Testing device and testing method for micro-motion crevice corrosion between metal fasteners

By designing a micro-claw corrosion test device for testing metal fasteners, the problem of the inability of the prior art to simulate fastener wear and corrosion coupling is solved, and efficient testing of fasteners in aerospace equipment is achieved, and the equipment is extended service life.

CN118980632APending Publication Date: 2024-11-19UNIV OF SCI & TECH BEIJING
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411078845.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing test system cannot test the coupling between micro-wear and crevice corrosion of metal fasteners at the same time and in the same area, and cannot accurately simulate the wear and corrosion environment of aluminum alloy fasteners for aerospace during actual service.

Method used

A test device for corrosion of micro-moving gaps between metal fasteners is designed, including upper and lower metal samples, electrochemical reaction cells, reference electrodes and counter electrodes. The micro-moving motion is achieved through the voice coil motor, combined with a six-dimensional mechanical sensor. and stepper motors, simulate the micro-movement wear and crevice corrosion environment in the aircraft structure, and conduct electrochemical testing.

Benefits of technology

The device can test the coupling between micro-corrosion and crevice corrosion in a corrosive environment, provides important data for fastener material selection and maintenance of aerospace equipment, extends the service life of the fastener, and is suitable for medical use and metal fasteners in marine environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118980632A_ABST
    Figure CN118980632A_ABST
Patent Text Reader

Abstract

The embodiment of the invention relates to a testing device for micro-crevice corrosion between metal fasteners and a testing method of the testing device, and belongs to the technical field of electrochemical corrosion. The embodiment of the invention aims to solve the technical problem that an existing testing system cannot test fretting wear and crevice corrosion at the same time in the same area. The testing device for micro crevice corrosion between the metal fasteners comprises an upper metal sample and a lower metal sample, the lower metal sample is fixed in an electrochemical reaction tank, a NaCl solution is contained in the electrochemical reaction tank, a reference electrode and a counter electrode are further arranged in the electrochemical reaction tank, and the upper metal sample and the lower metal sample are arranged in the electrochemical reaction tank. The upper metal sample is at least partially immersed in the NaCl solution and is in contact with the lower metal sample to jointly form a working electrode, and the upper metal sample, the lower metal sample, the reference electrode and the counter electrode jointly form a three-electrode testing system and are electrically connected with an electrochemical workstation. The testing device provided by the embodiment of the invention is suitable for testing fretting wear (corrosion) and fretting corrosion in artificial gaps.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The embodiments of the present application relate to the field of electrochemical corrosion technology, and in particular to a test device and a test method for micro-motion crevice corrosion between metal fasteners. Background Art

[0002] For decades, aluminum alloys have been the cornerstone of the aerospace industry. Their unique combination of properties makes them ideal materials for manufacturing aircraft and spacecraft. The main alloy series include 5xxx, 6xxx, 2xxx and 7xxx series. Aluminum alloys have a low density. Using aluminum alloys can reduce the total weight of an aircraft, improve fuel efficiency and load capacity. At the same time, after alloying and heat treatment, the strength and hardness of aluminum alloys can be significantly improved, and they can be used in high-load and vibration environments. In recent years, although composite materials have been widely used in the aerospace field, high-strength aluminum alloys still play an indispensable role. The use of aluminum alloys in aerospace applications ranges from structural components to engine components, providing a balance between performance and cost-effectiveness. However, in the aerospace industry, millions of rivets and bolts are required in the assembly operation of aircraft structures. In addition, in the harsh aerospace environment, aircraft may be affected by various climatic conditions and wear and corrosion.

[0003] Fretting wear refers to a composite type of wear caused by small amplitude vibration between metal surfaces that are pressed against each other. It usually occurs at the tight-fitting journals; the fitting of turbine and compressor blades; the joints of bolts, rivets and other fasteners affected by vibration. The fretting wear process is as follows: the contact pressure causes the micro-convex bodies on the surface of the friction pair to produce plastic deformation and adhesion. Under the action of small amplitude vibration from the outside, the adhesion points are sheared, the adhesion falls off, and the sheared surface is oxidized. During the wear process, the wear debris is not easy to be discharged. These wear debris act as abrasives and accelerate the process of fretting wear. This long-term cycle eventually leads to the destruction of the surface of the parts. The main feature of fretting wear is the presence of colored spots on the friction surface, which are filled with pressed oxides. If the fretting wear products are difficult to be discharged from the contact area, and the volume of the corrosion products often expands, the local contact pressure increases, which can lead to the bonding of the parts and even the seizure. Fretting wear between metal materials of implanted prostheses in the human body may cause metal ions to enter the human body and cause physiological reactions such as poisoning. Wear depressions under the fastener heads can cause joints to loosen, greatly reducing the service life of fasteners such as riveted and bolted connections.

[0004] When metal parts are in the medium, due to the formation of particularly small gaps between metal and metal or metal and non-metal, the medium in the gap is in a stagnant state, causing accelerated corrosion of the metal in the gap. This local corrosion is called crevice corrosion. Crevice corrosion often occurs in holes, gasket contact surfaces, lap joints, under sediments, fastener interface gaps and other places.

[0005] As far as fasteners are concerned, the gaps at the fastening interfaces and the harsh service environment of the aircraft provide the prerequisites for crevice corrosion. More seriously, during the service of the aircraft, the mechanical parts are tightly matched. Under load and certain frequency vibration conditions, the micro friction between the fastener interfaces will lead to micro-motion wear. The displacement of this micro-motion friction is very small, generally in the micron level. If crevice corrosion occurs, the micro displacement is not enough to allow the relatively closed corrosion environment in the crevice to exchange substances with the outside world. Therefore, the corrosion environment in the crevice can be maintained, but the friction and wear between the contact surfaces will lead to more serious corrosion problems.

[0006] In addition, as a basic component of aviation equipment, aluminum alloys are often exposed to rain, seawater and other corrosive environments. Generally speaking, a stable passivation film will naturally form on the surface of aluminum alloys, which can prevent corrosion damage to aluminum alloys. However, during the service of aluminum alloy fasteners, the vibration of the fuselage will cause micro-wear between the fasteners, resulting in the rupture of the passivation film. Frequent wear and abrasion will remove the protective coating or damage the surface of the aluminum alloy, making it more susceptible to corrosion. When friction occurs under corrosive conditions, friction corrosion will occur. In fact, this corrosion process is affected by both mechanical and electrochemical factors. It is a coupling of the two, and it is a mutually reinforcing coupling, which accelerates both corrosion and wear, and further shortens the service life.

[0007] Studying the fretting wear at the interface of aluminum alloy fasteners for aerospace can detect the laws of fasteners under the coupling of fretting wear and crevice corrosion, evaluate the corrosion resistance of aerospace fasteners, and guide the material selection and maintenance of aluminum alloy fasteners for aerospace, which is of great significance for the replacement and maintenance of fasteners. However, most of the current experimental devices conduct single fretting wear experiments and crevice corrosion experiments, which cannot accurately simulate the coupling conditions of aluminum alloy fasteners in actual service. Therefore, it is necessary to construct an experimental test device that can reproduce the coupled service conditions of wear and corrosion at the interface of fasteners, and design corresponding experimental methods. Summary of the invention

[0008] In view of this, an embodiment of the present application provides a test device and a test method for fretting corrosion between metal fasteners. The test device is suitable for testing fretting wear (corrosion) and fretting corrosion in artificial gaps to solve the technical problem that the existing test system cannot test fretting wear and crevice corrosion at the same time and in the same area.

[0009] A first aspect of an embodiment of the present application provides a test device for micro-motion crevice corrosion between metal fasteners, comprising an upper metal sample and a lower metal sample, wherein the lower metal sample is fixed in an electrochemical reaction cell, wherein the electrochemical reaction cell contains a NaCl solution, and wherein a reference electrode and a counter electrode are also provided in the electrochemical reaction cell, wherein the reference electrode and the counter electrode are immersed in the NaCl solution, wherein the upper metal sample is at least partially immersed in the NaCl solution and contacts the lower metal sample to jointly constitute a working electrode, wherein the upper metal sample, the lower metal sample, the reference electrode and the counter electrode jointly constitute a three-electrode test system and are electrically connected to an electrochemical workstation.

[0010] In some embodiments that may include the above embodiments, micro-protrusions are provided at the bottom of the upper metal sample, and the micro-protrusions are located between the upper metal sample and the lower metal sample to form an artificial gap.

[0011] In some embodiments that may include the above embodiments, the electrochemical reaction cell is fixed to the module slider by screws, and a voice coil motor is installed at one end of the module slider.

[0012] In some embodiments that may include the above embodiments, the voice coil motor is externally connected to a controller, and the controller is used to control the voice coil motor to perform reciprocating motion, and the voice coil motor in turn drives the lower metal sample in the electrochemical reaction cell to perform reciprocating motion.

[0013] In some embodiments that may include the above-mentioned embodiments, the upper metal sample is fixed on a six-dimensional mechanical sensor through an upper clamp, the six-dimensional mechanical sensor is fixedly connected to a mechanical cantilever beam, the mechanical cantilever beam is fixedly connected to a support frame of an optical platform, and the support frame is arranged perpendicular to the optical platform, and the optical platform is used to support the voice coil motor and the module slider.

[0014] In some embodiments that may include the above embodiments, the mechanical cantilever beam is also connected to a stepper motor, and the stepper motor is used to control the mechanical cantilever beam to move up and down, so that the upper metal sample moves closer to / away from the lower metal sample.

[0015] In some embodiments that may include the above embodiments, the counter electrode is a platinum sheet electrode; and the reference electrode is an Ag / AgCl electrode.

[0016] In some embodiments that may include the above embodiments, the electrochemical reaction cell and the upper clamp are both made of PEEK material.

[0017] In some embodiments that may include the above embodiments, the upper metal sample and the lower metal sample are both made of aluminum alloy.

[0018] A second aspect of the embodiment of the present application further provides a test method for fretting crevice corrosion between metal fasteners, which is completed using the above-mentioned test device for fretting crevice corrosion between metal fasteners, and includes the following steps:

[0019] Step 1, preparing an upper metal sample and a lower metal sample, and performing preliminary processing on the upper metal sample, that is, processing it into an upper metal sample with micro-convex bodies by a CNC machine tool, wherein the micro-convex bodies are located between the upper metal sample and the lower metal sample to form an artificial gap;

[0020] Step 2, preparing a NaCl solution to simulate the marine atmospheric environment, and injecting an appropriate amount of the NaCl solution into the electrochemical reaction cell;

[0021] Step 3, fixing the lower metal sample in an electrochemical reaction cell, wherein the electrochemical reaction cell contains a NaCl solution, and the upper metal sample is at least partially immersed in the NaCl solution and in contact with the lower metal sample to form a working electrode together. The electrochemical reaction cell is also provided with a reference electrode and a counter electrode, wherein the reference electrode and the counter electrode are immersed in the NaCl solution. The upper metal sample, the lower metal sample, the reference electrode and the counter electrode together form a three-electrode test system, and the three electrodes are connected to an electrochemical workstation via wires;

[0022] Step 4, fix the electrochemical reaction cell on the module slider by screws, a voice coil motor is installed on one end of the module slider, the voice coil motor is externally connected to a controller, the controller is used to control the voice coil motor to reciprocate, and the voice coil motor drives the lower metal sample in the electrochemical reaction cell to reciprocate, fix the voice coil motor and the module slider on an optical platform, and place and fix the optical platform perpendicular to the upper fixture;

[0023] Step 5, fix the upper metal sample on the six-dimensional mechanical sensor through the upper clamp, the six-dimensional mechanical sensor is fixedly connected to the mechanical cantilever beam, the mechanical cantilever beam is fixedly connected to the support frame of the optical platform, and the support frame is arranged perpendicular to the optical platform, the mechanical cantilever beam is also connected to a stepper motor, and the stepper motor is used to adjust the position of the mechanical cantilever beam so that the upper metal sample and the lower metal sample are in the same vertical line;

[0024] Step 6: Lower the mechanical cantilever beam by controlling the stepper motor so that the upper metal sample and the lower metal sample are in contact and maintain the load;

[0025] Step 7: After the upper metal sample and the lower metal sample are in contact, the voice coil motor is controlled by the controller to perform micro-movement, so that the upper metal sample and the lower metal sample are worn with a relative displacement of micrometer level;

[0026] Step 8, while performing step 7, electrochemical testing is performed by adjusting the electrochemical workstation, and the result measured at this time is the coupling result of fretting corrosion and crevice corrosion;

[0027] After the test of step 9 and step 8 is completed, the solution in the electrochemical reaction cell is preserved and its ion concentration is tested; at the same time, the upper metal sample and the lower metal sample are taken out and the surface morphology is observed, and the wear volume and corrosion morphology are measured.

[0028] Compared with the prior art, the embodiments of the present application have the following beneficial effects:

[0029] The embodiments of the present application provide a testing device and scheme for the coupling effect of fretting corrosion and crevice corrosion on the interface of metal fasteners in a corrosive environment. The device is suitable for testing fretting wear (corrosion) and fretting corrosion in artificial crevice, and aims to solve the dilemma that the existing testing system cannot test fretting wear and crevice corrosion at the same time and in the same area, and provides a testing device and scheme for the study of fretting crevice corrosion of aviation aluminum alloy equipment; it can be applied to the field of medical implants, as well as metal fasteners serving in marine environments (carrier-based aircraft fasteners, ships, marine oil and gas equipment, etc., which have certain gaps and small relative displacements). BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0031] Figure 1 A schematic diagram of the structure of a test device for fretting crevice corrosion between metal fasteners according to an embodiment of the present application;

[0032] Figure 2 A schematic diagram of the structure of an upper metal specimen and a lower metal specimen in a test device for fretting crevice corrosion between metal fasteners according to an embodiment of the present application;

[0033] Figure 3 This is a laser confocal image of the micro-convex body in Example 1;

[0034] Figure 4 is a light microscope image of the artificial slit formed in Example 1;

[0035] Figure 5 This is the SEM image of the corrosion morphology in Example 1.

[0036] Description of reference numerals:

[0037] 1. Six-dimensional mechanical sensor; 2. Upper fixture; 3. Upper metal sample; 4. Lower metal sample; 5. Electrochemical reaction cell; 6. Mechanical cantilever beam; 7. Voice coil motor; 8. NaCl solution; 9. Reference electrode; 10. Counter electrode; 11. Screw; 12. Module slider; 13. Micro-protrusion; 14. Artificial gap. DETAILED DESCRIPTION

[0038] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0039] First, those skilled in the art should understand that these implementations are only used to explain the technical principles of the present application and are not intended to limit the scope of protection of the present application. Those skilled in the art can make adjustments to them as needed to adapt to specific application scenarios.

[0040] Secondly, it should be noted that in the description of the present application, terms such as "up", "down", "left", "right", "front", "back", "inside" and "outside" indicating directions or positional relationships are based on the directions or positional relationships shown in the drawings. This is merely for the convenience of description and does not indicate or imply that the device or component must have a specific orientation, be constructed and operated in a specific orientation. Therefore, it should not be understood as a limitation on the present application.

[0041] The existing testing system in the related technology cannot test the technical problem of micro-wear and crevice corrosion in the same area at the same time.

[0042] Example 1

[0043] In order to solve the above technical problems, Figure 1 and Figure 2 As shown, an embodiment of the present application provides a test device for micro-motion crevice corrosion between metal fasteners, including an upper metal sample 3 and a lower metal sample 4, the lower metal sample 4 is fixed in an electrochemical reaction cell 5, the electrochemical reaction cell 5 is filled with a NaCl solution 8, and a reference electrode 9 and a counter electrode 10 are also provided in the electrochemical reaction cell 5, the reference electrode 9 and the counter electrode 10 are immersed in the NaCl solution 8, the upper metal sample 3 is at least partially immersed in the NaCl solution 8 and contacts the lower metal sample 4 to jointly form a working electrode, the upper metal sample 3, the lower metal sample 4, the reference electrode 9 and the counter electrode 10 jointly form a three-electrode test system and are electrically connected to the electrochemical workstation.

[0044] Exemplarily, the upper metal sample 3 is processed by a CNC lathe, and the clamping section connected to the upper fixture 2 is a cylinder with a diameter of 10 mm and a length of 15 mm. The lower end is made into a 45° cone with a length of 5 mm. The bottom of the cone is a circular platform with a diameter of 3 mm. There is also a micro-protrusion 13 with a diameter of 300 um in the center of the platform. The height of the micro-protrusion 13 can be controlled between 10-300 um, that is, the width of the artificial gap 14 formed can be precisely adjusted; the upper metal sample 3 is connected to the wire and is connected to the electrochemical workstation through the wire.

[0045] Exemplarily, the lower metal sample 4 is a disc with a diameter of 15 mm and a thickness of 3 mm, which is encapsulated in epoxy resin. Specifically, after machining, the surface rust layer is removed by rough mechanical polishing, the wire is soldered on the back, and the conductivity between the sample and the far end of the wire is tested by a multimeter. The PVC pipe mold (height 6 mm, diameter Φ25 mm) and the sample facing down in the center are fixed on the horizontal plane by double-sided tape, and the sample wire extends from the through hole on one side of the PVC pipe mold; the anhydrous ethylenediamine and epoxy resin uniformly mixed in a fixed proportion are poured into the PVC pipe mold, the bubbles are removed, and the mixture is left to stand for a period of time. After the epoxy resin mixture is fixed, the encapsulated sample is formed. The encapsulated sample is pre-processed, and mechanical polishing is performed with 1000#, 1500#, 3000#, and 5000# sandpaper in turn, and then mechanically polished to a mirror surface, rinsed with deionized water and alcohol, and dried with cold air from a hair dryer. The lower metal sample 4 is encapsulated in epoxy resin, and a concave groove is provided in the electrochemical reaction cell 5 to fix the lower metal sample 4.

[0046] Exemplarily, the counter electrode 10 is a platinum sheet electrode; the reference electrode 9 is an Ag / AgCl electrode. More specifically, the lower metal sample 4 is fixed in a concave groove inside the electrochemical reaction cell 5, the wire is led out and connected to the working electrode chuck of the electrochemical workstation, the Ag / AgCl electrode is used as the reference electrode 9, and the 10×10×3mm platinum sheet is used as the counter electrode 10.

[0047] In a specific embodiment, a micro-protrusion 13 is provided at the bottom of the upper metal sample 3, and the micro-protrusion 13 is located between the upper metal sample 3 and the lower metal sample 4 to form an artificial gap 14, and the width of the artificial gap 14 and the ratio of the inner and outer areas of the artificial gap 14 can be artificially controlled (by controlling the height of the micro-protrusion 13 and the bottom end surface area of ​​the upper metal sample 3).

[0048] Exemplarily, after the micro-protrusions 13 of the upper metal sample 3 and the lower metal sample 4 are in contact and the load is maintained, the width of the formed artificial gap 14 can be photographed by an industrial CCD camera.

[0049] Specifically, the electrochemical reaction cell 5 is fixed on the module slider 12 by means of screws 11 , and a voice coil motor 7 is installed at one end of the module slider 12 .

[0050] Exemplarily, the voice coil motor 7 is externally connected to a controller (not shown in the figure), which is used to control the voice coil motor 7 to perform reciprocating motion. The voice coil motor 7 then drives the lower metal sample 4 in the electrochemical reaction cell 5 to perform reciprocating motion. The frequency, displacement and motion type of the micro-motion are adjustable.

[0051] Specifically, the upper metal sample 3 is fixed on the six-dimensional mechanical sensor 1 through the upper clamp 2, the six-dimensional mechanical sensor 1 is fixedly connected to the mechanical cantilever beam 6, the mechanical cantilever beam 6 is fixedly connected to the support frame of the optical platform, and the support frame is arranged perpendicular to the optical platform, and the optical platform is used to support the voice coil motor 7 and the module slider 12.

[0052] The voice coil motor 7 and the module slider 12 are fixed on the optical platform, and the entire optical platform is placed under the mechanical cantilever beam 6. During assembly, the upper fixture 2 is ensured to be vertical to the optical platform.

[0053] Exemplarily, the mechanical cantilever beam 6 is also connected to a stepper motor (not shown in the figure), which is used to control the up and down displacement of the mechanical cantilever beam 6, so that the upper metal sample 3 moves closer to / away from the lower metal sample 4 and maintains the selected load. At the same time, the friction data during the movement process can be collected in real time.

[0054] Exemplarily, the electrochemical reaction cell 5 is fixed on the module slider 12, and the NaCl solution 8 is injected into the electrochemical reaction cell 5. The stepper motor controls the mechanical cantilever beam 6 to move downward, thereby driving the upper metal sample 3 to move downward and contact the lower metal sample 4. At this time, the actual situation is that the micro-convex body 13 of the upper metal sample 3 is in contact with the lower metal sample 4, and the plane where the micro-convex body 13 is located and the plane of the lower metal sample 4 are artificial gaps 14. Therefore, the width of the artificial gap 14 can be adjusted by controlling the height of the micro-convex body 13.

[0055] Exemplarily, the electrochemical reaction cell 5 and the upper fixture 2 are both made of PEEK material to ensure their insulation and inertness.

[0056] Exemplarily, the upper metal sample 3 and the lower metal sample 4 are both made of aluminum alloy.

[0057] The test device for micro-motion crevice corrosion between metal fasteners of this embodiment is composed of three systems. The first is the micro-motion power system, which mainly includes the voice coil motor module (voice coil motor 7 and module slider 12), the controller of the voice coil motor 7 (which can also include the control software for controlling the controller). The second is the mechanical test and control system, which mainly includes the six-dimensional mechanical sensor 1, the stepper motor (which can also include the operating software for controlling the stepper motor). The last part is the electrochemical reaction cell 5 and the electrochemical test system. The electrochemical reaction cell 5 is fixed on the voice coil motor module, and the voice coil motor 7 pushes the module slider 12 and drives the electrochemical reaction cell 5 to make micro-motions of different frequencies.

[0058] During the test, electrochemical pretreatment was first performed by applying a potential of -0.8V vs Ag / AgCl for 300s to clean the sample surface; then the open circuit potential was maintained for 30min, and an anode potential greater than the open circuit potential of 100mV was applied after the sample surface was stabilized.

[0059] During the electrochemical test, the voice coil motor 7 is controlled by the controller to drive the lower metal sample 4 to perform a sinusoidal motion with a displacement of 50um and a frequency of 1Hz. At this time, there is a micro-slip between the micro-protrusions 13 of the upper metal sample 3 and the surface of the lower metal sample 4, and this slip occurs at the center of the artificial gap 14.

[0060] During the test, the electrochemical data such as the potential and current during the test are recorded by the electrochemical workstation, the mechanical data such as the load and friction are recorded by the six-dimensional mechanical sensor 1, and the kinematic data such as the theoretical displacement, actual displacement and actual speed are recorded by the voice coil motor 7.

[0061] After the test, the macro-microscopic corrosion morphology and corrosion degree were characterized by laser confocal microscopy, artificial gap light microscopy, SEM, etc. The results are as follows Figure 3-5 shown.

[0062] The present application can study the micro-corrosion (micro-motion crevice corrosion) in the crevices of aluminum alloy under different loads, different displacements (amplitudes), different frequencies, and different periods. The applied load and time can also be controlled. The voice coil motor 7 can control the micro-motion displacement (amplitude) and frequency.

[0063] The present application can also study the influence of different gap widths and different gap inner and outer area ratios on micro-motion gap corrosion; the width of the artificial gap 14 can be adjusted by controlling the height of the micro-protrusion 13. By changing the area of ​​the bottom surface of the upper metal sample 3 where the micro-protrusion 13 is located and the area of ​​the lower metal sample 4, the influence of different gap inner and outer area ratios can be measured.

[0064] Example 2

[0065] The present application embodiment provides a test method for fretting crevice corrosion between metal fasteners, which is completed using the test device for fretting crevice corrosion between metal fasteners in Example 1, and includes the following steps:

[0066] Step 1, prepare an upper metal sample 3 and a lower metal sample 4, and perform preliminary processing on the upper metal sample 3, that is, process it into an upper metal sample 3 with micro-convex bodies 13 by a CNC machine tool, and the micro-convex bodies 13 are located between the upper metal sample 3 and the lower metal sample 4 to form an artificial gap 14;

[0067] Step 2: prepare a NaCl solution 8 to simulate the marine atmosphere environment, and inject an appropriate amount of the NaCl solution 8 into the electrochemical reaction cell 5;

[0068] Step 3, fix the lower metal sample 4 in the electrochemical reaction cell 5, wherein the electrochemical reaction cell 5 is filled with a NaCl solution 8, and the upper metal sample 3 is at least partially immersed in the NaCl solution 8 and in contact with the lower metal sample 4 to form a working electrode together, and a reference electrode 9 and a counter electrode 10 are also provided in the electrochemical reaction cell 5, and the reference electrode 9 and the counter electrode 10 are immersed in the NaCl solution 8, and the upper metal sample 3, the lower metal sample 4, the reference electrode 9 and the counter electrode 10 together form a three-electrode test system, and the three electrodes are connected to the electrochemical workstation through wires;

[0069] Step 4, fix the electrochemical reaction cell 5 on the module slider 12 by means of screws 11, a voice coil motor 7 is installed at one end of the module slider 12, the voice coil motor 7 is externally connected to a controller, the controller is used to control the voice coil motor 7 to reciprocate, and the voice coil motor 7 then drives the lower metal sample 4 in the electrochemical reaction cell 5 to reciprocate, fix the voice coil motor 7 and the module slider 12 on an optical platform, and place and fix the optical platform perpendicular to the upper fixture 2;

[0070] Step 5, fix the upper metal sample 3 on the six-dimensional mechanical sensor 1 through the upper fixture 2, the six-dimensional mechanical sensor 1 is fixedly connected to the mechanical cantilever beam 6, the mechanical cantilever beam 6 is fixedly connected to the support frame of the optical platform, and the support frame is arranged perpendicular to the optical platform, the mechanical cantilever beam 6 is also connected to a stepper motor, and the stepper motor is used to adjust the position of the mechanical cantilever beam 6 so that the upper metal sample 3 and the lower metal sample 4 are in the same vertical line;

[0071] Step 6: lower the mechanical cantilever beam 6 by controlling the stepper motor so that the upper metal sample 3 and the lower metal sample 4 are in contact and maintain the load;

[0072] Step 7, after the upper metal sample 3 and the lower metal sample 4 are in contact, the voice coil motor 7 is controlled by the controller to perform micro-movement, so that the upper metal sample 3 and the lower metal sample 4 are worn with a relative displacement of micrometer level;

[0073] Step 8, while performing step 7, electrochemical testing is performed by adjusting the electrochemical workstation, and the result measured at this time is the coupling result of fretting corrosion and crevice corrosion;

[0074] After the test of step 9 and step 8 is completed, the solution in the electrochemical reaction cell 5 is preserved and its ion concentration is tested; at the same time, the upper metal sample 3 and the lower metal sample 4 are taken out and the surface morphology is observed, and the wear volume and corrosion morphology are measured.

[0075] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.

Claims

1. A test device for fretting crevice corrosion between metal fasteners, characterized in that: The invention comprises an upper metal sample (3) and a lower metal sample (4), wherein the lower metal sample (4) is fixed in an electrochemical reaction cell (5), wherein the electrochemical reaction cell (5) contains a NaCl solution (8), and wherein a reference electrode (9) and a counter electrode (10) are also arranged in the electrochemical reaction cell (5), wherein the reference electrode (9) and the counter electrode (10) are immersed in the NaCl solution (8), wherein the upper metal sample (3) is at least partially immersed in the NaCl solution (8) and contacts the lower metal sample (4) to form a working electrode together, wherein the upper metal sample (3), the lower metal sample (4), the reference electrode (9) and the counter electrode (10) together form a three-electrode test system and are electrically connected to an electrochemical workstation.

2. The test device for fretting crevice corrosion between metal fasteners according to claim 1, characterized in that: A micro-convex body (13) is arranged at the bottom of the upper metal sample (3), and the micro-convex body (13) is located between the upper metal sample (3) and the lower metal sample (4) to form an artificial gap (14).

3. The test device for fretting crevice corrosion between metal fasteners according to claim 1, characterized in that: The electrochemical reaction cell (5) is fixed to a module slider (12) by means of screws (11), and a voice coil motor (7) is installed at one end of the module slider (12).

4. The test device for fretting crevice corrosion between metal fasteners according to claim 3, characterized in that: The voice coil motor (7) is externally connected to a controller, and the controller is used to control the voice coil motor (7) to perform reciprocating motion, and the voice coil motor (7) in turn drives the lower metal sample (4) in the electrochemical reaction cell (5) to perform reciprocating motion.

5. The test device for fretting crevice corrosion between metal fasteners according to claim 3, characterized in that: The upper metal sample (3) is fixed on the six-dimensional mechanical sensor (1) through the upper clamp (2), the six-dimensional mechanical sensor (1) is fixedly connected to the mechanical cantilever beam (6), the mechanical cantilever beam (6) is fixedly connected to the support frame of the optical platform, and the support frame is arranged perpendicular to the optical platform, and the optical platform is used to support the voice coil motor (7) and the module slider (12).

6. The test device for fretting crevice corrosion between metal fasteners according to claim 5, characterized in that: The mechanical cantilever beam (6) is also connected to a stepper motor, and the stepper motor is used to control the mechanical cantilever beam (6) to move up and down, so that the upper metal sample (3) moves towards / away from the lower metal sample (4).

7. The test device for fretting crevice corrosion between metal fasteners according to claim 1, characterized in that: The counter electrode (10) is a platinum sheet electrode; and the reference electrode (9) is an Ag / AgCl electrode.

8. The test device for fretting crevice corrosion between metal fasteners according to claim 5, characterized in that: The electrochemical reaction cell (5) and the upper clamp (2) are both made of PEEK material.

9. The test device for fretting crevice corrosion between metal fasteners according to claim 1, characterized in that: The upper metal sample (3) and the lower metal sample (4) are both made of aluminum alloy.

10. A test method for fretting crevice corrosion between metal fasteners, characterized in that: The test device for fretting crevice corrosion between metal fasteners according to any one of claims 1 to 9 is used, and the test method comprises the following steps: Step 1, preparing an upper metal sample (3) and a lower metal sample (4), and performing preliminary processing on the upper metal sample (3), that is, processing it into an upper metal sample (3) having micro-convex bodies (13) by a numerically controlled machine tool, wherein the micro-convex bodies (13) are located between the upper metal sample (3) and the lower metal sample (4) to form an artificial gap (14); Step 2, preparing a NaCl solution (8) to simulate the marine atmospheric environment, and injecting an appropriate amount of the NaCl solution (8) into the electrochemical reaction cell (5); Step 3, fixing the lower metal sample (4) in an electrochemical reaction cell (5), wherein the electrochemical reaction cell (5) contains a NaCl solution (8), and the upper metal sample (3) is at least partially immersed in the NaCl solution (8) and in contact with the lower metal sample (4) to form a working electrode together, and the electrochemical reaction cell (5) is also provided with a reference electrode (9) and a counter electrode (10), wherein the reference electrode (9) and the counter electrode (10) are immersed in the NaCl solution (8), and the upper metal sample (3), the lower metal sample (4), the reference electrode (9) and the counter electrode (10) together form a three-electrode test system, and the three electrodes are connected to an electrochemical workstation via wires; Step 4, fix the electrochemical reaction cell (5) on the module slider (12) by means of screws (11), a voice coil motor (7) is installed at one end of the module slider (12), the voice coil motor (7) is externally connected to a controller, the controller is used to control the voice coil motor (7) to perform reciprocating motion, the voice coil motor (7) further drives the lower metal sample (4) in the electrochemical reaction cell (5) to perform reciprocating motion, the voice coil motor (7) and the module slider (12) are both fixed on an optical platform, and the optical platform is placed and fixed perpendicular to the upper fixture (2); Step 5, fix the upper metal sample (3) on the six-dimensional mechanical sensor (1) through the upper clamp (2), the six-dimensional mechanical sensor (1) is fixedly connected to the mechanical cantilever beam (6), the mechanical cantilever beam (6) is fixedly connected to the support frame of the optical platform, and the support frame is arranged perpendicular to the optical platform, the mechanical cantilever beam (6) is also connected to a stepper motor, and the stepper motor is used to adjust the position of the mechanical cantilever beam (6) so that the upper metal sample (3) and the lower metal sample (4) are on the same vertical line; Step 6: lowering the mechanical cantilever beam (6) by controlling the stepper motor so that the upper metal sample (3) and the lower metal sample (4) are in contact and maintain the load; Step 7: After the upper metal sample (3) and the lower metal sample (4) are in contact, the voice coil motor (7) is controlled by the controller to perform micro-movement, so that the upper metal sample (3) and the lower metal sample (4) are worn with a relative displacement of micrometer level; Step 8: While performing step 7, an electrochemical test is performed by adjusting the electrochemical workstation. The result measured at this time is the coupling result of fretting corrosion and crevice corrosion; After the test of step 9 and step 8 is completed, the solution in the electrochemical reaction cell (5) is preserved and its ion concentration is tested; at the same time, the upper metal sample (3) and the lower metal sample (4) are taken out and the surface morphology is observed, and the wear volume and corrosion morphology are measured.

Citation Information

Cited By

  • Experimental device for corrosion of arc-shaped crevice between metal pipeline fasteners and experimental method of experimental device

    CN122448725A