Example 1 of the present application tests the resistive random access memory based on the strontium stannate resistive random access film provided in Example 1.

[0069] Among them, the scanning electron microscope image before polydimethylsiloxane encapsulation is as follows Figure 3 As shown in Figure a, the scanning electron microscope image after polydimethylsiloxane is encapsulated by spin coating is as follows Figure 3 As shown in Figure b, the scanning electron microscope image after encapsulation using polydimethylsiloxane by spraying is as follows Figure 3 As shown in Figure c; Figure 3 It can be seen from Figures a~c that before polydimethylsiloxane encapsulation, the resistive memory based on strontium stannate resistive film has many pores. After polydimethylsiloxane encapsulation, spin coating or spray encapsulation can form a smooth, uniform, dense and crack-free PDMS encapsulation layer on the surface of the resistive memory, thereby reducing the adverse effects of the external environment on the resistive memory and improving the performance of the resistive memory.

[0070] The X-ray diffraction pattern of the resistive memory based on strontium stannate resistive film is as follows: Figure 4 As shown, from Figure 4 It can be seen that the resistive memory exhibits a series of diffraction peaks at 23.17°, 31.44°, and 65.63°, corresponding to strontium stannate (SrSnO3), silver (Ag), and fluorine-doped tin oxide conductive glass (FTO), respectively. This shows that the resistive memory provided by the present application uses silver and fluorine-doped tin oxide conductive glass as top / bottom electrodes, and strontium stannate as a resistive film between the top / bottom electrodes.

[0071] The digital source meter Keithley2400 was used to test the current-voltage (IV) characteristics of the resistive memory based on the strontium stannate resistive film. The working principle of the resistive memory during the test is as follows: Figure 5 As shown in Figure 1, under the action of an applied voltage, the strontium stannate resistive film forms and breaks conductive filaments, switching back and forth between a high resistance state and a low resistance state; the test results are shown in Figure 1. Figures 6 to 10 shown; from Figure 6It can be seen that when the voltage of the RRAM is cycled between 4V and -8V, the RRAM is initially in a high-resistance state. When the working bias voltage exceeds the threshold voltage of 0.74V, the current suddenly increases, indicating that the RRAM changes from a high-resistance state to a low-resistance state. When the voltage is scanned in the reverse direction, the low-resistance state can be stably maintained. When the bias voltage exceeds the threshold voltage When the current drops sharply, the resistive memory changes from low resistance state to high resistance state, with a low resistance value of 0.153KΩ and a high resistance value of 1.983KΩ. The switching ratio exceeds 10, which has a good switching ratio. Figure 7 It can be seen that the turn-on voltage of the resistive memory provided in this application is mostly concentrated at 0.65V, and the reset voltage is concentrated at , while Figure 8 As shown in Figure 2, the switching ratio of the RRAM after 20 cycles is concentrated in the range of 10~20, while Fig. 9 It can be seen that when the working voltage is applied to the resistive memory for 10,000 seconds, its low resistance state and high resistance state remain stable. Fig.10 As shown, within the operating voltage range of -6 to 0V and 0 to 3V, the resistance state modes of the 10th, 20th and 50th switching cycles are similar, which indicates that the resistive random access memory provided by the present application uses strontium stannate, an oxide with a perovskite structure, as the resistive random access memory thin film material, which can improve the stability of the resistive random access memory, thereby solving the technical problem in the prior art that the conventional perovskite resistive random access memory (RRAM) is easy to deliquesce, resulting in poor stability of the resistive random access memory (RRAM).

[0072] Experimental Example 2

[0073] Experimental Example 1 of the present application conducts a thermal simulation experiment on the resistive switching memory based on the strontium stannate resistive switching film provided in Example 1 using polydimethylsiloxane packaging. Fig.11 shown.

[0074] The simulation software used in the thermal simulation experiment is COMSOL. In the resistive memory model of strontium stannate resistive film, the size of FTO conductive glass is 25×20×5mm, the air domain is 50×50×20mm, the size of strontium stannate resistive film is 15×10×0.5mm, the radius of silver electrode is 1mm, the height is 1mm, and the size of PDMS is 20×20×1.5mm.

[0075] For power consumption calculation, since the resistive memory provided in the present application can maintain the original state without external stimulation, it is only necessary to calculate the switch power consumption. The power consumption calculation is shown in Formula 1:

[0076] (1)

[0077] V is the switching voltage, T is the switching time; taking the classic switch diagram as an example, Vset is 0.74V, Vreset is -4.95V, Ron is 0.15339231KΩ, Roff is 1.983495699KΩ, Tset is 0.1s, Treset is 0.1s, and the power consumption of the resistive memory provided in the present application is calculated to be approximately 1.59×10 -3 J; while the core temperature is around 30°C.

[0078] The above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, a person skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some or all of the technical features thereof may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present application.

Claims

1. A resistive random access memory based on a strontium stannate resistive random access film, characterized in that: It includes a top electrode, a bottom electrode, and a strontium stannate resistive film; A strontium stannate resistive film is arranged between the top electrode and the bottom electrode.

2. The resistive random access memory based on the strontium stannate resistive random access film according to claim 1, characterized in that: The top electrode is selected from any one of gold, platinum and silver; The bottom electrode is selected from any one of FTO conductive glass and ITO conductive glass.

3. The resistive random access memory based on the strontium stannate resistive random access film according to claim 1, characterized in that: The size of the bottom electrode is 25×20×5 mm; The size of the strontium stannate resistive film is 15×10×0.5 mm; The top electrode is a cylindrical top electrode with a radius of 1 mm and a height of 1 mm.

4. A method for preparing a resistive random access memory based on a strontium stannate resistive random access film according to any one of claims 1 to 3, characterized in that: Includes steps: Step A1, spin coating a strontium stannate precursor solution on the surface of FTO conductive glass or ITO conductive glass to obtain a strontium stannate precursor film covering the surface of the FTO conductive glass or ITO conductive glass; Step A2, annealing the strontium stannate precursor film covering the surface of the FTO conductive glass or the ITO conductive glass to obtain a strontium stannate resistive switching film covering the surface of the FTO conductive glass or the ITO conductive glass; Step A3: depositing gold, platinum or silver on the surface of the strontium stannate resistive variable film to obtain a resistive variable memory of the strontium stannate resistive variable film.

5. The method for preparing a resistive random access memory based on a strontium stannate resistive random access film according to claim 4, characterized in that: In step A1, the spin coating speed is 1000-3000 rpm, and the time is 10-20 s; In step A2, the annealing temperature is 600-700° C. and the time is 2-4 hours; In step A3, the deposition is to deposit gold, platinum or silver on the surface of the strontium stannate resistive film by magnetron sputtering.

6. A method for preparing a resistive random access memory based on a strontium stannate resistive random access film according to any one of claims 1 to 3, characterized in that: Includes steps: Step B1, placing a T-shaped barrier on the surface of the FTO conductive glass or the ITO conductive glass to obtain the FTO conductive glass or the ITO conductive glass covered with the T-shaped barrier; Step B2, spin coating a strontium stannate precursor solution on the surface of the FTO conductive glass or the ITO conductive glass covering the T-shaped barrier to obtain a strontium stannate precursor film covering the surface of the FTO conductive glass or the ITO conductive glass; Step B3, annealing the strontium stannate precursor film covering the surface of the FTO conductive glass or the ITO conductive glass to obtain a strontium stannate resistive switching film covering the surface of the FTO conductive glass or the ITO conductive glass; Step B4: depositing gold, platinum or silver on the surface of the strontium stannate resistive variable film, removing the T-shaped blocking area to obtain a resistive variable memory of the strontium stannate resistive variable film.

7. The method for preparing a resistive random access memory based on a strontium stannate resistive random access film according to claim 6, characterized in that: In step B1, the T-shaped barrier is selected from T-shaped PI glue or T-shaped waterproof insulation glue; In step B2, the spin coating speed is 1000-3000 rpm, and the time is 10-20 s; In step B3, the annealing temperature is 600-700° C. and the time is 2-4 hours; In step B4, the deposition is to deposit gold, platinum or silver on the surface of the strontium stannate resistive film by magnetron sputtering.

8. A packaging method for a resistive random access memory based on a strontium stannate resistive random access film according to any one of claims 1 to 3, characterized in that: The method comprises the following steps: spin coating a n-hexane solution of polydimethylsiloxane on the surface of a resistive memory based on a strontium stannate resistive film, and obtaining a packaged resistive memory based on a strontium stannate resistive film after drying.

9. A resistive random access memory based on a strontium stannate resistive random access film as claimed in any one of claims 1 to 3 The packaging method is characterized in that The method comprises the following steps: spraying a n-hexane solution of polydimethylsiloxane on the surface of a resistive memory based on a strontium stannate resistive film, and obtaining a packaged resistive memory based on the strontium stannate resistive film after drying.

10. Use of a memristor based on a strontium stannate resistive film as claimed in any one of claims 1 to 3 in the preparation of integrated circuits.

Citation Information

Patent Citations

  • Memister

    CN101546811A

  • Application of strontium stannate titanate film

    CN101800282A

  • Trap state regulation and control based nonvolatile multi-bit micro / nanometer resistive random access memory and use method therefor