Large-temperature-difference well cementation cement paste as well as preparation method and application thereof

By introducing gypsum, red mud and sulfoaluminate cement into the cement slurry, the problem of setting time in the cement slurry in a large temperature difference environment is solved, the construction safety and progress are improved, and the construction safety and progress are achieved. Good compressive strength and adaptability.

CN119019145AActive Publication Date: 2024-11-26CHINA PETROLEUM & CHEMICAL CORP +1

Patent Information

Application Number
CN202310592960.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-24
Publication Date
2024-11-26
Estimated Expiration
2043-05-24

AI Technical Summary

Technical Problem

The existing cement slurry is not suitable for the solidification time under a large temperature difference environment, which affects the safety and progress of cementing construction, especially during the transmission process between high-temperature bottom and low-temperature wellhead.

Method used

By adding gypsum, red mud and sulfoaluminate cement to the cement slurry formula, the hydration reaction is used to generate ettringite, which improves the temperature difference adaptability of the cement slurry, and combines auxiliary agents such as water loss reducing agents, retarders and expansion agents , adjust the settling time of the cement slurry.

Benefits of technology

The thickening time of cement slurry at high temperatures and the condensation speed at low temperatures are significantly improved, the construction safety and progress of the cement slurry under a large temperature difference environment is ensured, and good compressive strength and adaptability are achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004246185330000061
    Figure BDA0004246185330000061
Patent Text Reader

Abstract

The invention belongs to the technical field of oil and gas wells, and discloses large-temperature-difference well cementation cement paste as well as a preparation method and application thereof. The cement paste comprises oil well cement, gypsum, red mud, sulphoaluminate cement, silicon powder, water and an auxiliary agent. The large temperature difference adaptive capacity of the cement paste is improved by generating ettringite in the hydration reaction process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of oil and gas wells, and more specifically, relates to a large temperature difference cementing slurry and a preparation method and application thereof. Background Art

[0002] As oil exploration and development continue to advance into deeper layers, oil and gas wells are being drilled deeper and deeper. At present, the deepest oil and gas wells in my country have exceeded 9,000 meters. Ultra-deep well construction brings many challenges such as high temperature and high pressure. Among them, the large temperature difference between the bottom of the well and the wellhead brings great difficulty to cementing construction. In normal cementing construction, cement slurry needs to be pumped from the wellhead to the bottom of the well through the casing, and then returned from the bottom of the well through the annulus between the casing and the well wall to the ground or a certain depth. For natural gas wells, cement slurry often needs to be returned from the bottom of the well to the ground. In order to meet the requirements of cementing construction, the pumpable time of cement slurry is generally required to reach more than 4 hours under the conditions of bottom hole circulation temperature test. For deep wells and ultra-deep wells, the bottom hole temperature is often more than 150°C. At such a high bottom hole temperature, a large amount of retarder needs to be added to the cement slurry to ensure the thickening time of the cement slurry. However, for natural gas wells, the cement slurry needs to be returned to the ground, which causes the cement slurry at the top of the casing and the well wall annulus to face a low temperature environment. Traditional cement slurry with a large amount of retarder does not solidify for a long time in a low temperature environment and has poor ability to adapt to large temperature differences, which seriously affects cementing safety and construction progress. Therefore, it is of great significance to develop high-performance large temperature difference cement slurry. Summary of the invention

[0003] The purpose of the present invention is to address the deficiencies of the prior art and to provide a large temperature difference cementing slurry and a preparation method and application thereof. The present invention improves the large temperature difference adaptability of the cement slurry by generating ettringite during the hydration reaction.

[0004] In order to achieve the above-mentioned object, the first aspect of the present invention provides a large temperature difference cementing slurry, which comprises oil well cement, gypsum, red mud, sulphoaluminate cement, silica powder, water and additives.

[0005] According to the present invention, preferably, the cement slurry comprises the following components in parts by weight: 95-105 parts of oil well cement, 5-15 parts of gypsum, 15-35 parts of red mud, 8-25 parts of sulphoaluminate cement, 30-50 parts of silica fume, 70-95 parts of water and 1-15 parts of additives;

[0006] Preferably, the cement slurry comprises the following components in parts by weight: 98-102 parts of oil well cement, 6-10 parts of gypsum, 20-35 parts of red mud, 10-20 parts of sulphoaluminate cement, 30-50 parts of silica fume, 73-95 parts of water and 1-15 parts of additives.

[0007] According to the present invention, preferably, the oil well cement is oil well G grade cement.

[0008] According to the present invention, preferably, the gypsum is hemihydrate gypsum.

[0009] According to the present invention, preferably, the red mud is Bayer process red mud.

[0010] According to the present invention, preferably, the mesh size of the silicon powder is 200-400 mesh, wherein the SiO 2 The content is greater than 99%.

[0011] According to the present invention, preferably, the water is water of different mineralization degrees, preferably at least one of fresh water, brackish water, salt water, salt water and brine.

[0012] The fresh water, brackish water, salt water, brine and brine are waters of different mineralizations known in the art, including: (1) fresh water, with a mineralization of less than 1 g / L; (2) brackish water (weakly mineralized water), with a mineralization of 1 to 3 g / L; (3) salt water (medium mineralized water), with a mineralization of 3 to 10 g / L; (4) salt water (strongly mineralized water), with a mineralization of 10 to 50 g / L; and (5) brine, with a mineralization of more than 50 g / L.

[0013] According to the present invention, preferably, the auxiliary agent comprises at least one of the following components in parts by weight: 1-5 parts of fluid loss additive, 1-2 parts of retarder, 1-4 parts of expansion agent and 1-4 parts of defoaming agent.

[0014] According to the present invention, preferably, the fluid loss agent is an acrylamide-based fluid loss agent and / or a polyvinyl alcohol-based fluid loss agent.

[0015] According to the present invention, preferably, the retarder is a copolymer of 2-acrylamido-2-methylpropanesulfonic acid and itaconic acid.

[0016] According to the present invention, preferably, the expansion agent is a calcium oxide expansion agent and / or a magnesium oxide expansion agent.

[0017] According to the present invention, preferably, the defoaming agent is an organosiloxane defoaming agent and / or a polyether defoaming agent.

[0018] In the present invention, oil well G-grade cement is used as a base material to ensure the strength of cement slurry. Gypsum and red mud react to form calcium sulfonate, and sulphoaluminate cement also reacts to form calcium sulfonate. Calcium sulfonate has an ultra-high specific surface area and decomposes at high temperatures. After the ultra-high specific surface area of ​​calcium sulfonate is generated under medium and low temperature conditions, it will adsorb a large amount of retarder, thereby reducing the amount of retarder used to delay cement hydration, thereby shortening the low-temperature setting time of cement slurry. However, at high temperatures, calcium sulfonate will decompose, so there is no calcium sulfonate in the cement slurry at high temperatures, and the retarder can better delay the hydration rate of cement, which is conducive to the guarantee of high-temperature thickening time.

[0019] The second aspect of the present invention provides a method for preparing the large temperature difference cementing slurry, which comprises mixing and stirring the oil well cement, gypsum, red mud, sulphoaluminate cement, silica powder, water and additives to obtain the large temperature difference cementing slurry.

[0020] The third aspect of the present invention provides application of the large temperature difference cementing slurry in large temperature difference cementing.

[0021] The beneficial effects of the technical solution of the present invention are as follows:

[0022] The invention introduces external admixtures such as gypsum, red mud, sulphoaluminate cement and the like which can additionally produce ettringite into the cement slurry formula, and produces ettringite in the hydration reaction process to improve the large temperature difference adaptability of the cement slurry.

[0023] Other features and advantages of the present invention will be described in detail in the following detailed description. DETAILED DESCRIPTION

[0024] The preferred embodiments of the present invention will be described in more detail below. Although the preferred embodiments of the present invention are described below, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided to make the present invention more thorough and complete, and to fully convey the scope of the present invention to those skilled in the art.

[0025] In the following examples and comparative examples, all components used can be obtained commercially;

[0026] The mesh number of the silicon powder is 200-400 mesh, wherein SiO 2 The content is greater than 99%.

[0027] Example 1

[0028] The present embodiment provides a large temperature difference cementing slurry, which includes the following components in parts by weight: 100 parts of oil well G grade cement, 6 parts of hemihydrate gypsum, 20 parts of Bayer red mud, 10 parts of sulphoaluminate cement, 35 parts of silica fume, 73 parts of fresh water, 2 parts of acrylamide fluid loss additive, 1 part of a copolymer of 2-acrylamido-2-methylpropane sulfonic acid and itaconic acid, 1 part of a calcium oxide expansion agent and 1 part of a polyether defoaming agent.

[0029] The preparation method of the large temperature difference cementing slurry comprises mixing and stirring the above components evenly to obtain the large temperature difference cementing slurry.

[0030] Example 2

[0031] The present embodiment provides a large temperature difference cementing slurry, which includes the following components in parts by weight: 100 parts of oil well G-grade cement, 10 parts of hemihydrate gypsum, 30 parts of Bayer red mud, 20 parts of sulphoaluminate cement, 35 parts of silica fume, 93 parts of slightly salty water, 4 parts of acrylamide fluid loss additive, 1.8 parts of a copolymer of 2-acrylamido-2-methylpropane sulfonic acid and itaconic acid, 3 parts of calcium oxide expansion agent and 1 part of polyether defoaming agent.

[0032] The preparation method of the large temperature difference cementing slurry comprises mixing and stirring the above components evenly to obtain the large temperature difference cementing slurry.

[0033] Example 3

[0034] The present embodiment provides a large temperature difference cementing slurry, which includes the following components in parts by weight: 100 parts of oil well G grade cement, 13 parts of hemihydrate gypsum, 35 parts of Bayer red mud, 8 parts of sulphoaluminate cement, 35 parts of silica fume, 80 parts of fresh water, 3 parts of acrylamide fluid loss additive, 1.3 parts of a copolymer of 2-acrylamido-2-methylpropane sulfonic acid and itaconic acid, 4 parts of magnesium oxide expansion agent and 1 part of polyether defoaming agent.

[0035] The preparation method of the large temperature difference cementing slurry comprises mixing and stirring the above components evenly to obtain the large temperature difference cementing slurry.

[0036] Example 4

[0037] The present embodiment provides a large temperature difference cementing slurry, which includes the following components in parts by weight: 100 parts of oil well G grade cement, 5 parts of hemihydrate gypsum, 15 parts of Bayer red mud, 8 parts of sulphoaluminate cement, 50 parts of silica fume, 73 parts of fresh water, 5 parts of acrylamide fluid loss additive, 2 parts of a copolymer of 2-acrylamido-2-methylpropane sulfonic acid and itaconic acid, 1 part of a magnesium oxide expansion agent, and 2 parts of a polyether defoaming agent.

[0038] The preparation method of the large temperature difference cementing slurry comprises mixing and stirring the above components evenly to obtain the large temperature difference cementing slurry.

[0039] Comparative Example 1

[0040] The comparative example provides a cementing slurry, which includes the following components in parts by weight: 100 parts of oil well G-grade cement, 35 parts of silica powder, 60 parts of fresh water, 1.5 parts of acrylamide fluid loss additive, 1 part of a copolymer of 2-acrylamide-2-methylpropane sulfonic acid and itaconic acid, 1 part of a calcium oxide expansion agent and 1 part of a polyether defoaming agent.

[0041] The preparation method of the cementing cement slurry comprises mixing and stirring the above components uniformly to obtain the cementing cement slurry.

[0042] Test Case

[0043] This test example tests the cement slurries of Examples 1-2 and Comparative Example 1. The test method is GBT 19139-2012 Oil Well Cement Test Method, and the results are shown in Table 1.

[0044] Table 1

[0045]

[0046] According to the results in Table 1, the thickening time of Comparative Example 1 at 160°C is 351min, and the compressive strength at 70°C for 48h is only 3MPa. The thickening time of Example 1 at 160°C is 319min, and the compressive strength at 70°C for 48h can reach 16MPa, showing good adaptability to large temperature differences. The thickening time of Example 2 at 160°C is 379min, and the compressive strength at 70°C for 48h can reach 14MPa, also showing good adaptability to large temperature differences. The thickening time of Example 3 at 160°C is 335min, and the compressive strength at 70°C for 48h can reach 12MPa, also showing good adaptability to large temperature differences. The thickening time of Example 4 at 160°C is 402min, and the compressive strength at 70°C for 48h can reach 9MPa, also showing good adaptability to large temperature differences. The thickening time at 160°C of Example 1, Example 2, and Example 3 are similar, the compressive strength at 70°C is also similar, and the large temperature difference performance is similar overall. However, the thickening time at 160°C of Example 4 is slightly longer, resulting in a slightly lower compressive strength at 70°C, but the large temperature difference performance is also better.

[0047] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.

Claims

1. A large temperature difference cementing slurry, characterized in that: The cement slurry comprises oil well cement, gypsum, red mud, sulphoaluminate cement, silica powder, water and additives.

2. The large temperature difference cementing slurry according to claim 1, wherein: The cement slurry comprises the following components in parts by weight: 95-105 parts of oil well cement, 5-15 parts of gypsum, 15-35 parts of red mud, 8-25 parts of sulphoaluminate cement, 30-50 parts of silica fume, 70-95 parts of water and 1-15 parts of additives; Preferably, the cement slurry comprises the following components in parts by weight: 98-102 parts of oil well cement, 6-10 parts of gypsum, 20-35 parts of red mud, 10-20 parts of sulphoaluminate cement, 30-50 parts of silica fume, 73-95 parts of water and 1-15 parts of additives.

3. The large temperature difference cementing slurry according to claim 1 or 2, wherein: The oil well cement is oil well G grade cement.

4. The large temperature difference cementing slurry according to claim 1 or 2, wherein: The gypsum is hemihydrate gypsum.

5. The large temperature difference cementing slurry according to claim 1 or 2, wherein: The red mud is Bayer process red mud.

6. The large temperature difference cementing slurry according to claim 1 or 2, wherein: The mesh number of the silicon powder is 200-400 meshes, and the SiO2 content thereof is greater than 99%.

7. The large temperature difference cementing slurry according to claim 1 or 2, wherein: The water is at least one of fresh water, brackish water, salt water, brine and brine.

8. The large temperature difference cementing slurry according to claim 1 or 2, wherein: The auxiliary agent comprises at least one of the following components in parts by weight: 1-5 parts of fluid loss reducer, 1-2 parts of retarder, 1-4 parts of expansion agent and 1-4 parts of defoamer; The fluid loss agent is an acrylamide fluid loss agent and / or a polyvinyl alcohol fluid loss agent; The retarder is a copolymer of 2-acrylamide-2-methylpropanesulfonic acid and itaconic acid; The expansion agent is a calcium oxide expansion agent and / or a magnesium oxide expansion agent; The defoamer is an organosiloxane defoamer and / or a polyether defoamer.

9. The method for preparing the large temperature difference cementing slurry according to any one of claims 1 to 8, characterized in that: The preparation method comprises the steps of mixing and stirring the oil well cement, gypsum, red mud, sulphoaluminate cement, silica powder, water and an auxiliary agent to obtain the large temperature difference well cementing cement slurry.

10. Use of the large temperature difference cementing slurry according to any one of claims 1 to 8 in large temperature difference cementing.

Citation Information

Patent Citations

  • Low temperature rapid hardening grouting material for offshore oil well and preparation method thereof

    CN105199692A

  • High-temperature-resistant large-temperature-difference elastic-tough cement paste system and preparation method thereof

    CN112479635A

Cited By

  • Process for preparing red mud cement and concrete compositions comprising the red mud cement

    WO2026154188A1