Titanium oxide coated titanium niobate negative electrode material as well as preparation method and application thereof
By preparing titanium suboxide-coated titanium niobate anode material, the problem of poor rate performance of titanium niobium oxide was solved, and the conductivity and rate performance of the material were improved, making it suitable for lithium-ion batteries.
Patent Information
- Application Number
- CN202411088778.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-22
AI Technical Summary
Existing titanium niobium oxide anode materials have poor rate performance, low electronic and ionic conductivity, and high synthesis costs, making them difficult to meet the needs of industrial production.
The preparation method of titanium suboxide-coated titanium niobate anode material involves calcining a titanium source and a niobium source to form a titanium niobate precursor, which is then sintered with a carbon source in a protective atmosphere to form titanium suboxide. Subsequently, it is mixed with a dispersant and water for nano-sizing, drying, and solid-phase sintering to form titanium suboxide-coated titanium niobate anode material.
This method improves the electrical conductivity and rate performance of titanium niobate, provides an electron conduction channel, shortens the diffusion paths of lithium ions and electrons, enhances the active sites for electrochemical reactions, and solves the problems of electrical conductivity and rate performance of titanium niobate oxide materials.
Smart Images

Figure CN118993146A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion battery materials, and in particular to a titanium suboxide-coated titanium niobate negative electrode material and a preparation method and application thereof. Background Art
[0002] In the past decade, lithium-ion batteries (LIBs) have been widely used in energy storage, portable electronics, and are expected to play an important role in electric vehicles. 12 It is considered to be a very promising anode, but there are still some problems to be solved. In commercial lithium-ion batteries, graphite has been used as an anode, but the potential of lithium ion embedding in graphite is close to 0V, which easily forms lithium dendrites and causes battery short circuit. In addition, the electrochemical performance of graphite at high current density is not ideal. For Li4Ti5O 12 , Li + The insertion potential rises to 1.5V, and the theoretical specific capacity is only 175mAh g / 1. All of the above problems will limit its application in the future. Therefore, it is necessary to find another material that is safer and has better performance.
[0003] Advantages of titanium niobium oxides such as Nb 4+ / Nb 3+ , Nb 5+ / Nb 4+ and Ti 4+ / Ti 3+ Two electrons undergo redox reactions, and titanium niobium oxide has a capacity of about 390 mAh / g (which is about the same as commercial lithium titanate Li4Ti5O 12 Titanium niobium oxide has a high theoretical specific capacity of about twice that of lithium ions. Titanium niobium oxide has a high operating voltage platform, which can effectively inhibit the formation of lithium dendrites and SEI films, and therefore has good safety performance. It also has a channel for rapid lithium ion extraction and a stable lithium intercalation structure, which improves the service life of the battery. High energy density titanium niobium oxide negative electrode materials also have great advantages in fast charging. Titanium niobium oxide materials replace Li4Ti5O 12 The material has attracted widespread attention. Low electronic and ionic conductivity severely limits the Coulombic efficiency and rate performance of titanium niobium oxide materials. At the same time, the high phase formation temperature of titanium niobium oxide materials (generally 700-1100°C) leads to a large crystal size, which further affects the improvement of rate performance. In recent years, there have been many reports on the improvement of the performance of titanium niobium oxide negative electrode materials.
[0004] At present, the synthesis methods of titanium niobium oxide in the market are mostly sol-gel method and hydrothermal method, but their production cost is high and not suitable for industrial production. Although the solid phase method can reduce the production cost to a large extent, the intrinsic electronic conductivity and ionic conductivity of titanium niobium oxide are low, and the rate performance is poor. Summary of the invention
[0005] The object of the present invention is to provide a titanium suboxide-coated titanium niobate negative electrode material and a preparation method and application thereof, so as to solve the problem of poor rate performance of existing titanium niobium oxide.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] The present invention provides a method for preparing a titanium niobate negative electrode material coated with titanium suboxide, comprising the following steps:
[0008] Mixing the first titanium source and the niobium source, and calcining them to obtain a titanium niobate precursor;
[0009] The second titanium source is mixed with the carbon source, and sintered in a protective atmosphere to obtain titanium oxide;
[0010] The titanium suboxide, titanium niobate precursor, dispersant and water are mixed, the obtained mixed slurry is nano-sized, and then dried and solid-phase fired in sequence to obtain a titanium suboxide-coated titanium niobate negative electrode material.
[0011] Preferably, the first titanium source and the second titanium source independently include one or more of titanium dioxide, tetrabutyl titanate, titanium tetrachloride and titanium isopropoxide; the niobium source includes one or more of niobium pentoxide, niobium pentachloride and niobium oxalate; and the molar ratio of the titanium element in the first titanium source to the niobium element in the niobium source is 1:1.8-6.
[0012] Preferably, the carbon source includes one or more of graphite, glucose, asphalt, carbon nanotubes and graphene; the mass ratio of the second titanium source to the carbon source is 3 to 5:1; and the protective atmosphere includes nitrogen or argon.
[0013] Preferably, the first titanium source and the niobium source are mixed by dry grinding, and the conditions of the dry grinding include: the equipment is a planetary ball mill, the grinding medium is one or more of stainless steel balls, agate beads and zirconium oxide beads, the grinding speed is 200-500rpm, the grinding time is 1-2h, and the grinding particle size D 50 =0.4~0.6μm;
[0014] The calcination temperature is 700-1200° C. and the calcination time is 8-16 hours.
[0015] Preferably, the second titanium source and the carbon source are mixed by dry grinding, and the conditions of the dry grinding include: the equipment is a planetary ball mill, the grinding medium is stainless steel balls, the grinding speed is 200-500 rpm, and the grinding time is 1-2 hours;
[0016] The sintering temperature is 800-1200° C. and the sintering time is 4-14 hours.
[0017] Preferably, the equipment used for the nano-processing is one or both of a ball mill and a sand mill, the grinding line speed is ≥16 m / s, the grinding time is 4 to 8 h, and the grinding particle size is 0.3 to 1 μm; the solid content of the mixed slurry is 35 to 45 wt%;
[0018] The dispersant includes one or more of polyethylene glycol, polyacrylamide and carboxymethyl cellulose; the mass of the dispersant is 0.5-3% of the total mass of the first titanium source and the niobium source;
[0019] The drying method is one or more of two-fluid spray drying, centrifugal spray drying and freeze drying.
[0020] Preferably, the mass of the titanium suboxide is 1-3% of the mass of the titanium niobate precursor; the temperature of the solid phase sintering is 700-850° C., the time is 6-16 hours, and the atmosphere is nitrogen or argon.
[0021] Preferably, the titanium niobate in the titanium oxide-coated titanium niobate negative electrode material includes Ti2Nb2O9, TiNb2O7, TiNb6O 17 、Ti2Nb 10 O 29 and TiNb 24 O 64 One or more of the .
[0022] The present invention provides a titanium suboxide-coated titanium niobate negative electrode material prepared by the preparation method described in the above technical solution.
[0023] The present invention provides the use of the titanium niobate negative electrode material coated with titanium suboxide described in the above technical solution in a lithium ion battery.
[0024] The present invention provides a method for preparing a titanium suboxide-coated titanium niobate negative electrode material, comprising calcining a titanium source and a niobium source to obtain a titanium niobate precursor, mixing a carbon source with a titanium source, reducing and sintering in a protective atmosphere to obtain titanium suboxide, and then nano-sizing and spray-drying the dispersant, the titanium niobate precursor and the titanium suboxide, and sintering again to obtain a high-rate and long-cycle titanium suboxide-coated titanium niobate negative electrode material. The present invention improves the conductivity of titanium niobate and the rate performance by using titanium suboxide for surface coating and material nano-sizing. Specifically, by surface coating the conductive layer, the coating layer provides an electron conduction channel, facilitates the lithium ion transmission between active phases, and can effectively buffer volume expansion and maintain structural integrity. By nano-sizing the material, the diffusion path of lithium ions and electrons is shortened, and at the same time, the active sites of the electrochemical reaction are increased, thereby increasing the Li + The kinetic properties of embedding and extraction. Therefore, the present invention can solve the problem of low intrinsic electronic conductivity and ionic conductivity of titanium niobate, and obtain a titanium niobate negative electrode material with high initial efficiency and good rate performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a SEM image (500 times) of the titanium niobate precursor prepared in Example 1;
[0026] Figure 2 XRD pattern of titanium oxide prepared in Example 1;
[0027] Figure 3 This is the XRD pattern of titanium niobate coated with titanium oxide prepared in Example 1;
[0028] Figure 4 This is a charge and discharge curve diagram of the titanium niobate negative electrode material coated with titanium oxide prepared in Example 1. DETAILED DESCRIPTION
[0029] The present invention provides a method for preparing a titanium niobate negative electrode material coated with titanium suboxide, comprising the following steps:
[0030] Mixing the first titanium source and the niobium source, and calcining them to obtain a titanium niobate precursor;
[0031] The second titanium source is mixed with the carbon source, and sintered in a protective atmosphere to obtain titanium oxide;
[0032] The titanium suboxide, titanium niobate precursor, dispersant and water are mixed, the obtained mixed slurry is nano-sized, and then dried and solid-phase fired in sequence to obtain a titanium suboxide-coated titanium niobate negative electrode material.
[0033] In the present invention, unless otherwise specified, the required raw materials for preparation are all commercially available products well known to those skilled in the art.
[0034] The present invention mixes a first titanium source with a niobium source and calcines the mixture to obtain a titanium niobate precursor.
[0035] In the present invention, the first titanium source preferably includes one or more of titanium dioxide, tetrabutyl titanate, titanium tetrachloride and titanium isopropoxide; when the first titanium source is two or more of the above, the present invention has no special limitation on the ratio of different types of titanium sources, which can be adjusted according to actual needs.
[0036] In the present invention, the niobium source preferably includes one or more of niobium pentoxide, niobium pentachloride and niobium oxalate; when the niobium source is two or more of the above, the present invention has no special limitation on the ratio of different types of niobium sources, which can be adjusted according to actual needs.
[0037] In the present invention, the molar ratio of the titanium element in the first titanium source to the niobium element in the niobium source is preferably 1:1.8-6, more preferably 1:2, 2:5 or 1:6.
[0038] In the present invention, the first titanium source and the niobium source are preferably mixed by dry grinding; the conditions for the dry grinding preferably include: the equipment is a planetary ball mill, the grinding medium is one or more of stainless steel balls, agate beads and zirconium oxide beads, the grinding speed is 200-500rpm, more preferably 300rpm, the grinding time is 1-4h, more preferably 2-3h, and the grinding particle size D 50 =0.4~0.6μm; the ball-to-material ratio is preferably 2~6:1, more preferably 3:1.
[0039] In the present invention, the calcination temperature is preferably 700-1200°C, more preferably 800-1100°C, further preferably 900-1000°C, the time is preferably 8-16h, more preferably 10-12h, further preferably 10h; the heating rate to the calcination temperature is preferably 5°C / min; the calcination is preferably carried out in an air atmosphere; the equipment used for the calcination is preferably one or more of a muffle furnace, a tubular furnace, a high-temperature resistance furnace, a high-temperature vertical furnace, an atmosphere box-type resistance furnace, and a kiln.
[0040] The titanium niobate precursor prepared by the present invention is titanium niobate not coated with titanium suboxide, and titanium suboxide-coated titanium niobate is obtained after being coated with titanium suboxide.
[0041] The invention mixes the second titanium source with the carbon source and sinters them in a protective atmosphere to obtain titanium suboxide.
[0042] In the present invention, the second titanium source preferably includes one or more of titanium dioxide, tetrabutyl titanate, titanium tetrachloride and titanium isopropoxide; when the second titanium source is two or more of the above, the present invention has no special limitation on the ratio of different types of titanium sources, which can be adjusted according to actual needs.
[0043] In the present invention, the carbon source preferably includes one or more of graphite, glucose, asphalt, carbon nanotubes and graphene, more preferably glucose or graphite, and further preferably graphite; the mass ratio of the second titanium source to the carbon source is preferably 3 to 5:1, more preferably 3:1; the present invention utilizes the carbon source to exert a reducing effect to form titanium dioxide.
[0044] In the present invention, the method of mixing the second titanium source and the carbon source is preferably dry grinding, and the conditions of the dry grinding preferably include: the equipment is a planetary ball mill, the grinding medium is stainless steel balls, the grinding speed is 200-500rpm, more preferably 300rpm, the grinding time is 1-2h, and the ball-to-material ratio is 2:1; the protective atmosphere preferably includes nitrogen or argon; when nitrogen and argon are used, there is no special limitation on the volume ratio of different types of gases, and any ratio is acceptable.
[0045] In the present invention, the sintering temperature is preferably 800-1200°C, more preferably 900-1100°C, and further preferably 1000°C. The time is preferably 4-14h, more preferably 6-12h, and further preferably 10h. The heating rate to the sintering temperature is preferably 5°C / min.
[0046] After obtaining titanium suboxide and titanium niobate precursor, the present invention mixes the titanium suboxide, titanium niobate precursor, dispersant and water, nanosizes the obtained mixed slurry, and then sequentially dries and solid-phase sinters to obtain a titanium suboxide-coated titanium niobate negative electrode material.
[0047] In the present invention, the mass of the titanium suboxide is preferably 1-3% of the mass of the titanium niobate precursor, and more preferably 1.5-2%, that is, the coating amount of the titanium suboxide on the titanium niobate.
[0048] In the present invention, the dispersant preferably includes one or more of polyethylene glycol, polyacrylamide and carboxymethyl cellulose, and more preferably polyethylene glycol-6000; when the dispersant is more than two of the above two, the present invention has no special limitation on the ratio of different types of dispersants, which can be determined according to actual needs; the mass of the dispersant is 0.5-3% of the total mass of the first titanium source and the niobium source, and more preferably 0.77-2.0%.
[0049] In the present invention, the solid content of the mixed slurry is preferably 35-45wt%, more preferably 38-43wt%.
[0050] In the present invention, the nano-forming method is preferably wet grinding; the equipment used for the nano-forming is preferably one or both of a ball mill and a sand mill, the grinding medium is preferably a zirconia ball, the diameter of the zirconia ball is preferably 0.1 to 6 mm, the grinding linear speed is preferably ≥16 m / s, more preferably 20 m / s, the grinding time is preferably 4 to 8 h, more preferably 6 h, and the grinding particle size D is preferably 0.1 to 6 mm. 50 =0.3-1 μm, more preferably 0.6-0.8 μm. In the present invention, the dispersant is preferably mixed with water for wet grinding, and then the titanium niobate precursor and titanium suboxide are added, and the obtained mixed slurry is further wet ground for nano-sizing. When the equipment used for the nano-sizing is a ball mill and a sand mill, it is preferred to first use a ball mill for coarse grinding and then use a sand mill for fine grinding.
[0051] In the present invention, the drying method is preferably one or more of two-fluid spray drying, centrifugal spray drying and freeze drying. When the drying method is two or more of the above, the present invention has no special limitation on the combination of different types of drying methods, which can be adjusted according to actual needs; the conditions of the two-fluid spray drying preferably include: an inlet temperature of 180 to 240°C, preferably 210 to 220°C; an outlet temperature of 90 to 120°C, preferably 100 to 110°C, and a spray material D 50 The particle size is 4 to 8 μm. Single particle coating of titanium oxide is achieved during the spray drying process.
[0052] In the present invention, the temperature of the solid phase sintering is preferably 700-850°C, preferably 750-800°C, and more preferably 780°C; the time is preferably 6-16h, preferably 8-14h, and more preferably 12h; the heating rate is preferably 5°C / min; and the atmosphere is preferably nitrogen and / or argon.
[0053] The present invention coats titanium suboxide on a titanium niobate precursor through solid phase sintering to form titanium suboxide-coated titanium niobate.
[0054] After the solid phase sintering is completed, the present invention preferably cools the obtained product to room temperature, takes it out, grinds it through a 200-mesh screen, and obtains a titanium suboxide-coated titanium niobate negative electrode material.
[0055] In the present invention, the titanium niobate in the titanium oxide-coated titanium niobate negative electrode material preferably includes Ti2Nb2O9, TiNb2O7, TiNb6O 17 、Ti2Nb 10 O 29 、TiNb 24 O 64 One or more of the above, more preferably TiNb2O7.
[0056] The present invention provides a titanium suboxide-coated titanium niobate negative electrode material prepared by the preparation method described in the above technical solution.
[0057] The present invention provides the use of the titanium niobate negative electrode material coated with titanium suboxide described in the above technical solution in a lithium ion battery.
[0058] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0059] Example 1
[0060] 1) Add 300g titanium dioxide and 984g niobium pentoxide to a ball mill, and perform dry ball milling. Set the ball-to-material ratio to 3:1, adjust the speed to 300rpm, use zirconium oxide balls as the ball milling medium, set the ball milling time to 2h, and grind the particle size D50 =0.4~0.6μm, placing the mixed powder in a muffle furnace, calcining in an air atmosphere, heating to 1000℃ at a heating rate of 5℃ / min, keeping the temperature for 10h, cooling to room temperature and taking out to obtain titanium niobate precursor powder (TiNb2O7);
[0061] 2) Add 50.0g titanium dioxide and 10g graphite into a ball mill with a ball-to-material ratio of 2:1, adjust the rotation speed to 300rpm, perform dry grinding for 1h, calcine under nitrogen atmosphere, increase the temperature at a rate of 5°C / min to 1000°C, keep the temperature for 10h, cool to room temperature and take out to obtain titanium dioxide powder;
[0062] 3) Add 10.0 g of PEG-6000 powder to 1200 mL of ultrapure water, and wet-mill for 2 min using a ball mill. The grinding medium is zirconia balls with a diameter of 0.1 to 6 mm. Then, add 500.0 g of the titanium niobate precursor and 5 g of titanium suboxide obtained in step 1) and step 2). Continue to ball mill the resulting mixed slurry (solid content of 43 wt%) (titanium suboxide coating amount of 1 wt%), the grinding line speed is 20 m / s, the grinding time is 6 h, the grinding particle size is 0.3 to 0.6 μm, the rotation speed is adjusted to 30 Hz, the slurry is transferred to a 1 L sand mill for fine grinding, and then two-fluid spray drying is performed, the inlet temperature is controlled at 220° C., the outlet temperature is 110° C., and the spray particle size D is controlled. 50 =6±2μm, the obtained mixed powder is placed in an atmosphere furnace, solid-phase sintered in a nitrogen atmosphere, the heating rate is 5℃ / min to 750℃, kept warm for 6h, cooled to room temperature, taken out, ground and sieved with 200 mesh, to obtain titanium suboxide-coated titanium niobate negative electrode material.
[0063] Example 2
[0064] Same as Example 1, except that in step 1), the calcination condition is 900° C. / 10 h.
[0065] Example 3
[0066] Same as Example 1, except that in step 1), the ball milling time is 1 h.
[0067] Example 4
[0068] Same as Example 1, except that in step 3), the grinding particle size D 50 =0.6~0.8μm.
[0069] Example 5
[0070] The same as Example 1, except that in step 3), 500.0 g of titanium niobate precursor and 15 g of titanium oxide are used, that is, the titanium oxide coating amount is 3 wt %.
[0071] Example 6
[0072] Same as Example 1, except that in step 3), the solid phase sintering condition is 700°C / 6h.
[0073] Comparative Example 1
[0074] Same as Example 1, except that in step 1), the ball milling time is 4 h.
[0075] Comparative Example 2
[0076] Same as Example 1, except that in step 2), the carbon source is replaced with PVA.
[0077] Comparative Example 3
[0078] Same as Example 1, except that in step 3), the temperature is raised to 900° C. and kept at this temperature for 3 h.
[0079] Characterization and performance testing
[0080] 1) Figure 1 The SEM image (500 times) of the titanium niobate precursor prepared in Example 1; Figure 1 It can be seen that the particles of this sample are complete and have a high degree of sphericity, making it easier for titanium oxide to coat the surface of titanium niobate.
[0081] Figure 2 is the XRD pattern of the titanium oxide prepared in Example 1; Figure 2 It can be seen that this method can form pure phase titanium oxide.
[0082] Figure 3 The XRD pattern of titanium niobate coated with titanium oxide prepared in Example 1 is shown in FIG. Figure 3 It can be seen that this method can form pure phase titanium niobate.
[0083] 2) Titanium suboxide-coated titanium niobate negative electrode materials prepared in different cases: PVDF:SuperP were mixed in a mass ratio of 80:10:10, and then dissolved and dispersed evenly with N-methylpyrrolidone, coated on aluminum foil, dried and rolled into pole pieces. The negative electrode material pole piece was used as the working electrode, the metal lithium sheet was used as the counter electrode and reference electrode, 1 mol LiPF6 (EC:DMC:EMC=1:1:1, v / v) was used as the electrolyte, and the PP / PE composite film was used as the diaphragm to assemble the battery in a glove box. The assembled battery was activated by cycling 3 times at a current of 0.2C, and the charge and discharge range was set to 1.0~2.5V. The rate performance test of the material was performed by cycling 3 times at 1C, then 3 times at 3C, 3 times at 5C, and then 3C continued to cycle. The results are shown in Table 1; Figure 4 This is a charge and discharge curve diagram of the titanium niobate negative electrode material coated with titanium oxide prepared in Example 1.
[0084] Table 1 Rate performance of negative electrode materials in Examples 1 to 6 and Comparative Examples 1 to 3
[0085]
[0086]
[0087] according to Figure 4 Compared with Table 1, by comparing Examples 1 to 2, it can be seen that lowering the primary sintering temperature will lead to poor particle forming and affect the subsequent titania coating. By comparing Examples 1 to 3 and Comparative Example 1, the grinding time affects the size of the primary particles. The longer the grinding time, the more fine powder in the primary particles. The shorter the time, the larger the primary particles. This proves that the primary particles have a greater impact on the subsequent secondary wet grinding and titania coating. By comparing Examples 1 and 4, it can be seen that the secondary grinding particle size has a greater impact on the spheroidization of the secondary particles. The secondary grinding cannot destroy the integrity of the primary particles. The more complete the spherical shape of the secondary particles, the better the rate performance. By comparing Examples 1 and 5, it can be seen that too high a titania coating amount leads to poor rate performance. By comparing Example 1 and Comparative Example 2, it can be seen that PVP will lead to lower purity of titania and too many by-products, which will affect the buckling performance. By comparing Example 1 and Comparative Example 3, it can be seen that too high a secondary solid phase sintering temperature will lead to low rate performance.
[0088] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a titanium niobate negative electrode material coated with titanium suboxide, characterized in that: The following steps are involved: Mixing the first titanium source and the niobium source, and calcining them to obtain a titanium niobate precursor; The second titanium source is mixed with the carbon source, and sintered in a protective atmosphere to obtain titanium oxide; The titanium suboxide, titanium niobate precursor, dispersant and water are mixed, the obtained mixed slurry is nano-sized, and then dried and solid-phase fired in sequence to obtain a titanium suboxide-coated titanium niobate negative electrode material.
2. The preparation method according to claim 1, characterized in that: The first titanium source and the second titanium source independently include one or more of titanium dioxide, tetrabutyl titanate, titanium tetrachloride and titanium isopropoxide; the niobium source includes one or more of niobium pentoxide, niobium pentachloride and niobium oxalate; the molar ratio of the titanium element in the first titanium source to the niobium element in the niobium source is 1:1.8-6.
3. The preparation method according to claim 1, characterized in that: The carbon source includes one or more of graphite, glucose, asphalt, carbon nanotubes and graphene; the mass ratio of the second titanium source to the carbon source is 3 to 5:1; and the protective atmosphere includes nitrogen or argon.
4. The preparation method according to claim 1, characterized in that: The first titanium source and the niobium source are mixed by dry grinding, and the conditions of the dry grinding include: the equipment is a planetary ball mill, the grinding medium is one or more of stainless steel balls, agate beads and zirconium oxide beads, the grinding speed is 200-500rpm, the grinding time is 1-2h, and the grinding particle size D 50 =0.4~0.6μm; The calcination temperature is 700-1200° C. and the calcination time is 8-16 hours.
5. The preparation method according to claim 1 or 3, characterized in that: The second titanium source and the carbon source are mixed by dry grinding, and the conditions of the dry grinding include: the equipment is a planetary ball mill, the grinding medium is stainless steel balls, the grinding speed is 200-500 rpm, and the grinding time is 1-2 hours; The sintering temperature is 800-1200° C. and the sintering time is 4-14 hours.
6. The preparation method according to claim 1, characterized in that: The equipment used for nano-processing is one or both of a ball mill and a sand mill, the grinding line speed is ≥16m / s, the grinding time is 4-8h, and the grinding particle size is 0.3-1μm; the solid content of the mixed slurry is 35-45wt%; The dispersant includes one or more of polyethylene glycol, polyacrylamide and carboxymethyl cellulose; the mass of the dispersant is 0.5-3% of the total mass of the first titanium source and the niobium source; The drying method is one or more of two-fluid spray drying, centrifugal spray drying and freeze drying.
7. The preparation method according to claim 6, characterized in that: The mass of the titanium suboxide is 1-3% of the mass of the titanium niobate precursor; the temperature of the solid phase sintering is 700-850°C, the time is 6-16 hours, and the atmosphere is nitrogen or argon.
8. The preparation method according to claim 7, characterized in that: The titanium niobate in the titanium oxide-coated titanium niobate negative electrode material includes Ti2Nb2O9, TiNb2O7, TiNb6O 17 、Ti2Nb 10 O 29 and TiNb 24 O 64 One or more of the .
9. Titanium suboxide-coated titanium niobate negative electrode material prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the titanium niobate negative electrode material coated with titanium suboxide according to claim 9 in lithium ion batteries.
Citation Information
Cited By
Preparation method and application of sodium ion battery negative electrode material
CN119841350A