Photo-thermal catalyst as well as preparation method and application thereof
By using a metal cluster-modified nano-zero-valent iron photothermal catalyst to reform waste polyethylene wax under sunlight, the high temperature, high pressure, and high energy consumption problems of traditional catalytic reforming technology have been solved, realizing the efficient and environmentally friendly conversion of resources into high-value fuels and lubricants.
Patent Information
- Application Number
- CN202411089116.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-22
AI Technical Summary
Existing technologies are insufficient to efficiently and environmentally convert waste polyethylene wax into high-value liquid fuels and lubricants. Traditional catalytic reforming technologies suffer from problems such as high temperature and pressure, high energy consumption, and high equipment costs.
Using metal cluster-modified nano-zero-valent iron materials as photothermal catalysts, waste polyethylene wax is converted into liquid fuel and lubricating oil under solar irradiation through photothermal reforming technology. The in-situ separation of products is achieved by utilizing the enhanced local plasma resonance effect of metal clusters.
It enables the efficient, environmentally friendly, and low-cost conversion of waste polyethylene wax into high-value gasoline, kerosene, and lubricating oil, thereby improving resource utilization and economic benefits while reducing environmental pollution.
Smart Images

Figure CN118988343A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of energy catalysis technology, and in particular to a photothermal catalyst and a preparation method and application thereof. Background Art
[0002] Polyethylene wax is an industrial product with the characteristics of high softening point and low viscosity. According to different sources, polyethylene wax can be divided into three types: polymerization type, cracking type and by-product type. Polymerization type polyethylene wax is produced through the ethylene polymerization process; cracking type polyethylene wax mainly comes from the cracking products of polyethylene resin or waste polyethylene plastic; by-product polyethylene wax is a by-product of the polyethylene production process. The molecular weight of polyethylene wax (1000-4000g / mol) is higher than that of paraffin-based lubricating oil (250-540g / mol), and it is difficult to be directly used as a lubricant in the fields of medicine and chemical industry. At the same time, the density of polyethylene wax is lower than that of polyethylene (3000-6000000g / mol), so it does not have the high melting point and thermal stability similar to polyethylene plastic, and cannot be used as daily necessities such as food packaging bags. In particular, the quality of by-product polyethylene wax is difficult to control, and its application range is very limited. With the increasing production of polyethylene plastics in the world, the output of by-product polyethylene wax has increased accordingly, and its market size has reached an annual output of more than 6 million tons. However, polyethylene wax is a surplus product in the current market, and its economic value and application range are very limited.
[0003] The key to improving the economic value of polyethylene wax is to improve its quality and expand its application range. The catalytic oxidation process can use oxidants (KMnO4, H2O2, O2) to introduce hydroxyl or carbonyl groups into polyethylene wax molecules to improve their wettability, dispersibility and resin compatibility. However, the emission of residual KMnO4 and H2O2 will cause environmental pollution; the greener O2 is limited by insufficient oxidation capacity, and the reaction usually requires high pressure and the use of catalysts (zinc stearate, tetrabutyl titanate and metallocene, etc.) to proceed. Compared with improving the performance of polyethylene wax, catalytic conversion of polyethylene wax provides a new idea for other high-value chemicals to increase their economic added value. Polyethylene wax can be cracked into hydrocarbon compounds with smaller molecular weight at high temperature, but CC bond cracking usually requires high temperature (400-1000℃) to occur, which not only increases the reaction cost, but also the uncontrollable cracking process will lead to overly complex product types and increase the difficulty of purification. Catalytic reforming is an important process in the oil refining process, in which catalysts induce long-chain hydrocarbon molecules to rearrange at relatively low reaction temperatures (200-600°C) to generate new substances, thereby increasing the added value of the products. Under heating, hydrogenation and catalyst conditions, crude oil (or naphtha) selectively breaks CC bonds and CH bonds and is converted into gasoline, kerosene, high-octane gasoline rich in aromatics, and liquefied petroleum gas. However, the high-temperature heating process consumes a large amount of fossil energy to provide energy, and the high-pressure conditions increase the operating costs of the equipment.
[0004] Solar energy is the most abundant and pollution-free clean energy on earth, and has great potential to replace traditional fossil energy. Under the background of the "dual carbon" policy, the use of photothermal catalytic technology to convert waste plastics is expected to fundamentally solve its surplus problem without generating additional energy consumption and carbon footprint. Patent CN202210551688.7 discloses a method for photothermal conversion of waste plastics into high-value-added fuels and environmental remediation materials using zero-valent iron. Zero-valent iron materials modified with oxygen-containing acid groups are used as catalysts for photothermal conversion of waste plastics. However, compared with polyethylene, waste polyethylene wax has a shorter molecular chain, a wider carbon number distribution, and better thermal stability. It is difficult for zero-valent iron modified with oxygen-containing acid groups to completely crack polyethylene wax, resulting in a low reforming rate, and the product is still a low-value, high-carbon wax. Therefore, it is urgent to develop efficient and green polyethylene wax reforming technology. Summary of the invention
[0005] The purpose of the present invention is to provide a photothermal catalyst and a preparation method and application thereof, and to photothermal catalytically reform waste polyethylene wax into liquid fuel and lubricating oil.
[0006] The objective of the present invention can be achieved through the following technical scheme: a photothermal catalyst, wherein the photothermal catalyst is a metal cluster-modified nano zero-valent iron material having a nanoscale scale, wherein the metal clusters exist in a loaded form, wherein the loaded metal clusters include but are not limited to d-zone and ds-zone transition metals, and the diameter of the metal cluster particles is between 0.5 and 5 nm.
[0007] Preferably, the d-block and ds-block transition metals include but are not limited to ruthenium, platinum, palladium, nickel, and copper.
[0008] Further preferably, the ruthenium content on the surface of the metal cluster-modified nano zero-valent iron material is 0.8wt% to 7.2wt%.
[0009] Further preferably, the content of platinum on the surface of the metal cluster modified nano zero-valent iron material is 1.0wt% to 6.0wt%.
[0010] Further preferably, the content of palladium on the surface of the metal cluster modified nano zero-valent iron material is 0.1wt% to 5.1wt%.
[0011] Further preferably, the nickel content on the surface of the metal cluster modified nano zero-valent iron material is 0.4wt% to 7.7wt%.
[0012] Further preferably, the copper content on the surface of the metal cluster modified nano zero-valent iron material is 0.5wt% to 6.8wt%.
[0013] Preferably, the metal cluster modified nano zero-valent iron material has an irregular nanowire structure at the nanoscale. The present invention uses the metal cluster modified nano zero-valent iron material as a catalyst for photothermal reforming of waste polyethylene wax, and the metal cluster modified nano zero-valent iron material has a nanoscale and irregular microscopic morphology.
[0014] Further preferably, the diameter of the metal cluster modified nano zero-valent iron material particles is between 50 and 300 nm.
[0015] A method for preparing the above-mentioned photothermal catalyst comprises the following steps:
[0016] 1) Using aqueous phase reduction technology, a sodium borohydride solution is dropped into a ferric chloride solution to obtain a nano zero-valent iron suspension;
[0017] 2) Using the self-organization method induced by nano-zero-valent iron, the metal chloride precursor aqueous solution is dropped into the nano-zero-valent iron suspension for immersion reduction. After the reaction is completed, the suspension is filtered, the solid is washed and dried in an inert atmosphere, and the metal cluster-modified nano-zero-valent iron material is collected.
[0018] Preferably, the concentration of the sodium borohydride solution in step 1) is 4-6 g / L, preferably 5 g / L, and the concentration of the ferric chloride solution is 1.5-2.5 g / L, preferably 2 g / L.
[0019] Preferably, in step 1), the flow rate of dripping the sodium borohydride aqueous solution into the ferric chloride aqueous solution is 25-35 mL / min, preferably 30 mL / min.
[0020] Preferably, the metal chloride precursor in step 2) includes ruthenium chloride, chloroplatinic acid, palladium chloride, nickel chloride, and copper chloride.
[0021] Preferably, in step 2), the metal chloride precursor aqueous solution is dripped into the nano zero-valent iron suspension at a flow rate of 4-6 mL / min, and the flow rate is preferably 5 mL / min.
[0022] Preferably, the immersion time in step 2) is 4 hours, and the drying time is 3 to 4 hours.
[0023] Preferably, the inert atmosphere in step 2) is nitrogen.
[0024] An application of the above-mentioned photothermal catalyst is to use the photothermal catalyst for photothermal reforming of waste polyethylene wax into liquid fuel and lubricating oil.
[0025] Preferably, the specific method is: uniformly mixing the photothermal catalyst with waste polyethylene wax, introducing an inert gas into a photothermal reactor, using a xenon lamp as a light source to simulate sunlight, and obtaining liquid fuel and lubricating oil as the products.
[0026] Further preferably, the specific method is: in a quartz atmospheric pressure photothermal reactor, a metal cluster-modified nano zero-valent iron material is used as a photothermal catalyst, which is evenly mixed with a waste polyethylene wax precursor, argon gas is introduced into the photothermal reactor, and a xenon lamp is used as a light source to simulate sunlight, and the obtained products are liquid fuel and lubricating oil.
[0027] Preferably, the liquid fuel and lubricating oil include C5-C 12 Light gasoline, C 13 -C 18 Kerosene and C 18 -C 36 Low carbon paraffin oil.
[0028] Preferably, the mass ratio of the photothermal catalyst to the waste polyethylene wax to be treated is 1:1 to 5:1.
[0029] Preferably, the photothermal reaction time is 3 to 15 hours.
[0030] More preferably, the photothermal reaction time is 3 to 12 hours.
[0031] Preferably, the light intensity of the photothermal reaction is 1 to 5 W / cm 2 .
[0032] In the present invention, the surface-loaded metal clusters can significantly enhance the solar energy utilization efficiency of the catalyst, have excellent photothermal effect and can efficiently crack the repeating structural unit (-CH2-). The key step of polyethylene wax cracking is the adsorption of atomic hydrogen in the molecule on the metal site, thereby providing a chemical driving force for the formation of new molecules. Since the Fe element's ability to adsorb hydrogen is weaker than that of precious metals (Ru, Pt, Pd, etc.), under the temperature-dependent physical phase change separation drive, polyethylene wax cracking is insufficient, resulting in the main product being a high-carbon hydrocarbon with lower value. Therefore, it is extremely challenging to develop efficient photothermal catalysts to realize the conversion of waste polyethylene wax into high-value low-carbon products.
[0033] In the present invention, the photothermal catalytic reforming technology realizes the resource utilization of waste polyethylene wax, a surplus product, and uses nano-iron materials with good light response to realize efficient reforming of waste polyethylene wax to obtain high-value gasoline, kerosene and lubricating oil under solvent-free and co-reactant-free conditions. The high temperature generated by the metal cluster-enhanced local plasma resonance effect and the temperature difference of the environment are used to realize in-situ separation of products, and the excellent hydrogen adsorption and cracking properties of precious metals are used to realize selective regulation of different components of the product. Compared with the traditional industrial thermal catalytic reforming technology, the present invention has created a precedent for the reforming of cluster-modified photothermal catalytic wax into high-value products, showing the strong vitality in the field of solar-driven solid waste resource utilization.
[0034] Compared with the prior art, the present invention has the following beneficial effects:
[0035] 1. The present invention provides a new photothermal catalyst that can reform waste polyethylene wax into liquid fuel and lubricating oil through photothermal catalysis.
[0036] 2. The present invention uses the self-organization method induced by nano zero-valent iron to successfully prepare a type of high-efficiency photothermal reforming catalyst for waste polyethylene wax. The catalyst can effectively photothermally reform waste polyethylene wax into liquid fuel and lubricating oil for a long time under solar irradiation.
[0037] 3. The metal loaded on the surface of the zero-valent iron of the present invention can improve the reforming rate of waste polyethylene wax and the selectivity of liquid fuel without changing the crystal structure of the zero-valent iron. A metal cluster-modified nano zero-valent iron photothermal catalyst with full solar spectrum response capability is prepared by an aqueous impregnation method.
[0038] 4. The present invention cleverly utilizes the ability of different transition metals to absorb atomic hydrogen, providing a new strategy for efficient, environmentally friendly, zero-carbon emission, and scalable photothermal reforming value-added of waste polyethylene wax. The liquid product can be used as gasoline and kerosene, and the solid product paraffin can be used as a material in daily necessities, medical care, construction, and chemical fields, thereby realizing the resource value-added of waste polyethylene wax.
[0039] 5. The present invention cleverly utilizes the temperature difference between the high temperature generated by the metal cluster enhanced local plasma resonance effect and the ambient temperature to achieve in-situ separation of the product.
[0040] 6. The metal cluster modified nano zero-valent iron photothermal catalytic material of the present invention uses less metal, which reduces the material cost and improves the economic benefit of the material.
[0041] 7. The material of the present invention is environmentally friendly, will not cause secondary pollution, and has a certain degree of recyclability.
[0042] 8. The present invention has low cost, no co-reactants, no need for external heat source, and has high economic benefits.
[0043] 9. The present invention provides a method for upgrading waste polyethylene wax into liquid fuel and lubricating oil by photothermal catalysis using metal cluster-modified nano zero-valent iron. The waste polyethylene wax is photothermally catalytically reformed using metal cluster-modified nano zero-valent iron material as a catalyst to achieve efficient preparation of liquid fuel and lubricating oil, with a total selectivity of more than 95% and a conversion rate of up to 88%. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 XRD patterns of zero-valent iron and metal cluster-modified nano-zero-valent iron;
[0045] Figure 2 SEM images of zero-valent iron and metal cluster-modified nano-zero-valent iron;
[0046] Figure 3 The C5-C 12 Light gasoline, C 13 -C 18 Kerosene and C 18 -C 36 Relative content of low carbon paraffin oil;
[0047] Figure 4 The photothermal conversion effect diagram of zero-valent iron and metal cluster-modified nano-zero-valent iron;
[0048] Figure 5 The reforming rate of waste polyethylene wax with zero-valent iron and metal cluster-modified nano-zero-valent iron at different photothermal reaction times;
[0049] Figure 6 The C5-C 12 Light gasoline, C 13 -C 18 Kerosene and C 18 -C 36 Changes in the content of low carbon paraffin oil;
[0050] Figure 7 The C5-C 12 Light gasoline, C 13 -C 18 Kerosene and C 18 -C 36 Changes in the content of low carbon paraffin oil;
[0051] Figure 8 The C5-C 12 Light gasoline, C 13 -C 18 Kerosene and C 18 -C 36 Low carbon paraffin oil content;
[0052] Fig. 9 The reforming rate of waste polyethylene wax after 5 hours of thermal reforming and photothermal catalytic reforming of metal cluster-modified nano zero-valent iron;
[0053] Fig.10 The content of lubricating oil and liquid fuel collected after 5 hours of photothermal reforming of waste polyethylene wax by metal cluster-modified nano zero-valent iron and waste polyethylene wax under unmixed and mixed conditions;
[0054] Fig.11 The content of lubricating oil and liquid fuel collected after 5 hours of photothermal reforming of waste polyethylene wax by metal single atom-modified nano-zero-valent iron and metal cluster-modified nano-zero-valent iron;
[0055] Fig.12 The content of lubricating oil and liquid fuel collected after 5 hours of photothermal reforming of waste polyethylene wax by various metal single atom-modified nano-zero-valent iron and metal cluster-modified nano-zero-valent iron;
[0056] Fig.13 C5-C prepared by oxygen-containing acid radical-modified zero-valent iron and metal cluster-modified nano-zero-valent iron 12 Light gasoline, C 13 -C 18 Kerosene and C 18 -C 36 Low carbon paraffin oil content;
[0057] Fig.14 C5-C was prepared by indium cluster-modified nano-zero-valent iron and d-block metal cluster-modified nano-zero-valent iron. 12 Light gasoline, C 13 -C 18 Kerosene and C 18 -C 36 Low carbon paraffin oil content;
[0058] Fig.15 The reforming rate of waste polyethylene wax after 5 hours of reforming with nano-zero-valent iron modified by zero-valent iron and metal clusters of platinum, palladium, nickel and copper;
[0059] Fig.16 This is the cycling performance diagram of metal cluster modified nano zero-valent iron materials. DETAILED DESCRIPTION
[0060] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to the following embodiments.
[0061] Unless otherwise specified, the reagents, methods, instruments and equipment used in the present invention are conventional reagents, methods, instruments and equipment in the art. Unless otherwise specified, the reagents and materials used in the following examples are commercially available.
[0062] In the following examples, polyethylene wax was purchased from Kangjin Plastic Additive Factory and produced as domestic NM94.
[0063] Example 1
[0064] A method for photothermal catalytic reforming of waste polyethylene wax into liquid fuel and lubricating oil by metal cluster modified nano zero-valent iron comprises the following steps:
[0065] S1 Preparation of metal cluster modified nano zero-valent iron: 1000mL 2g / L ferric chloride solution and 500mL 5g / L sodium borohydride solution were mixed for reaction. After the reaction was completed, 150mL 0.5g / L ruthenium chloride aqueous solution was dripped into the suspension at a rate of 5mL / min. After the reaction was completed, the suspension was filtered, the solid was washed and dried in an argon atmosphere for 3.5 hours, and the metal cluster modified nano zero-valent iron material was collected, wherein the surface ruthenium content was 7.1wt%.
[0066] S2 Photothermal reforming of waste polyethylene wax into high-value liquid fuel and lubricant: 0.1g polyethylene wax and 0.3g metal cluster modified nano zero-valent iron material obtained in step S1 were mixed evenly, argon was introduced into the photothermal reactor, and the oxygen content in the gas in the reactor was sampled and tested until the oxygen concentration was lower than the detection line. The simulated solar light source was turned on, and the waste polyethylene wax was photothermally reformed under different light intensities. The gas chromatography detected C5-C 12 Light gasoline, C 13 -C 18 Kerosene and C 18 -C 36 The content of low carbon paraffin oil and the reforming rate of waste polyethylene wax.
[0067] Comparative Example 1
[0068] A method for photothermal catalytic reforming of waste polyethylene wax using nano zero-valent iron comprises the following steps:
[0069] Preparation of S1 nano zero-valent iron: 1000 mL 2 g / L ferric chloride solution and 500 mL 5 g / L sodium borohydride solution were mixed and reacted. After aging, the suspension was filtered, the solid was washed and dried in an argon atmosphere for 3.5 hours, and the zero-valent iron material was collected.
[0070] S2 Photothermal reforming of waste polyethylene wax: 0.1g of waste polyethylene wax and 0.3g of zero-valent iron material obtained in step S1 were mixed evenly, argon gas was introduced into the photothermal reactor, and the oxygen content in the gas in the reactor was sampled and tested until the oxygen concentration was lower than the detection line. The simulated sunlight light source was turned on, and the waste polyethylene wax was photothermally reformed under different light intensities. The gas chromatography detected C5-C 12 Light gasoline, C 13 -C 18 Kerosene and C 18 -C 36 The content of low carbon paraffin oil and the reforming rate of waste polyethylene wax.
[0071] The zero-valent iron materials of Example 1 and Comparative Example 1 were tested:
[0072] Figure 1 The XRD diagrams of nano zero-valent iron and metal cluster-modified nano zero-valent iron; from the XRD diagrams, it can be seen that the main component of the synthetic material is zero-valent iron.
[0073] Figure 2 SEM images of nano-zero-valent iron and metal cluster-modified nano-zero-valent iron: From the SEM images, we can see that nano-zero-valent iron and metal cluster-modified nano-zero-valent iron both have irregular nanowire structures at the nanoscale, the diameter of metal cluster particles is 0.5-5nm, and the diameter of nano-zero-valent iron and metal cluster-modified nano-zero-valent iron material particles is 50-300nm. (Figure a is nano-zero-valent iron, and Figure b is ruthenium cluster-modified nano-zero-valent iron)
[0074] The experimental results of Example 1 and Comparative Example 1 are as follows:
[0075] Figure 3 In order to compare the photothermal reforming of waste polyethylene wax by nano-zero-valent iron and metal cluster-modified nano-zero-valent iron, the C5-C 12 Light gasoline, C 13 -C 18 Kerosene and C 18 -C 36 Low carbon paraffin oil content.
[0076] Figure 4 This is a diagram of the photothermal conversion effect of nano zero-valent iron and metal cluster-modified nano zero-valent iron.
[0077] Figure 5 Changes in the reforming rate of waste polyethylene wax with nano zero-valent iron and metal cluster-modified nano zero-valent iron at different photothermal reaction times.
[0078] Figure 6 The C5-C 12 Light gasoline, C 13 -C 18 Kerosene and C 18 -C 36 Changes in the content of low carbon paraffin oil.
[0079] Figure 7 The photothermal reforming of waste polyethylene wax by metal cluster-modified nano-zero-valent iron under different light intensities was performed. After 5 hours, C5-C 12 Light gasoline, C 13 -C 18 Kerosene and C 18 -C 36 Changes in the content of low carbon paraffin oil.
[0080] from Figure 3 and Figure 5It can be seen that using metal cluster modified nano zero-valent iron as a catalyst, under the same conditions, the polyethylene wax reforming rate can be increased by 200% within five hours compared with unmodified nano zero-valent iron, and the total content of light gasoline, kerosene and low-carbon paraffin oil in the reforming product is increased from 31% to 90%, indicating that metal cluster modification has greatly improved the performance of zero-valent iron photothermal reforming polyethylene wax. Figure 4 It can be seen that metal cluster modification enhances the photothermal effect of zero-valent iron.
[0081] Comparative Example 2
[0082] Photothermal reforming of waste polyethylene wax into liquid fuel and lubricating oil without catalyst:
[0083] Place 0.1g of waste polyethylene wax in a photothermal reactor and introduce argon gas. Take samples to detect the oxygen content in the gas in the reactor until the oxygen concentration is lower than the detection line. Turn on the simulated sunlight light source at a light intensity of 5W / cm 2 Photothermal reforming of waste polyethylene wax under the same conditions, testing the C5-C 12 Light gasoline, C 13 -C 18 Kerosene and C 18 -C 36 The content of low carbon paraffin oil. Figure 8 As shown in the figure, compared with the addition of zero-valent iron and metal clusters to modify nano-zero-valent iron, the waste polyethylene wax cannot be reformed by photothermal reaction to produce C5-C 12 Light gasoline, C 13 -C 18 Kerosene and C 18 -C 36 Low carbon paraffin oil.
[0084] Comparative Example 3
[0085] Thermal reforming of waste polyethylene wax into liquid fuel and lubricating oil:
[0086] 0.1g of waste polyethylene wax sample and 0.3g of metal cluster modified nano zero-valent iron were mixed evenly, argon was introduced into the photothermal reactor, and the oxygen content in the gas in the reactor was sampled and tested until the oxygen concentration was lower than the detection line. The heating source was turned on and the reforming rate of the waste polyethylene wax was tested after heating for 5 hours. The experimental results are as follows: Fig. 9 As shown: Compared with light conditions, metal cluster-modified nano zero-valent iron cannot thermally reform waste polyethylene wax.
[0087] Comparative Example 4
[0088] Metal cluster modified nano zero-valent iron and waste polyethylene wax are used for photothermal reforming of waste polyethylene wax into liquid fuel and lubricating oil under non-mixing conditions:
[0089] 0.1g of waste polyethylene wax sample and 0.3g of metal cluster-modified nano-zero-valent iron were placed in a photothermal reactor and argon was introduced. The oxygen content in the gas in the reactor was sampled and tested until the oxygen concentration was lower than the detection line. The simulated solar light source was turned on at a light intensity of 5W / cm 2 The waste polyethylene wax was reformed by photothermal reforming, and the liquid fuel and lubricating oil collected after 5 hours of photothermal reforming were tested. Fig.10 As shown: The relative yield of liquid fuel and lubricating oil produced by photothermal reforming of waste polyethylene wax with metal cluster-modified nano zero-valent iron under non-mixed conditions is significantly lower than that under mixed conditions.
[0090] Comparative Example 5
[0091] Metal single atom modified nano zero-valent iron photothermal reforming of waste polyethylene wax into liquid fuel and lubricant:
[0092] (Taking atomic ruthenium as an example) Preparation of single-atom ruthenium modified nano zero-valent iron: 50 mg of nano zero-valent iron material was immersed in 100 mL of 1 mg / L triruthenium dodecacarbonyl tetrahydrofuran solution for 3 h, and then the solvent was removed by reduced pressure distillation. The remaining solid was calcined in a tubular furnace in an argon atmosphere (the calcination temperature was set to 300°C and the calcination time was set to 4 h), and the single-atom ruthenium modified nano zero-valent iron material was collected.
[0093] Mix 0.1g of waste polyethylene wax sample and 0.3g of metal single atom modified nano zero-valent iron evenly, introduce argon into the photothermal reactor, and sample and detect the oxygen content in the gas in the reactor until the oxygen concentration is lower than the detection line. Turn on the simulated solar light source at a light intensity of 5W / cm 2 The waste polyethylene wax was reformed by photothermal reforming, and the liquid fuel and lubricating oil collected after 5 hours of photothermal reforming were tested. Fig.11 As shown: The relative yield of liquid fuel and lubricating oil produced by photothermal reforming of waste polyethylene wax by metal single atom modified nano zero-valent iron is significantly lower than that by metal cluster modified nano zero-valent iron.
[0094] Comparative Example 6
[0095] Photothermal reforming of waste polyethylene wax into liquid fuel and lubricant by composite modified nano zero-valent iron with multiple metal single atoms:
[0096] (Taking single-atom ruthenium, platinum and nickel as examples) Preparation of multiple metal single-atom composite modified nano zero-valent iron: 50 mg of nano zero-valent iron material was immersed in 100 mL of 1 mg / L tetrahydrofuran mixed solution of triruthenium dodecacarbonyl, chloroplatinic acid and nickel tetracarbonyl for 3 h, and then the solvent was removed by reduced pressure distillation. The remaining solid was calcined in a tubular furnace in an argon atmosphere (the calcination temperature was set to 300°C and the calcination time was set to 4 h), and the multiple metal single-atom composite modified nano zero-valent iron material was collected.
[0097] Mix 0.1g of waste polyethylene wax sample and 0.3g of multi-metal single-atom composite modified nano zero-valent iron evenly, introduce argon into the photothermal reactor, and sample and detect the oxygen content in the gas in the reactor until the oxygen concentration is lower than the detection line. Turn on the simulated solar light source at a light intensity of 5W / cm 2 The waste polyethylene wax was reformed by photothermal reforming, and the liquid fuel and lubricating oil collected after 5 hours of photothermal reforming were tested. Fig.12 As shown: The relative yield of liquid fuel and lubricating oil produced by photothermal reforming of waste polyethylene wax by nano zero-valent iron modified by multiple metal single atom composites is significantly lower than that by nano zero-valent iron modified by metal clusters.
[0098] Comparative Example 7
[0099] Photothermal reforming of waste polyethylene wax into liquid fuel and lubricating oil by oxygen-containing acid radical-modified zero-valent iron:
[0100] 0.1g of waste polyethylene wax sample and 0.3g of phosphate and borate co-modified zero-valent iron (surface phosphate content 3wt%, surface borate content 2.7wt%, particle size 0.5-10μm) were mixed evenly, argon was introduced into the photothermal reactor, and the oxygen content in the gas in the reactor was sampled and tested until the oxygen concentration was below the detection line. The simulated solar light source was turned on at a light intensity of 5W / cm 2 The waste polyethylene wax was reformed by photothermal reforming, and the liquid fuel and lubricating oil collected after 5 hours of photothermal reforming were tested. Fig.13 As shown: The content of liquid fuel and lubricating oil produced by the photothermal reforming of waste polyethylene wax by oxygen-containing acid group-modified zero-valent iron is significantly lower than that of metal cluster-modified nano zero-valent iron.
[0101] Comparative Example 8
[0102] Indium cluster modified nano zero-valent iron photothermal reforming of waste polyethylene wax into liquid fuel and lubricant:
[0103] Mix 0.1g of waste polyethylene wax sample and 0.3g of indium cluster-modified nano-zero-valent iron evenly, introduce argon into the photothermal reactor, and take samples to detect the oxygen content in the gas in the reactor until the oxygen concentration is lower than the detection line. Turn on the simulated solar light source at a light intensity of 5W / cm 2The waste polyethylene wax was reformed by photothermal reforming, and the liquid fuel and lubricating oil collected after 5 hours of photothermal reforming were tested. Fig.14 As shown: The content of liquid fuel and lubricating oil produced by the photothermal reforming of waste polyethylene wax by indium cluster-modified nano zero-valent iron is significantly lower than that of nano zero-valent iron modified by d-block metal clusters (taking ruthenium as an example).
[0104] Example 2
[0105] In this example, the ruthenium chloride precursor aqueous solution was replaced with a 1 g / L chloroplatinic acid aqueous solution, 180 mL of chloroplatinic acid aqueous solution was added at a drip rate of 8 mL / min, and the surface platinum content was 5.9 wt %. The rest was the same as in Example 1. The experimental results are shown in FIG. Fig.15 As shown in a: Platinum metal clusters modified nano zero-valent iron can reform waste polyethylene wax through photothermal reaction.
[0106] Example 3
[0107] In this embodiment, the ruthenium chloride precursor aqueous solution is replaced with a palladium chloride aqueous solution with a concentration of 0.6 g / L, 180 mL of palladium chloride aqueous solution is added, the dripping rate is 6 mL / min, the surface palladium content is 4.9 wt%, and the rest is the same as in Example 1. The experimental results are shown in Fig.15 As shown in b: Palladium metal clusters modified nano zero-valent iron can reform waste polyethylene wax through photothermal reaction.
[0108] Example 4
[0109] In this example, the ruthenium chloride precursor aqueous solution was replaced with a nickel chloride aqueous solution with a concentration of 0.4 g / L, 145 mL of nickel chloride aqueous solution was added, the dripping rate was 4 mL / min, and the surface nickel content was 6.1 wt %. The rest was the same as in Example 1. The experimental results are shown in Fig.15 As shown in c: Nickel metal clusters modified nano zero-valent iron can reform waste polyethylene wax through photothermal reaction.
[0110] Example 5
[0111] In this embodiment, the ruthenium chloride precursor aqueous solution is replaced with a 0.5 g / L copper chloride aqueous solution, 160 mL of the copper chloride aqueous solution is added at a drip rate of 5 mL / min, and the surface copper content is 6.3 wt %. The rest is the same as in Example 1. The experimental results are shown in FIG. Fig.15 As shown in d: Copper metal clusters modified nano zero-valent iron can reform waste polyethylene wax through photothermal reaction.
[0112] Example 6
[0113] In this example, 0.1 g of waste polyethylene wax was mixed with the reacted catalyst and the photothermal reforming was continued for 5 hours. The rest was the same as in Example 1. Fig.16As shown: Metal cluster modified nano zero-valent iron material has good recyclability in photothermal reforming of waste polyethylene wax.
[0114] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.
Claims
1. A photothermal catalyst, characterized in that: The photothermal catalyst is a metal cluster-modified nano zero-valent iron material with a nanometer scale. The loaded metal clusters include d-zone and ds-zone transition metals, and the diameter of the metal cluster particles is between 0.5 and 5 nm.
2. The photothermal catalyst according to claim 1, characterized in that: The d-block and ds-block transition metals include ruthenium, platinum, palladium, nickel, and copper.
3. The photothermal catalyst according to claim 2, characterized in that: The ruthenium content on the surface of the metal cluster modified nano zero-valent iron material is 0.8wt%-7.2wt%, the platinum content on the surface is 1.0wt%-6.0wt%, the palladium content on the surface is 0.1wt%-5.1wt%, the nickel content on the surface is 0.4wt%-7.7wt%, and the copper content on the surface is 0.5wt%-6.8wt%.
4. The photothermal catalyst according to claim 1, characterized in that: The metal cluster modified nano zero-valent iron material has an irregular nanowire structure of nanometer scale, and the particle diameter of the metal cluster modified nano zero-valent iron material is between 50 and 300 nm.
5. A method for preparing a photothermal catalyst according to any one of claims 1 to 4, characterized in that: The following steps are involved: 1) Using aqueous phase reduction technology, a sodium borohydride solution is dropped into a ferric chloride solution to obtain a nano zero-valent iron suspension; 2) Using the self-organization method induced by nano-zero-valent iron, the metal chloride precursor aqueous solution is dropped into the nano-zero-valent iron suspension for immersion reduction. After the reaction is completed, the suspension is filtered, the solid is washed and dried in an inert atmosphere, and the metal cluster-modified nano-zero-valent iron material is collected.
6. The method for preparing a photothermal catalyst according to claim 5, characterized in that: Step 1) The flow rate of the sodium borohydride solution dripping into the ferric chloride solution is 25-35 mL / min.
7. The method for preparing a photothermal catalyst according to claim 5, characterized in that: Step 2) The metal chloride precursor includes ruthenium chloride, chloroplatinic acid, palladium chloride, nickel chloride and cupric chloride.
8. The method for preparing a photothermal catalyst according to claim 5, characterized in that: Step 2) The immersion time is 4 hours and the drying time is 3 to 4 hours.
9. Use of the photothermal catalyst according to any one of claims 1 to 4, characterized in that: The photothermal catalyst is used for photothermal reforming of waste polyethylene wax into liquid fuel and lubricating oil.
10. The use of the photothermal catalyst according to claim 9, characterized in that: The specific method is: the photothermal catalyst is uniformly mixed with waste polyethylene wax, an inert gas is introduced into the photothermal reactor, a xenon lamp is used as a light source to simulate sunlight, and the obtained products are liquid fuel and lubricating oil; The mass ratio of the photothermal catalyst to the waste polyethylene wax to be treated is 1:10 to 20:1; The photothermal reaction time is 0.5 to 12 hours.