Growth method and application of yttrium fluoride deep ultraviolet birefringent crystal
By growing YF3 powder under vacuum, the obtained yttrium fluoride deep ultraviolet birefringent crystals solve the problem of insufficient performance of existing materials, achieving high birefringence and performance improvement in important application fields.
Patent Information
- Application Number
- CN202411226897.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-22
AI Technical Summary
The existing deep ultraviolet birefringent crystal materials are insufficient in performance, especially in terms of birefringence and ultraviolet cut-off edges, which are difficult to meet the needs of high-tech fields.
YF3 powder was used to grow yttrium fluoride deep ultraviolet birefringent crystals under vacuum conditions, and by controlling the temperature and cooling rate in a high temperature furnace, yttrium fluoride deep ultraviolet birefringent crystals with high birefringent index were obtained.
The obtained yttrium fluoride deep ultraviolet birefringent crystal has a birefringent index of four times that of commercial material MgF2 at 1064 nm. It is suitable for the preparation of a variety of optical components and significantly improves performance.
Smart Images

Figure CN118996600A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a growth method and application of yttrium fluoride deep ultraviolet birefringent crystal, belonging to the field of deep ultraviolet birefringent crystal materials. Background Art
[0002] Birefringent crystals play an indispensable role in many fields and high-precision scientific research instruments such as optical isolators, Glan prisms, polarization optical devices, circulators, photoelectric modulators, and laser polarization technology. Commonly used commercial birefringent crystals include MgF2, α -BaB2O4, CaCO3, YVO4, TiO2 and LiNbO3, among which only MgF2 and α -BaB2O4 is used as a deep ultraviolet birefringent material. MgF2 has a short ultraviolet cutoff edge (110 nm) and a small birefringence index (0.014 @193 nm); α -BaB2O4 has a large birefringence (0.122 @532 nm) and a UV cutoff edge close to 200 nm (189 nm). With the development of technology and the improvement of requirements, the demand for deep ultraviolet birefringent crystals with better performance is more urgent. Therefore, the exploration of new deep ultraviolet birefringent crystals and the growth of birefringent materials are huge challenges in this direction. Summary of the invention
[0003] The object of the present invention is to provide a growth method and application of yttrium fluoride deep ultraviolet birefringent crystal. The chemical formula of the crystal is YF3, the molecular weight is 145.90, the crystal system is orthorhombic, and the space group is Pnma , unit cell parameters a = 6.3537(7)Å, b = 6.8545(7)Å, c = 4.3953(4)Å, β = 90, Z = 4, unit cell volume V = 191.42 Å 3 The YF3 powder is grown into a crystal under vacuum conditions. The deep purple birefringent yttrium fluoride crystal obtained by the method of the present invention has a birefringence of 0.051 at 1064nm, which is four times that of the commercial material MgF2. It can be used to make polarization beam splitting prisms such as Glan prisms, light separation polarizers, and optical components such as optical isolators, circulators, and beam shifters, and has important applications in the fields of optics and communications.
[0004] The method for growing the yttrium fluoride deep ultraviolet birefringent crystal of the present invention is carried out according to the following steps: a. In a sealed container of a glove box filled with nitrogen inert gas and containing 0.05 ppm of water and oxygen, 5 g of YF3 powder with a purity of 99.99% was placed in a quartz glass tube and the quartz tube was placed in a vacuum of 10 -5 -10 -3Pa is sealed after vacuuming; b. Place the sealed quartz tube in step a into a high temperature furnace, heat the temperature to 1350-1450°C at a heating rate of 35-40°C / h for 20-40h, keep warm for 80-100h, and cool at a rate of 4°C / h to obtain a deep ultraviolet birefringent yttrium fluoride YF3 crystal.
[0005] The yttrium fluoride deep ultraviolet birefringent crystal is used in preparing Glan-type prisms, light separation polarizers, polarization beam splitting prisms and optical isolators, circulators, and beam shifter optical elements.
[0006] The yttrium fluoride deep ultraviolet birefringent crystal obtained by the method of the present invention has important applications in many fields such as the preparation of optical isolators, Glan prisms, polarization optical devices, circulators, photoelectric modulators and laser polarization technology. BRIEF DESCRIPTION OF THE DRAWINGS
[0007] Figure 1 A comparison of the X-ray powder diffraction pattern of the polycrystalline powder of the present invention and the theoretical value, wherein A is the experimental value and B is the theoretical value; Figure 2 It is a schematic diagram of the wedge-shaped birefringent crystal polarization beam splitter of the present invention; Figure 3 Schematic diagram of the optical isolator of the present invention; Figure 4 Schematic diagram of the beam displacer of the present invention, wherein 1 is incident light, 2 is o light, 3 is e light, 4 is the optical axis, 5 is yttrium fluoride crystal, 6 is the light transmission direction, and 7 is the optical axis plane. DETAILED DESCRIPTION
[0008] The present invention is illustrated in detail by the following examples, but is not limited to the examples given. Example 1
[0009] The method for growing the yttrium fluoride deep ultraviolet birefringent crystal is carried out according to the following steps: a. In a sealed container of a glove box filled with nitrogen inert gas and containing 0.05 ppm of water and oxygen, 5 g of yttrium fluoride powder with a purity of 99.99% was placed in a quartz glass tube and the quartz tube was placed in a vacuum of 10 -53 Pa is sealed after vacuuming; b. Place the sealed quartz tube in step a into a high temperature furnace, heat it to 1450°C at a rate of 35°C / h for 20 hours, keep it warm for 80 hours, and cool it down at a rate of 4°C / h to obtain a quartz tube with a size of 0.7×0.5×0.8 mm. 3 Yttrium fluoride deep ultraviolet birefringent crystal. Example 2
[0010] The method for growing the Yttrium fluoride deep ultraviolet birefringent crystal is carried out according to the following steps: a. In a sealed container of a glove box filled with nitrogen inert gas and containing 0.05 ppm of water and oxygen, 5 g of yttrium fluoride powder with a purity of 99.99% was placed in a quartz glass tube and the quartz tube was placed in a vacuum of 10 -3 Pa is sealed after vacuuming; b. Place the sealed quartz tube in step a into a high temperature furnace, heat the temperature to 1350°C at a rate of 40°C / h for 30 hours, keep the temperature for 90 hours, and cool at a rate of 4°C / h to obtain a quartz tube with a size of 0.75×0.7×0.8 mm. 3 Yttrium fluoride deep ultraviolet birefringent crystal. Example 3
[0011] The method for growing the yttrium fluoride deep ultraviolet birefringent crystal is carried out according to the following steps: a. In a sealed container of a glove box filled with nitrogen inert gas and containing 0.05 ppm of water and oxygen, 5 g of yttrium fluoride powder with a purity of 99.99% was placed in a quartz glass tube and the quartz tube was placed in a vacuum of 10 -5 Pa is sealed after vacuuming; b. Place the sealed quartz tube in step a into a high temperature furnace, heat it to 1400°C at a rate of 38°C / h for 40h, keep it warm for 100h, and cool it down at a rate of 4°C / h to obtain a quartz tube with a size of 0.7×0.8×0.8 mm. 3 Yttrium fluoride deep ultraviolet birefringent crystal. Example 4
[0012] The method for growing the Yttrium fluoride deep ultraviolet birefringent crystal is carried out according to the following steps: a. In a sealed container of a glove box filled with nitrogen inert gas and containing 0.05 ppm of water and oxygen, 5 g of yttrium fluoride powder with a purity of 99.99% was placed in a quartz glass tube and the quartz tube was placed in a vacuum of 10 -3 Pa is sealed after vacuuming; b. Place the sealed quartz tube in step a into a high temperature furnace, heat the temperature to 1380°C at a rate of 36°C / h for 35h, keep warm for 95h, and cool at a rate of 4°C / h to obtain a quartz tube with a size of 0.8×1×0.9 mm. 3 Yttrium fluoride deep ultraviolet birefringent crystal. Example 5
[0013] Any of the yttrium fluoride birefringent crystals obtained in Examples 1-4 is used to prepare a birefringent crystal polarization beam splitter such as Figure 2As shown, a wedge-shaped birefringent crystal has the orientation of the optical axis. After a beam of natural light is incident on the crystal, it can be separated into two beams of linearly polarized light. The greater the birefringence, the farther the two beams of light can be separated, which facilitates the separation of the light beams. Example 6
[0014] Any of the yttrium fluoride birefringent crystals obtained in Examples 1-4 is used to prepare an optical isolator. A Faraday light rotator that rotates the polarization plane of an incident light beam by 45° is placed between a pair of birefringent crystal deflectors that are placed 45° across from each other. This can form an optical isolator that only allows a forward propagating light beam to pass through the system, while blocking a reverse propagating light beam. Figure 3 a means that the incident light beam can pass through, Figure 3 b indicates that the reflected light is blocked. Example 7
[0015] Any of the yttrium fluoride birefringent crystals obtained in Examples 1-4 is used to prepare a beam displacer, and a birefringent crystal is processed so that its optical axis plane forms an angle with the edge. θ like Figure 4 As shown in a, when natural light is incident vertically, it can be divided into two linearly polarized lights with vibration directions perpendicular to each other. Figure 4 As shown in b, they are o light and e light respectively. The greater the birefringence, the farther the two light beams can be separated, which facilitates the separation of the light beams.
Claims
1. A method for growing yttrium fluoride deep ultraviolet birefringent crystals, characterized in that Follow these steps: a. In a sealed container of a glove box filled with nitrogen inert gas and containing 0.05 ppm of water and oxygen, 5 g of YF3 powder with a purity of 99.99% was placed in a quartz glass tube and the quartz tube was placed in a vacuum of 10 -5 -10 -3 Pa is sealed after vacuuming; b. Place the sealed quartz tube in step a into a high temperature furnace, heat the temperature to 1350-1450°C at a heating rate of 35-40°C / h for 20-40h, keep the temperature for 80-100h, and cool at a rate of 4°C / h to obtain a deep ultraviolet birefringent yttrium fluoride YF3 crystal.
2. Use of the yttrium fluoride deep ultraviolet birefringent crystal obtained by the method as claimed in claim 1 in the preparation of Glan-type prisms, light separation polarizers, polarization beam splitter prisms and optical isolators, circulators, and beam shifter optical elements.
Citation Information
Patent Citations
Praseodymium-doped yttrium lithium fluoride crystal growth method
CN102925973A
Neodymium-doped yttrium fluoride gadolinium lithium crystal and growing method of same
CN103103610A
696nm red light total-solid laser of Blu-ray pump praseodymium-doped yttrium lithium fluoride
CN103117509A
All-solid-state short wave ultraviolet laser source
CN103199429A
Yttrium lithium fluoride composite crystal and preparation method thereof
CN104099665A