Modified titanium dioxide photocatalyst as well as preparation method and application thereof

By loading CuNi, CuCo or CuFe alloy nanoparticles on ultrathin titanium dioxide nanosheets, the problems of high recombination rate of TiO2 photocatalysts in photocatalytic reforming and high cost of precious metals are solved, achieving efficient and stable visible light response and high efficiency Hydrogen production performance reduces costs and avoids environmental pollution.

CN118976496APending Publication Date: 2024-11-19SOUTHWEST FORESTRY UNIVERSITY

Patent Information

Application Number
CN202411070673.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

During the photocatalytic reforming of the existing TiO2 photocatalyst, there are problems such as high photogenerating carrier recombination, low solar energy utilization, high cost of precious metal cocatalysts and complex modification process, which limits its hydrogen production in glucose reforming. efficiency and sustainability in.

Method used

Ultrathin titanium dioxide nanosheets containing oxygen vacancies were used to support CuNi, CuCo or CuFe alloy nanoparticles, and modified titanium dioxide photocatalysts were prepared by hydrothermal method and photoreduction method to expand the light absorption range and improve the electron-hole separation efficiency.

Benefits of technology

It achieves efficient and stable visible light response, improves photocatalytic hydrogen production performance, reduces costs, and avoids the dependence of traditional sacrificial agents and environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118976496A_ABST
    Figure CN118976496A_ABST
Patent Text Reader

Abstract

The invention discloses a modified titanium dioxide photocatalyst as well as a preparation method and application thereof, and belongs to the technical field of catalyst preparation. The modified titanium dioxide photocatalyst comprises a carrier and an active component loaded on the carrier; the carrier is a titanium dioxide nanosheet containing oxygen vacancies (OVs); and the active component is alloy nanoparticles. According to the modified titanium dioxide photocatalyst, the titanium dioxide nanosheets are synergistically promoted to produce hydrogen through the OVs and the alloy nanoparticles, the efficiency is high, the stability is good, and response can be achieved within the visible light range.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalyst preparation, and in particular to a modified titanium dioxide photocatalyst and a preparation method and application thereof. Background Art

[0002] Hydrogen (H2) has emerged as a renewable energy alternative that can solve the fossil fuel combustion crisis and environmental burden, but current H2 production mainly relies on steam reforming of fossil fuels and is therefore energy-intensive and unsustainable. Photocatalytic reforming of lignocellulose to produce hydrogen using solar energy to drive the reaction between lignocellulose and water provides a clean and promising method to convert lignocellulose into chemical fuels. Photocatalytic reforming is the reduction of protons by excited electrons from a semiconductor to form H2 fuel. Since Kawai and Sakata first reported the photocatalytic conversion of carbohydrates into H2 using Pt and RuO2 co-loaded TiO2 as a photocatalyst, researchers have made great efforts to develop efficient lignocellulose-to-H2 conversion systems, but the conversion performance of lignocellulose to H2 is still low. The main reason for the low performance is related to the complex structure and high inertness of lignocellulose.

[0003] Glucose is the most widely distributed and important monosaccharide in nature. It is an energy source and metabolic intermediate for living cells. Due to its high hydrogen / carbon ratio, low price, and easy access to cellulose, glucose has become an important biorenewable resource for photocatalytic reforming to produce hydrogen. In the process of glucose photocatalytic reforming to produce hydrogen, glucose is oxidized by excited holes left in the valence band of the semiconductor as a sacrificial agent. Therefore, the recombination rate of photogenerated electron-hole pairs is delayed and the H2 production rate is increased. Compared with the conventional photocatalytic H2 reduction using non-renewable and expensive chemicals such as methanol and triethanolamine as sacrificial agents, the use of cheap glucose is obviously scalable and sustainable. In addition, as a hole trap, glucose can also be oxidized into high-value-added chemicals such as gluconic acid, glucagon, arabinose, 5-hydroxymethylfurfural, lactic acid, formic acid, etc. Therefore, reforming hydrogen production with glucose as a substrate has more advantages than reforming hydrogen production with lignocellulose as a substrate. However, in order to achieve good hydrogen production efficiency by reforming hydrogen production with glucose as a substrate, high-quality photocatalysts are still indispensable.

[0004] As one of the earliest studied n-type semiconductor photocatalysts, TiO2 has the advantages of being cheap, stable, non-toxic, and environmentally friendly. More importantly, the photogenerated holes generated by the high oxidation potential of TiO2 have a stronger ability to open glucose bonds. Therefore, TiO2 has become an ideal candidate for photocatalytic reforming to produce hydrogen. In the process of photocatalytic reforming to produce hydrogen, when the energy of the incident ultraviolet light is greater than the bandgap width of TiO2, electrons jump from the valence band to the conduction band, and holes are generated in the valence band, realizing the spatial separation of carriers, and the excited electrons reduce protons to form H2. However, in the actual photocatalytic reaction process, a large number of photogenerated electrons and holes recombine inside or on the surface of the semiconductor, which in turn limits the improvement of photocatalytic efficiency. Therefore, the current practical application of TiO2 in the field of photocatalytic reforming hydrogen production mainly has the following problems: (1) Anatase TiO2 can only absorb the ultraviolet light part that accounts for 5% of the solar spectrum, which greatly limits its utilization rate of sunlight; (2) The high recombination rate of photogenerated carriers leads to low photocatalytic efficiency. In order to improve the hydrogen production efficiency, various co-catalysts are usually required to be loaded on TiO2 to improve the separation efficiency of electron-hole pairs, thereby significantly improving its photocatalytic hydrogen production performance. Commonly used TiO2 co-catalysts are mainly precious metals such as Pt, Pd, and Au. In practical applications, they are limited by the high price and scarcity of precious metals; (3) Although some non-precious metal co-catalysts (such as transition metal sulfides) have been studied to enhance the photocatalytic performance of TiO2, the performance improvement of a single co-catalyst is limited due to the lack of synergistic sites; (4) The process of modifying TiO2 in the existing technology is complicated. Therefore, it is of great practical significance to construct glucose reforming hydrogen production photocatalytic materials that are responsive to visible light, highly efficient, stable, have excellent photocatalytic hydrogen production performance, are highly efficient, easily available, and inexpensive. Summary of the invention

[0005] The purpose of the present invention is to provide a modified titanium dioxide photocatalyst and its preparation method and application to solve the problems existing in the above-mentioned prior art. Specifically, the present invention provides an ultra-thin titanium dioxide photocatalytic hydrogen production material rich in oxygen vacancies (OVs) and loaded with alloy nanoparticles, which has visible light response, high efficiency, stability, and excellent photocatalytic hydrogen production performance, and OVs and alloy nanoparticles are synergistically catalyzed to produce hydrogen from titanium dioxide nanosheets.

[0006] To achieve the above object, the present invention provides the following solutions:

[0007] One of the technical solutions of the present invention: a modified titanium dioxide (TiO2) photocatalyst, comprising a carrier and an active component loaded on the carrier; the carrier is a titanium dioxide nanosheet containing oxygen vacancies (OVs); the active component is an alloy nanoparticle; the alloy nanoparticle is a CuNi alloy nanoparticle, a CuCo alloy nanoparticle or a CuFe alloy nanoparticle.

[0008] Cu nanoparticles have properties similar to precious metals, which can capture solar radiation and generate high-energy electrons on the catalyst surface through the plasma resonance (SPR) effect, thereby expanding the light absorption range. Ni, Co or Fe can form bimetallic alloy nanoparticles with Cu, which effectively prevents the oxidation of single-phase Cu nanoparticles in air.

[0009] Furthermore, the titanium dioxide nanosheets containing oxygen vacancies are anatase titanium dioxide.

[0010] Furthermore, the titanium dioxide nanosheet containing oxygen vacancies is an ultra-thin nanosheet structure (or nanosheet structure).

[0011] Furthermore, the molar ratio of Cu to another metal in the alloy nanoparticles is 0.4:0.6-0.8:0.2 (the sum of the molar amounts of Cu and another metal is recorded as 1).

[0012] Furthermore, for the convenience of naming and distinction, the chemical formula of the titanium dioxide nanosheet containing oxygen vacancies is recorded as TiO 2-X , X represents oxygen vacancies, and the chemical formula of the modified titanium dioxide photocatalyst is Cu y M 1-y -TiO 2-X , wherein M = Ni, Co or Fe, and y is 0.4-0.8.

[0013] Furthermore, the y is preferably 0.4, 0.59 or 0.71, that is, the molar ratio of Cu to another metal in the alloy nanoparticles is preferably 0.4:0.6, 0.59:0.41 or 0.71:0.29.

[0014] Furthermore, the loading amount of the alloy nanoparticles on the titanium dioxide nanosheets containing oxygen vacancies (OVs) is 3-7 wt %.

[0015] The second technical solution of the present invention is as follows: the preparation method of the modified titanium dioxide photocatalyst comprises the following steps: preparing anatase titanium dioxide nanosheets (referred to as TiO2 nanosheets) by a hydrothermal method; reducing the anatase titanium dioxide nanosheets by a reducing agent to obtain titanium dioxide nanosheets containing oxygen vacancies (referred to as TiO 2-X Nanosheets); alloy nanoparticles are loaded on the titanium dioxide nanosheets containing oxygen vacancies by a photoreduction method to obtain the modified titanium dioxide photocatalyst (abbreviated as Cu y M 1-y -TiO 2-X ).

[0016] Furthermore, the anatase titanium dioxide nanosheet is anatase titanium dioxide nanosheet with exposed (001) crystal plane.

[0017] Furthermore, the anatase titanium dioxide nanosheet is an ultra-thin nanosheet structure.

[0018] Furthermore, the preparation of anatase titanium dioxide nanosheets by hydrothermal method includes: mixing Ti(OBu)4 (tetrabutyl titanate), HF and anhydrous ethanol, and performing a hydrothermal reaction; after the hydrothermal reaction, washing the solid product with 0.1M NaOH, anhydrous ethanol and deionized water in sequence and filtering, and then drying to obtain the anatase titanium dioxide nanosheets.

[0019] Furthermore, the mixing volume ratio of Ti(OBu)4, HF and anhydrous ethanol is 3:1:5.

[0020] Furthermore, the concentration of HF is 6-7 mol / L.

[0021] Furthermore, the temperature of the hydrothermal reaction is 170-200° C., and the time is 16-18 hours.

[0022] Furthermore, the reducing agent includes sodium borohydride, hydrogen or MgH2.

[0023] Furthermore, the reducing agent is sodium borohydride, and the specific reduction operation is: mixing the anatase titanium dioxide nanosheets and sodium borohydride and grinding them for 20-40 minutes, and calcining to obtain the titanium dioxide nanosheets containing oxygen vacancies.

[0024] Furthermore, the mass ratio of the anatase titanium dioxide nanosheets to sodium borohydride is 1:0.8-1.3; the calcination temperature is 350-410° C., and the calcination time is 2-4 hours.

[0025] Furthermore, the reducing agent is MgH2, and the specific reduction operation is: mixing the anatase titanium dioxide nanosheets with MgH2 and grinding them for 20-40 minutes, calcining them in an Ar atmosphere, stirring the calcined product in dilute HCl for 1 day to remove Mg, then washing and drying to obtain the titanium dioxide nanosheets containing oxygen vacancies.

[0026] Furthermore, the mass ratio of the anatase titanium dioxide nanosheets to MgH2 is 1:0.8-1.3; the calcination temperature is 450-550°C, and the time is 7-9h; and the concentration of the dilute HCl is 10-15wt%.

[0027] Furthermore, the reducing agent is H2, and the specific operation of reduction is: grinding the anatase titanium dioxide nanosheets for 20-40 minutes, and then calcining them in a H2 flow at 450-550°C under normal pressure for 2-3 hours.

[0028] Furthermore, the method of loading alloy nanoparticles on the titanium dioxide nanosheets containing oxygen vacancies by photoreduction includes: mixing the titanium dioxide nanosheets containing oxygen vacancies with a metal source and water to obtain a mixed solution, and then performing a photoreduction reaction under irradiation of a light source.

[0029] Furthermore, the metal source is a Cu source and a Ni source, or a Cu source and a Co source, or a Cu source and a Fe source.

[0030] Furthermore, the Cu source is CuSO4·5H2O, the Ni source is NiCl2; the Co source is Co(NO3)2; and the Fe source is FeCl3.

[0031] Furthermore, the molar ratio of the Cu source to another metal source (Ni source, Co source or Fe source) is y:1-y.

[0032] Furthermore, the intensity of the light source is 300W, and the irradiation time of the light source is 50-70 minutes.

[0033] Furthermore, the light source is 20-30 cm away from the surface of the mixed solution.

[0034] The third technical solution of the present invention: Application of the above-mentioned modified titanium dioxide photocatalyst in photocatalytic glucose reforming to produce hydrogen.

[0035] The photocatalytic glucose reforming hydrogen production comprises the following steps: adding the modified titanium dioxide photocatalyst into a glucose aqueous solution, then transferring the glucose aqueous solution into a photoreactor, blowing N2 into the photoreactor before the reaction, removing air from the glucose aqueous solution, and then applying light to react.

[0036] Furthermore, the glucose aqueous solution is prepared by adding 0.5-1 g of glucose to every 100 ml of deionized water. The amount of the modified titanium dioxide photocatalyst added to the glucose aqueous solution is 0.05-0.1 g / 100 ml (photocatalyst dosage / volume of glucose aqueous solution).

[0037] Furthermore, the intensity of the illumination is 300W.

[0038] The present invention discloses the following technical effects:

[0039] (1) The present invention provides a modified titanium dioxide photocatalyst, comprising titanium dioxide nanosheets containing oxygen vacancies (OVs) as a carrier and active component alloy nanoparticles loaded on the carrier. The OVs and the alloy nanoparticles synergistically promote the titanium dioxide nanosheets to produce hydrogen, which has high efficiency, good stability, and can respond in the visible light range.

[0040] (2) The present invention firstly prepares anatase-type ultrathin TiO2 nanosheets with exposed (001) crystal planes by a hydrothermal method. The ultrathin nanosheet structure not only provides abundant active sites for the photocatalytic H2 production reaction, but also facilitates the transfer of photogenerated charges to the surface, thereby increasing the separation rate of photogenerated electrons and holes. Then, abundant OVs are introduced into the TiO2 nanosheets by reduction treatment to obtain TiO 2-X Nanosheets, TiO 2-X The light absorption range of OVs can be extended from ultraviolet light to infrared light, significantly improving the photocatalytic performance driven by solar energy. At the same time, the presence of a large number of OVs can serve as charge capture centers and adsorption sites generated by light, preventing the recombination of electrons and holes, thereby effectively improving the separation efficiency of photogenerated carriers and hydrogen production performance. Finally, the photoreduction method was used to remove the photogenerated charge from TiO 2-X The surface of the nanosheet is loaded with highly dispersed non-precious metal alloy nanoparticles (CuNi alloy nanoparticles, CuCo alloy nanoparticles or CuFe alloy nanoparticles), thereby obtaining Cu y M 1-y -TiO 2-X (M=Ni, Co or Fe, y is 0.4-0.8) composite photocatalyst. 2-X The loading on the surface of the nanosheets can produce a surface plasmon resonance (SPR) effect, which can show a more efficient electron-hole separation phenomenon, so the charge carriers will be easily transferred to the modified titanium dioxide-based TiO 2-X surface, further expanding the light response range and improving the separation efficiency of photogenerated carriers.

[0041] (3) The present invention uses glucose as a hydrogen production substrate to replace the traditional sacrificial agent, which not only avoids the problem of dependence on traditional sacrificial agents in the process of photocatalytic water decomposition to produce hydrogen, but also can further oxidize glucose into high value-added chemicals, such as gluconic acid, gluconic acid, arabinose, 5-hydroxymethylfurfural, lactic acid, formic acid, etc., thereby solving the problems of high cost and easy environmental pollution caused by traditional sacrificial agents. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0043] Figure 1 The ultrathin titanium dioxide TiO2 nanosheets prepared in step 1 of Example 1 (referred to as TiO2(1)) and the TiO2 nanosheets prepared in step 2 of Example 1 are 2-X And the XRD pattern (a) and Raman spectrum (b) of the conventional non-ultrathin TiO2 (denoted as TiO2(2)) prepared in Comparative Example 1;

[0044] Figure 2 The TiO2 prepared in step 1 of Example 1 (referred to as TiO2(1)) and the TiO2 prepared in step 2 of Example 1 2-X EPR spectrum of

[0045] Figure 3 The Cu with different CuNi loading ratios prepared in Examples 1-3 and Comparative Examples 2-3 y Ni 1-y -TiO 2-X XRD pattern comparison;

[0046] Figure 4 The TiO prepared in step 2 of Example 1 2-X SEM image (a) and TEM image (b);

[0047] Figure 5 The Cu prepared in Example 2 0.59 Ni 0.41 -TiO 2-X SEM images of

[0048] Figure 6 The Cu prepared in Example 2 0.59 Ni 0.41 -TiO 2-X Element mapping test results (ae) and EDS spectrum (f);

[0049] Figure 7 The TiO2 prepared in step 1 of Example 1 (referred to as TiO2(1)) and the TiO2 prepared in step 2 of Example 1 are 2-X And the Cu prepared in Example 2 0.59 Ni 0.41 -TiO 2-X UV-vis spectrum (a) and VB-XPS graph (b);

[0050] Figure 8 The Cu loaded with bimetallic materials of different ratios prepared in Examples 1-3 y Ni 1-y -TiO 2-X , Ni-TiO prepared in Comparative Example 2-3 2-X and Cu-TiO 2-X , TiO2 prepared in step 1 of Example 1 (referred to as TiO2(1)) and TiO2 prepared in step 2 of Example 1 2-X The curve of hydrogen production changing with time;

[0051] Fig. 9 The Cu loaded with bimetallic materials of different ratios prepared in Examples 1-3 y Ni 1-y -TiO 2-X , Ni-TiO prepared in Comparative Example 2-3 2-X and Cu-TiO 2-X , TiO prepared in step 1 of Example 1 2-2 (denoted as TiO2(1)) and the TiO prepared in step 2 of Example 1 2-X The hydrogen production rate;

[0052] Fig.10 Cu with different bimetallic loadings prepared in Examples 2, 4-5 0.59 Ni 0.41 -TiO 2-X Compared with 1wt% Pt-TiO prepared in Comparative Example 4 2-X The hydrogen production rate;

[0053] Fig.11 5wt% Cu prepared in Example 2 0.59 Ni 0.41 -TiO 2-X , 5wt% Cu prepared in Example 8 0.59 Fe 0.41 -TiO 2-X , 5wt% Cu prepared in Example 9 0.59 Co 0.41 -TiO 2-X , 5wt% Cu prepared in Comparative Example 5 0.59 Bi 0.41 -TiO 2-X And the 5wt% Cu prepared in Comparative Example 6 0.59 Zn 0.41 -TiO 2-X The hydrogen production rate;

[0054] Fig.12 5wt% Cu prepared in Example 2 0.59 Ni 0.41 -TiO2-X Example 6 Preparation of 5wt% Cu 0.59 Ni 0.41 -TiO 2-X (MgH2) and 5wt% Cu prepared in Example 7 0.59 Ni 0.41 -TiO 2-X (H2) hydrogen production rate;

[0055] Fig.13 5wt% Cu prepared in Example 2 under different pH conditions 0.59 Ni 0.41 -TiO 2-X The hydrogen production rate;

[0056] Fig.14 is the LC-MS spectrum of the oxidation products of glucose;

[0057] Fig.15 5wt% Cu after one reaction 0.59 Ni 0.41 -TiO 2-X (Prepared in Example 2) SEM image. DETAILED DESCRIPTION

[0058] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0059] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0060] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0061] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.

[0062] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0063] The room temperature or normal temperature involved in the specific implementation manner of the present invention specifically refers to 20-25°C.

[0064] Example 1

[0065] 5wt%Cu 0.44 Ni 0.56 -TiO 2-X The preparation steps of photocatalyst are as follows:

[0066] Step 1: Preparation of ultra-thin TiO2 nanosheets with anatase exposed (001) crystal plane by hydrothermal method

[0067] Add 12 ml of Ti(OBu)4 and 4 ml of 6.39 mol / L HF to a 50 ml polytetrafluoroethylene-lined autoclave, mix well, then add 20 ml of anhydrous ethanol and mix again. Move the autoclave to an oven and react at 180°C for 18 hours. Wash the solid product with 0.1 M NaOH, anhydrous ethanol and deionized water in turn and filter. Repeat 3 times, and place the filtered sample in a vacuum drying oven at 60°C for 12 hours to obtain ultrathin TiO2 nanosheets, which are recorded as TiO2(1) for distinction during testing.

[0068] Step 2: The ultra-thin TiO2 nanosheets with exposed (001) crystal plane prepared in step 1 were mixed with NaBH4 at a molar ratio of 1:1 and ground for 30 min. The ground mixture was placed in a tube furnace and calcined at 400 °C for 3 h to obtain black ultra-thin TiO2 nanosheets rich in OVs. 2-X Nanosheets;

[0069] Step 3: Synthesis of Cu by photoreduction y Ni 1-y Loaded TiO 2-X :

[0070] Take 1.16g of TiO prepared in step 2 2-X, 0.44mmol CuSO4·5H2O and 0.56mmol NiCl2 were dissolved in 48ml water to form a mixed solution. After degassing, the mixed solution was photoreduced with a xenon lamp. The light source was a 300W xenon lamp, which was about 20cm away from the surface of the mixed solution. The irradiation time was 50min, and Cu 0.44 Ni 0.56 -TiO 2-X .

[0071] The elemental composition of the product obtained in step 3 was determined by ICP elemental analysis. The results showed that the actual ratio of metal CuNi in the product and its content in TiO 2-X The loading amount on the nanosheets is consistent with the preset composition, and the product can be labeled as 5wt% Cu 0.44 Ni 0.56 -TiO 2-X .

[0072] Example 2

[0073] 5wt%Cu 0.59 Ni 0.41 -TiO 2-X The preparation steps of photocatalyst are as follows:

[0074] Step 1: Preparation of ultra-thin TiO2 nanosheets with anatase exposed (001) crystal plane by hydrothermal method

[0075] Add 12ml of Ti(OBu)4 and 4ml of 6.39mol / L HF to a 50ml polytetrafluoroethylene-lined autoclave, mix well, and add 20ml of anhydrous ethanol to mix well again. Move the autoclave to an oven and react at 180℃ for 18h. Wash the solid product after the reaction with 0.1M NaOH, anhydrous ethanol and deionized water in turn and filter. After repeating 3 times, place the filtered sample in a vacuum drying oven at 60℃ and dry it for 12h to obtain ultrathin TiO2 nanosheets.

[0076] Step 2: The ultra-thin TiO2 nanosheets with exposed (001) crystal plane prepared in step 1 were mixed with NaBH4 at a molar ratio of 1:1 and ground for 30 min. The ground mixture was placed in a tube furnace and calcined at 400 °C for 3 h to obtain black ultra-thin TiO2 nanosheets rich in OVs. 2-X Nanosheets;

[0077] Step 3: Synthesis of Cu by photoreduction y Ni 1-y Loaded TiO 2-X :

[0078] Take 1.17g of TiO prepared in step 2 2-X, 0.59mmol CuSO4·5H2O and 0.41mmol NiCl2 were dissolved in 50ml water to form a mixed solution. After degassing, the mixed solution was photoreduced with a xenon lamp. The light source was a 300W xenon lamp, which was about 20cm away from the surface of the mixed solution. The irradiation time was 60min, and Cu 0.59 Ni 0.41 -TiO 2-X .

[0079] The elemental composition of the product obtained in step 3 was determined by ICP elemental analysis. The results showed that the actual ratio of metal CuNi in the product and its content in TiO 2-X The loading amount on the nanosheets is consistent with the preset composition, and the product can be labeled as 5wt% Cu 0.59 Ni 0.41 -TiO 2-X .

[0080] Example 3

[0081] 5wt%Cu 0.71 Ni 0.29 -TiO 2-X The preparation steps of photocatalyst are as follows:

[0082] Step 1: Preparation of ultra-thin TiO2 nanosheets with anatase exposed (001) crystal plane by hydrothermal method

[0083] Add 12ml of Ti(OBu)4 and 4ml of 6.39mol / L HF to a 50ml polytetrafluoroethylene-lined autoclave, mix well, and add 20ml of anhydrous ethanol to mix well again. Move the autoclave to an oven and react at 180℃ for 18h. Wash the solid product after the reaction with 0.1M NaOH, anhydrous ethanol and deionized water in turn and filter. After repeating 3 times, place the filtered sample in a vacuum drying oven at 60℃ and dry it for 12h to obtain ultrathin TiO2 nanosheets.

[0084] Step 2: The ultra-thin TiO2 nanosheets with exposed (001) crystal plane prepared in step 1 were mixed with NaBH4 at a molar ratio of 1:1 and ground for 30 min. The ground mixture was placed in a tube furnace and calcined at 400 °C for 3 h to obtain black ultra-thin TiO2 nanosheets rich in OVs. 2-X Nanosheets;

[0085] Step 3: Synthesis of Cu by photoreduction y Ni 1-y Loaded TiO 2-X :

[0086] Take 1.18g of TiO prepared in step 2 2-X, 0.71mmol CuSO4·5H2O and 0.29mmol NiCl2 were dissolved in 48ml water to form a mixed solution. After degassing, the mixed solution was photoreduced with a xenon lamp. The light source was a 300W xenon lamp, which was about 30cm away from the surface of the mixed solution. The irradiation time was 60min, and Cu 0.71 Ni 0.29 -TiO 2-X .

[0087] The elemental composition of the product obtained in step 3 was determined by ICP elemental analysis. The results showed that the actual ratio of metal CuNi in the product and its content in TiO 2-X The loading amount on the nanosheets is consistent with the preset composition, and the product can be labeled as 5wt% Cu 0.71 Ni 0.29 -TiO 2-X .

[0088] Example 4

[0089] 3wt%Cu 0.59 Ni 0.41 -TiO 2-X The preparation steps of photocatalyst are as follows:

[0090] Step 1: Preparation of ultra-thin TiO2 nanosheets with anatase exposed (001) crystal plane by hydrothermal method

[0091] Add 12ml of Ti(OBu)4 and 4ml of 6.39mol / L HF to a 50ml polytetrafluoroethylene-lined autoclave, mix well, and add 20ml of anhydrous ethanol to mix well again. Move the autoclave to an oven and react at 180℃ for 18h. Wash the solid product after the reaction with 0.1M NaOH, anhydrous ethanol and deionized water in turn and filter. After repeating 3 times, place the filtered sample in a vacuum drying oven at 60℃ and dry it for 12h to obtain ultrathin TiO2 nanosheets.

[0092] Step 2: The ultra-thin TiO2 nanosheets with exposed (001) crystal plane prepared in step 1 were mixed with NaBH4 at a molar ratio of 1:1 and ground for 30 min. The ground mixture was placed in a tube furnace and calcined at 400 °C for 3 h to obtain black ultra-thin TiO2 nanosheets rich in OVs. 2-X Nanosheets;

[0093] Step 3: Synthesis of Cu by photoreduction y Ni 1-y Loaded TiO 2-X :

[0094] Take 1.99g of TiO prepared in step 2 2-X, 0.59mmol CuSO4·5H2O and 0.41mmol NiCl2 were dissolved in 48ml water to form a mixed solution. After degassing, the mixed solution was photoreduced with a xenon lamp. The light source was a 300W xenon lamp, which was about 25cm away from the surface of the mixed solution. The irradiation time was 50min, and Cu 0.59 Ni 0.41 -TiO 2-X .

[0095] The elemental composition of the product obtained in step 3 was determined by ICP elemental analysis. The results showed that the actual ratio of metal CuNi in the product and its content in TiO 2-X The loading amount on the nanosheets is consistent with the preset composition, and the product can be labeled as 3wt% Cu 0.59 Ni 0.41 -TiO 2-X .

[0096] Example 5

[0097] 7wt%Cu 0.59 Ni 0.41 -TiO 2-X The preparation steps of photocatalyst are as follows:

[0098] Step 1: Preparation of ultra-thin TiO2 nanosheets with anatase exposed (001) crystal plane by hydrothermal method

[0099] Add 12ml of Ti(OBu)4 and 4ml of 6.39mol / L HF to a 50ml polytetrafluoroethylene-lined autoclave, mix well, and add 20ml of anhydrous ethanol to mix well again. Move the autoclave to an oven and react at 180℃ for 18h. Wash the solid product after the reaction with 0.1M NaOH, anhydrous ethanol and deionized water in turn and filter. After repeating 3 times, place the filtered sample in a vacuum drying oven at 60℃ and dry it for 12h to obtain ultrathin TiO2 nanosheets.

[0100] Step 2: The ultra-thin TiO2 nanosheets with exposed (001) crystal plane prepared in step 1 were mixed with NaBH4 at a molar ratio of 1:1 and ground for 30 min. The ground mixture was placed in a tube furnace and calcined at 400 °C for 3 h to obtain black ultra-thin TiO2 nanosheets rich in OVs. 2-X Nanosheets;

[0101] Step 3: Synthesis of Cu by photoreduction y Ni 1-y Loaded TiO 2-X :

[0102] Take 0.81g of TiO prepared in step 2 2-X, 0.59mmol CuSO4·5H2O and 0.41mmol NiCl2 were dissolved in 50ml water to form a mixed solution. After degassing, the mixed solution was photoreduced with a xenon lamp. The light source was a 300W xenon lamp, which was about 25cm away from the surface of the mixed solution. The irradiation time was 70min, and Cu 0.59 Ni 0.41 -TiO 2-X .

[0103] The elemental composition of the product obtained in step 3 was determined by ICP elemental analysis. The results showed that the actual ratio of metal CuNi in the product and its content in TiO 2-X The loading amount on the nanosheets is consistent with the preset composition, and the product is marked as 7wt% Cu 0.59 Ni 0.41 -TiO 2-X .

[0104] Example 6

[0105] Preparation of 5wt% Cu using MgH2 as reducing agent 0.59 Ni 0.41 -TiO 2-X (MgH2), the steps are as follows:

[0106] Step 1: Preparation of ultra-thin TiO2 nanosheets with anatase exposed (001) crystal plane by hydrothermal method

[0107] The preparation steps are the same as step 1 of Example 1.

[0108] Step 2: The ultra-thin TiO2 nanosheets with exposed (001) crystal plane prepared in step 1 were mixed with MgH2 at a molar ratio of 1:1 and ground for 30 minutes. The ground mixture was placed in a tube furnace and calcined in an Ar atmosphere at 500°C for 8 hours. The obtained material was stirred in dilute HCl (10wt%) for 1 day to remove Mg, then washed and dried to obtain a black ultra-thin TiO2 nanosheet rich in OVs. 2-X (MgH2) nanosheets;

[0109] Step 3: Synthesis of Cu by photoreduction y Ni 1-y Loaded TiO 2-X :

[0110] Take 1.17g of TiO prepared in step 2 2-X (MgH2), 0.59mmol CuSO4·5H2O and 0.41mmol NiCl2 were dissolved in 50ml water to form a mixed solution. After degassing, the mixed solution was photoreduced with a xenon lamp. The light source was a 300W xenon lamp, which was about 20cm away from the surface of the mixed solution. The irradiation time was 60min, and Cu0.59 Ni 0.41 -TiO 2-X (MgH2).

[0111] The elemental composition of the product obtained in step 3 was determined by ICP elemental analysis. The results showed that the actual ratio of metal CuNi in the product and its content in TiO 2-X The loading amount on the (MgH2) nanosheets is consistent with the preset composition, and the product is marked as 5wt% Cu 0.59 Ni 0.41 -TiO 2-X (MgH2).

[0112] Example 7

[0113] Preparation of 5wt% Cu using H2 as reducing agent 0.59 Ni 0.41 -TiO 2-X (H2), the steps are as follows:

[0114] Step 1: Preparation of ultra-thin TiO2 nanosheets with anatase exposed (001) crystal plane by hydrothermal method

[0115] The preparation steps are the same as step 1 of Example 1.

[0116] Step 2: The ultra-thin TiO2 nanosheets with exposed (001) crystal plane prepared in step 1 were ground for 30 min and placed in a tube furnace. They were calcined in a H2 flow at 500 °C for 3 h under normal pressure to obtain black ultra-thin TiO2 nanosheets rich in OVs. 2-X (H2) nanosheets;

[0117] Step 3: Synthesis of Cu by photoreduction y Ni 1-y Loaded TiO 2-X :

[0118] Take 1.17g of TiO prepared in step 2 2-X (H2), 0.59mmol CuSO4·5H2O and 0.41mmol NiCl2 were dissolved in 50ml water to form a mixed solution. After degassing, the mixed solution was photoreduced with a xenon lamp. The light source was a 300W xenon lamp, which was about 20cm away from the surface of the mixed solution. The irradiation time was 60min, and Cu 0.59 Ni 0.41 -TiO 2-X (H2).

[0119] The elemental composition of the product obtained in step 3 was determined by ICP elemental analysis. The results showed that the actual ratio of metal CuNi in the product and its content in TiO 2-XThe loading amount on the nanosheets is consistent with the preset composition, and the product is marked as 5wt% Cu 0.59 Ni 0.41 -TiO 2-X (H2).

[0120] Example 8

[0121] 5wt%Cu 0.59 Co 0.41 -TiO 2-X The preparation steps of photocatalyst are as follows:

[0122] Step 1: Preparation of ultra-thin TiO2 nanosheets with anatase exposed (001) crystal plane by hydrothermal method

[0123] The preparation steps are the same as step 1 of Example 1.

[0124] Step 2: The ultra-thin TiO2 nanosheets with exposed (001) crystal plane prepared in step 1 were mixed with NaBH4 at a molar ratio of 1:1 and ground for 30 min. The ground mixture was placed in a tube furnace and calcined at 400 °C for 3 h to obtain black ultra-thin TiO2 nanosheets rich in OVs. 2-X Nanosheets;

[0125] Step 3: Synthesis of Cu by photoreduction y Co 1-y Loaded TiO 2-X :

[0126] Take 1.17g of TiO prepared in step 2 2-X , 0.59mmol CuSO4·5H2O and 0.41mmol Co(NO3)2 were dissolved in 50ml water to form a mixed solution. After degassing, the mixed solution was photoreduced with a xenon lamp. The light source was a 300W xenon lamp, which was about 20cm away from the surface of the mixed solution. The irradiation time was 60min, and Cu 0.59 Co 0.41 -TiO 2-X .

[0127] The elemental composition of the product obtained in step 3 was determined by ICP elemental analysis. The results showed that the actual ratio of metal CuCo in the product and its content in TiO 2-X The loading amount on the nanosheets is consistent with the preset composition of 5wt% Cu 0.59 Co 0.41 -TiO 2-X .

[0128] Example 9

[0129] 5wt%Cu 0.59 Fe 0.41 -TiO2-X The preparation steps of photocatalyst are as follows:

[0130] Step 1: Preparation of ultra-thin TiO2 nanosheets with anatase exposed (001) crystal plane by hydrothermal method

[0131] The preparation steps are the same as step 1 of Example 1.

[0132] Step 2: The ultra-thin TiO2 nanosheets with exposed (001) crystal plane prepared in step 1 were mixed with NaBH4 at a molar ratio of 1:1 and ground for 30 min. The ground mixture was placed in a tube furnace and calcined at 400 °C for 3 h to obtain black ultra-thin TiO2 nanosheets rich in OVs. 2-X Nanosheets;

[0133] Step 3: Synthesis of Cu by photoreduction y Fe 1-y Loaded TiO 2-X :

[0134] Take 1.17g of TiO prepared in step 2 2-X , 0.59mmol CuSO4·5H2O and 0.41mmol FeCl3 were dissolved in 50ml water to form a mixed solution. After degassing, the mixed solution was photoreduced with a xenon lamp. The light source was a 300W xenon lamp, which was about 20cm away from the surface of the mixed solution. The irradiation time was 60min, and Cu 0.59 Fe 0.41 -TiO 2-X .

[0135] The elemental composition of the product obtained in step 3 was determined by ICP elemental analysis. The results showed that the actual ratio of metal CuFe in the product and its content in TiO 2-X The loading amount on the nanosheets is consistent with the preset composition, and the product can be labeled as 5wt% Cu 0.59 Fe 0.41 -TiO 2-X .

[0136] Comparative Example 1

[0137] The preparation steps of conventional non-ultrathin TiO2 are as follows:

[0138] In a 50ml polytetrafluoroethylene-lined autoclave, add 12ml of Ti(OBu)4 and 4ml of 6.39mol / L HF, mix well, and then add 20ml of deionized water to mix well again. Move the autoclave to an oven and react at 180℃ for 18h. Wash the solid product after the reaction with 0.1M NaOH, anhydrous ethanol and deionized water in turn and filter. After repeating 3 times, place the filtered sample in a vacuum drying oven at 60℃ and dry it for 12h to obtain conventional non-ultrathin TiO2, recorded as TiO2(2).

[0139] Comparative Example 2

[0140] 5wt%Ni-TiO 2-X The preparation steps of photocatalyst are as follows:

[0141] Step 1: Preparation of ultra-thin TiO2 nanosheets with anatase exposed (001) crystal plane by hydrothermal method

[0142] The preparation steps are the same as step 1 of Example 1.

[0143] Step 2: The ultra-thin TiO2 nanosheets with exposed (001) crystal plane prepared in step 1 were mixed with NaBH4 at a molar ratio of 1:1 and ground for 30 min. The ground mixture was placed in a tube furnace and calcined at 400 °C for 3 h to obtain black ultra-thin TiO2 nanosheets rich in OVs. 2-X Nanosheets;

[0144] Step 3: Synthesis of Ni-loaded TiO by photoreduction 2-X :

[0145] Take 1.12g of TiO prepared in step 2 2-X and 1mmol NiCl2 were dissolved in 45ml water to form a mixed solution. After degassing, the mixed solution was photoreduced with a xenon lamp. The light source was a 300W xenon lamp, which was about 20cm away from the surface of the mixed solution. The irradiation time was 50min to obtain 5wt% Ni-TiO 2-X .

[0146] The elemental composition of the product obtained in step 3 was determined by ICP elemental analysis. The results showed that the metal Ni in the product was 2-X The loading amount on the nanosheets is consistent with the preset composition. The product can be labeled as 5wt% Ni-TiO 2-X .

[0147] Comparative Example 3

[0148] 5wt%Cu-TiO 2-X The preparation steps of photocatalyst are as follows:

[0149] Step 1: Preparation of ultra-thin TiO2 nanosheets with anatase exposed (001) crystal plane by hydrothermal method

[0150] The preparation steps are the same as step 1 of Example 1.

[0151] Step 2: The ultra-thin TiO2 nanosheets with exposed (001) crystal plane prepared in step 1 were mixed with NaBH4 at a molar ratio of 1:1 and ground for 30 min. The ground mixture was placed in a tube furnace and calcined at 400 °C for 3 h to obtain black ultra-thin TiO2 nanosheets rich in OVs. 2-X Nanosheets;

[0152] Step 3: Synthesis of Cu-loaded TiO by photoreduction 2-X :

[0153] Take 1.21g of TiO prepared in step 2 2-X and 1mmol CuSO4·5H2O were dissolved in 50ml water to form a mixed solution. After degassing, the mixed solution was photoreduced with a xenon lamp. The light source was a 300W xenon lamp, which was about 20cm away from the surface of the mixed solution. The irradiation time was 60min to obtain Cu-TiO 2-X .

[0154] The elemental composition of the product obtained in step 3 was determined by ICP elemental analysis. The results showed that the metal Cu in the product was 2-X The loading amount on the nanosheets is consistent with the preset composition. The product can be labeled as 5wt% Cu-TiO 2-X .

[0155] Comparative Example 4

[0156] 1wt%Pt-TiO 2-X The preparation steps of photocatalyst are as follows:

[0157] Step 1: Preparation of ultra-thin TiO2 nanosheets with anatase exposed (001) crystal plane by hydrothermal method

[0158] The preparation steps are the same as step 1 of Example 1.

[0159] Step 2: The ultra-thin TiO2 nanosheets with exposed (001) crystal plane prepared in step 1 were mixed with NaBH4 at a molar ratio of 1:1 and then fully ground. The ground mixture was placed in a tube furnace and calcined at 400 °C for 3 h to obtain black ultra-thin TiO2 nanosheets rich in OVs. 2-X Nanosheets;

[0160] Step 3: Synthesis of Pt-loaded TiO by photoreduction 2-X :

[0161] Take 3.71g of TiO prepared in step 22-X and 1mmol H2PtCl6 were dissolved in 48ml water to form a mixed solution. After degassing, the mixed solution was photoreduced with a xenon lamp. The light source was a 300W xenon lamp, which was about 25cm away from the surface of the mixed solution. The irradiation time was 70min to obtain Pt-TiO 2-X .

[0162] The elemental composition of the product obtained in step 3 was determined by ICP elemental analysis. The results showed that the metal Pt in the product was 2-X The loading amount on the nanosheets is consistent with the preset composition, and the product can be labeled as 1wt% Pt-TiO 2-X .

[0163] Comparative Example 5

[0164] 5wt%Cu 0.59 Bi 0.41 -TiO 2-X The preparation steps of photocatalyst are as follows:

[0165] Step 1: Preparation of ultra-thin TiO2 nanosheets with anatase exposed (001) crystal plane by hydrothermal method

[0166] The preparation steps are the same as step 1 of Example 1.

[0167] Step 2: The ultra-thin TiO2 nanosheets with exposed (001) crystal plane prepared in step 1 were mixed with NaBH4 at a molar ratio of 1:1 and ground for 30 min. The ground mixture was placed in a tube furnace and calcined at 400 °C for 3 h to obtain black ultra-thin TiO2 nanosheets rich in OVs. 2-X Nanosheets;

[0168] Step 3: Synthesis of Cu by photoreduction y Bi 1-y Loaded TiO 2-X :

[0169] Take 2.33g of TiO prepared in step 2 2-X , 0.59mmol CuSO4·5H2O and 0.41mmol BiCl3 were dissolved in 50ml water to form a mixed solution. After degassing, the mixed solution was photoreduced with a xenon lamp. The light source was a 300W xenon lamp, which was about 20cm away from the surface of the mixed solution. The irradiation time was 60min, and Cu 0.59 Bi 0.41 -TiO 2-X .

[0170] The elemental composition of the product obtained in step 3 was determined by ICP elemental analysis. The results showed that the actual ratio of metal CuBi in the product and its content in TiO 2-XThe loading amount on the nanosheets is consistent with the preset composition, and the product can be labeled as 5wt% Cu 0.59 Bi 0.41 -TiO 2-X .

[0171] Comparative Example 6

[0172] 5wt%Cu 0.59 Zn 0.41 -TiO 2-X The preparation steps of photocatalyst are as follows:

[0173] Step 1: Preparation of ultra-thin TiO2 nanosheets with anatase exposed (001) crystal plane by hydrothermal method

[0174] The preparation steps are the same as step 1 of Example 1.

[0175] Step 2: The ultra-thin TiO2 nanosheets with exposed (001) crystal plane prepared in step 1 were mixed with NaBH4 at a molar ratio of 1:1 and ground for 30 min. The ground mixture was placed in a tube furnace and calcined at 400 °C for 3 h to obtain black ultra-thin TiO2 nanosheets rich in OVs. 2-X Nanosheets;

[0176] Step 3: Synthesis of Cu by photoreduction y Zn 1-y Loaded TiO 2-X :

[0177] Take 1.22g of TiO prepared in step 2 2-X , 0.59mmol CuSO4·5H2O and 0.41mmol ZnCl2 were dissolved in 50ml water to form a mixed solution. After degassing, the mixed solution was photoreduced with a xenon lamp. The light source was a 300W xenon lamp, which was about 20cm away from the surface of the mixed solution. The irradiation time was 60min, and Cu 0.59 Zn 0.41 -TiO 2-X .

[0178] The elemental composition of the product obtained in step 3 was determined by ICP elemental analysis. The results showed that the actual ratio of metal CuZn in the product and its content in TiO 2-X The loading amount on the nanosheets is consistent with the preset composition, and the product can be labeled as 5wt% Cu 0.59 Zn 0.41 -TiO 2-X .

[0179] Test Example 1

[0180] Characterization of morphology, structure and composition

[0181] Figure 1 The ultrathin titanium dioxide TiO2 nanosheets prepared in step 1 of Example 1 (referred to as TiO2(1)) and the TiO2 nanosheets prepared in step 2 of Example 1 are 2-X And the X-ray diffraction (XRD) pattern and Raman (Raman) spectrum of the conventional non-ultrathin TiO2 (referred to as TiO2 (2)) prepared in Comparative Example 1, wherein (a) is the XRD pattern and (b) is the Raman spectrum. Figure 1 As shown in (a), TiO2(1), TiO2(2) and TiO 2-X The crystal morphology of TiO2 is anatase (JCPDS No. 21-1272). Its anatase crystal form does not change after reduction with NaBH4. Compared with TiO2(1), the peak corresponding to the (004) diffraction plane of TiO2(2) is higher, indicating that the thickness of the titanium dioxide flakes in the (001) direction of TiO2(2) is thicker. The peak corresponding to the (200) diffraction plane of TiO2(1) is higher, indicating that TiO2(1) has more exposed (001) crystal planes. Raman spectroscopy was used to study the crystal phase of TiO2 and the exposure percentage of the (001) crystal plane. Figure 1 As shown in (b), all TiO2 samples have a peak at 144.2, 396.0, 517.5 and 637.0 cm -1 The peaks at correspond to E g , B 1g , A 1g and E g The four Raman peaks once again confirm that the TiO2 samples are in the form of anatase, which is consistent with the XRD results. g , B 1g , A 1g They are caused by the symmetric stretching vibration, symmetric bending vibration and antisymmetric bending vibration of O-Ti-O in TiO2. The higher the percentage of (001) crystal plane exposure, the smaller the number of corresponding O-Ti-O symmetric stretching vibration modes, while the symmetric bending vibration and antisymmetric bending vibration increase relatively. 1g / E g The larger the value of , the higher the percentage of exposed (001) faces. Figure 1 (b) Raman spectra show that TiO 2-2 and TiO 2-X Sample B 1g and A 1g / E g The values ​​are significantly increased. Calculation shows that the TiO2(1)(001) crystal plane has an exposure ratio of 78%, while TiO2(2) has only 11%.

[0182] Figure 2The TiO2 prepared in step 1 of Example 1 (referred to as TiO2(1)) and the TiO2 prepared in step 2 of Example 1 2-X Electron paramagnetic resonance (EPR) spectroscopy. Oxygen vacancies are vacancies of oxygen atoms in the crystal structure, with unpaired free electrons. In the EPR test, materials with unpaired electrons will undergo energy level transitions under the action of magnetic fields and microwaves, showing specific spectral lines. Figure 2 It can be seen that after NaBH4 reduction calcination, TiO 2-X Compared with TiO2(1), the sample showed a g value of 2.004 from Ti 3+ The very strong EPR signal of the spin indicates that TiO 2-X A large number of oxygen vacancy defects were introduced during the thermal reduction process.

[0183] Figure 3 The Cu with different CuNi loading ratios prepared in Examples 1-3 and Comparative Examples 2-3 Y Ni 1-Y -TiO 2-X (TiO 2-X The XRD patterns of the product prepared in step 2 of Example 1 are compared. Figure 3 As shown, after loading Cu nanoparticles, Cu-TiO 2-X The corresponding diffraction peak of Cu(111) diffraction plane was observed in the TiO 2-X The crystal form of anatase TiO2 does not change. Y Ni 1-Y -TiO 2-X In the XRD spectrum of Ni-TiO, there are no separate Cu(111) and Ni diffraction peaks, indicating that CuNi exists in the form of an alloy rather than in the form of Cu particles and Ni particles. 2-X No diffraction peak of metallic nickel was observed in the sample because Ni usually has a weak diffraction peak and is amorphous in nature.

[0184] Figure 4 The TiO prepared in step 2 of Example 1 2-X SEM image (a) and TEM image (b). Figure 4 The SEM image of (a) shows that TiO 2-X The nanosheets are stacked in layers (the thickness of the nanosheets is about 6 nm). Figure 4 From the TEM image (b), it can be seen that transparency profiles were found in the nanoflakes, which can be attributed to their small thickness (i.e., ultrathin). Two sets of mutually perpendicular lattice fringes were observed on the front side of the nanoflakes with the same d-spacing of 0.19 nm, which can be attributed to the (200) and (020) planes.

[0185] Figure 5 The Cu prepared in Example 2 0.59 Ni 0.41 -TiO 2-X SEM images from Figure 5 It can be observed that after loading metal nanoparticles, the surface of the material shows well-dispersed small black spots. These black spots are alloy metal particles, which exist in the form of surface loading.

[0186] Figure 6 The Cu prepared in Example 2 0.59 Ni 0.41 -TiO 2-X Element mapping test results (ae) and EDS spectrum (f). Figure 6 (ae) It can be seen that metal nanoparticles exist and are uniformly loaded on the TiO 2-X The material surface is also Figure 6 (f) It can be seen that in addition to TiO 2-X In addition to the material, there are also Cu and Ni.

[0187] Test Example 2

[0188] Light absorption performance

[0189] Figure 7 The TiO2 prepared in step 1 of Example 1 (referred to as TiO2(1)) and the TiO2 prepared in step 2 of Example 1 are 2-X And the Cu prepared in Example 2 0.59 Ni 0.41 -TiO 2-X Ultraviolet-visible absorption (UV-vis) spectrum (a) and VB-XPS graph (b). Photocatalytic activity of semiconductors and bandgap width E g From the UV-vis graph, it can be seen that after CuNi bimetal loading, Cu 0.59 Ni 0.41 -TiO 2-X The material has strong absorption in the visible light region, Cu 0.59 Ni 0.41 -TiO 2-X The band gap is significantly smaller than that of ultra-thin TiO2(1), and the narrow band gap is more conducive to improving the performance of photocatalytic hydrogen production from glucose conversion. 2-X , Cu 0.59 Ni 0.41 -TiO 2-X The bandgap widths are 3.07, 2.34 and 2.62 eV respectively. It can be seen that the presence of OVs effectively reduces the 2-X The bandgap width of Cu 0.59Ni 0.41 -TiO 2-X The VB and CB positions are 2.11 eV and -0.56 eV, respectively, which meet the potential requirements for both the ability to oxidize glucose and photocatalytic hydrogen production.

[0190] Effect Example 1

[0191] Experiment on hydrogen production by photocatalytic decomposition of glucose.

[0192] Test method:

[0193] 200 mg of photocatalyst was dispersed in 200 ml of glucose aqueous solution (the preparation method of glucose aqueous solution was: 2 g of glucose was added to every 200 ml of deionized water to form a glucose aqueous solution with a concentration of 0.056 mol / L), and the solution was transferred to a 300 ml photoreactor (Labsolar IIIAG, Beijing Perfectlight) and sealed. N2 was blown into the reactor before the reaction to remove air from the solution. The photocatalytic reaction was irradiated with a 300 W xenon lamp (PLS-SXE-300C, Beijing Perfectlight) as a simulated light source, and the temperature of the photocatalytic system was maintained at room temperature by flowing cooling water. A gas chromatograph (GC9790) with N2 as carrier gas was used to regularly detect the photocatalytic gas product H2.

[0194] Test results:

[0195] Figure 8 The Cu loaded with bimetallic materials of different ratios prepared in Examples 1-3 y Ni 1-y -TiO 2-X (metal loading is 5 wt%), single metal loaded Ni-TiO prepared in Comparative Examples 2-3 2-X and Cu-TiO 2-X (the metal loading is 5 wt%), TiO2 prepared in step 1 of Example 1 (referred to as TiO2(1)), and TiO2 prepared in step 2 of Example 1 2-X The curve of hydrogen production changing with time; Fig. 9 The Cu loaded with bimetallic materials of different ratios prepared in Examples 1-3 x Ni 1-x -TiO 2-X , Single metal loaded Ni-TiO prepared in Comparative Example 2-3 2-X and Cu-TiO 2-X , TiO2 prepared in step 1 of Example 1 (referred to as TiO2(1)) and TiO2 prepared in step 2 of Example 1 2-X The hydrogen production rate; Fig.10Cu with different bimetallic loadings prepared in Examples 2, 4-5 0.59 Ni 0.41 -TiO 2-X Compared with 1wt% Pt-TiO prepared in Comparative Example 4 2-X The hydrogen production rate; Fig.11 5wt% Cu prepared in Example 2 0.59 Ni 0.41 -TiO 2-X , 5wt% Cu prepared in Example 8 0.59 Co 0.41 -TiO 2-X , 5wt% Cu prepared in Example 9 0.59 Fe 0.41 -TiO 2-X , 5wt% Cu prepared in Comparative Example 5 0.59 Bi 0.41 -TiO 2-X And the 5wt% Cu prepared in Comparative Example 6 0.59 Zn 0.41 -TiO 2-X The hydrogen production rate; Fig.12 5wt% Cu prepared in Example 2 0.59 Ni 0.41 -TiO 2-X Example 6 Preparation of 5wt% Cu 0.59 Ni 0.41 -TiO 2-X (MgH2) and 5wt% Cu prepared in Example 7 0.59 Ni 0.41 -TiO 2-X (H2) hydrogen production rate; Fig.13 5wt% Cu prepared in Example 2 under different pH conditions 0.59 Ni 0.41 -TiO 2-X Glucose is the most common monosaccharide in nature and was used as the main substrate for photocatalytic hydrogen production in this experiment. Figure 8 It shows that the unloaded metal TiO 2-X The hydrogen production is lower than that of monometallic or bimetallic supported TiO 2-X Hydrogen production. Fig. 9 It can be seen that under the same metal loading, Cu 0.59 Ni 0.41 -TiO 2-X The hydrogen production rate is the best, which is 389.88 μmol·g -1 ·h -1 .Depend on Fig.10It can be seen that with the increase of metal loading, the photocatalytic hydrogen production shows a trend of first increasing and then decreasing. When the bimetallic loading is low, more active sites can be introduced with the increase of loading, thus increasing the hydrogen production of H2. However, the gradual increase in loading will cause metal particles to agglomerate, thereby reducing the production of H2. Compared with the hydrogen production of 1wt% Pt loaded with precious metal under the same conditions, it can be seen that 5wt% Cu 0.59 Ni 0.41 -TiO 2-X The hydrogen production is slightly higher than that of 1wt% Pt-TiO 2-X , and has more cost advantages. Fig.11 It can be seen that under the condition of unchanged photocatalytic conditions, 5wt% Cu 0.59 Fe 0.41 -TiO 2-X and 5wt%Cu 0.59 Co 0.41 -TiO 2-X It also exhibits a higher hydrogen production rate, but is slightly lower than that of 5wt% Cu 0.59 Ni 0.41 -TiO 2-X . And 5wt%Cu 0.59 Bi 0.41 -TiO 2-X and 5wt%Cu 0.59 Zn 0.41 -TiO 2-X The hydrogen production rate is far less than that of 5wt% Cu 0.59 Fe 0.41 -TiO 2-X , 5wt%Cu 0.59 Co 0.41 -TiO 2-X and 5wt%Cu 0.59 Ni 0.41 -TiO 2-X This is because Fe, Co, and Ni are all transition metal elements of the fourth period, group VIII, and have similar atomic structures and chemical properties, especially similar orbital electron configurations. Therefore, Fe, Co, and Ni have similar MH (metal-hydrogen) binding energies, and the MH bond is neither too strong nor too weak, which is conducive to the formation of reaction intermediates (H + Bonded to the catalyst surface to form reaction intermediates) and molecular hydrogen. However, the binding of metal Bi and metal Zn to H is significantly weaker than that of Fe, Co, and Ni, which is not conducive to the formation of reaction intermediates, so the hydrogen production performance is poor. Fig.12 It can be seen that under the condition of unchanged photocatalytic conditions, 5wt% Cu prepared by using MgH2 and H2 as reducing agents 0.59 Ni 0.41 -TiO 2-X(MgH2) and 5wt%Cu 0.59 Ni 0.41 -TiO 2-X (H2) shows a similar 0.59 Ni 0.41 -TiO 2-X Comparable hydrogen production performance. Fig.13 It can be seen that when the photocatalytic conditions remain unchanged, the hydrogen production increases with the increase of pH. This is because there are more hydroxyl radicals in a higher pH environment, which helps the photocatalytic oxidation of glucose to proceed in the forward reaction direction, and is more conducive to charge separation and water reduction hydrogen production effect.

[0196] The oxidation products of glucose were determined by LC-MS. The LC-MS spectrum is shown in Fig.14 As shown. Fig.14 It can be seen that the peaks at m / z 195, 179 and 89 correspond to gluconic acid C6H 11 O7 - , glucose C6H 11 O6 - and lactic acid C3H5O3 - The molecular ion peaks of 119 and 60 in the figure are C4H7O4 produced by the breakage of the C2-C3 bond of the glucose molecule. - and C2H5O2 - The peak at m / z 97 is the molecular ion peak of H2SO4. Since the photocatalytic reaction in the experiment is a strong alkaline environment, adding H2SO4 solution after the reaction can make the solution acidic and prevent the reaction from continuing.

[0197] 5wt% Cu after one reaction 0.59 Ni 0.41 -TiO 2-X The SEM image of (prepared in Example 2) is as follows Fig.15 As shown. Fig.15 It can be seen that the stacking morphology of the flakes did not change after the reaction (the SEM image before the reaction is shown in Figure 5 As shown), the presence of CuNi metal nanoparticles was also observed in the form of surface loading.

[0198] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A modified titanium dioxide photocatalyst, characterized in that: The invention comprises a carrier and an active component loaded on the carrier; the carrier is a titanium dioxide nanosheet containing oxygen vacancies; the active component is an alloy nanoparticle; the alloy nanoparticle is a CuNi alloy nanoparticle, a CuCo alloy nanoparticle or a CuFe alloy nanoparticle.

2. The modified titanium dioxide photocatalyst according to claim 1, characterized in that The titanium dioxide nanosheets containing oxygen vacancies are anatase-type titanium dioxide.

3. The modified titanium dioxide photocatalyst according to claim 1, characterized in that The molar ratio of Cu to another metal in the alloy nanoparticles is 0.4:0.6-0.8:0.

2.

4. The method for preparing the modified titanium dioxide photocatalyst according to claim 3, characterized in that: The following steps are involved: Anatase titanium dioxide nanosheets are prepared by a hydrothermal method; the anatase titanium dioxide nanosheets are reduced by a reducing agent to obtain titanium dioxide nanosheets containing oxygen vacancies; alloy nanoparticles are loaded on the titanium dioxide nanosheets containing oxygen vacancies by a photoreduction method to obtain the modified titanium dioxide photocatalyst.

5. The preparation method according to claim 4, characterized in that: The reducing agent includes sodium borohydride, hydrogen or MgH2.

6. The preparation method according to claim 5, characterized in that: The reducing agent is sodium borohydride, and the specific reduction operation is: mixing the anatase titanium dioxide nanosheets with sodium borohydride and grinding for 20-40 minutes, and calcining to obtain the titanium dioxide nanosheets containing oxygen vacancies.

7. The preparation method according to claim 6, characterized in that: The mass ratio of the anatase titanium dioxide nanosheets to sodium borohydride is 1:0.8-1.3; the calcination temperature is 350-410° C., and the calcination time is 2-4 hours.

8. The preparation method according to claim 4, characterized in that: The method of loading alloy nanoparticles on the titanium dioxide nanosheets containing oxygen vacancies by photoreduction includes: mixing the titanium dioxide nanosheets containing oxygen vacancies with a metal source and water to obtain a mixed solution, and then performing a photoreduction reaction under irradiation of a light source.

9. The preparation method according to claim 8, characterized in that: The intensity of the light source is 300W, and the irradiation time of the light source is 50-70 minutes.

10. Use of the modified titanium dioxide photocatalyst according to any one of claims 1 to 3 in photocatalytic glucose reforming to produce hydrogen.

Citation Information

Patent Citations

  • TiO2 photocatalyst for photocatalytic reforming biomass hydrogen preparation and preparation and application

    CN101884914A

Cited By

  • Copper-based catalyst as well as preparation method and application thereof

    CN119588352A

  • Rare noble metal / Ti (at) TiO2-x self-supporting gas purification material, preparation and application thereof and air purifier

    CN120771858A