Hollow copper selenide box and preparation method and application thereof
The hollow Cu2-xSe microcube structure is constructed through the directional selenization reaction of Cu2O template, combined with paraffin composite materials, and the problem of insufficient absorption performance of low-frequency electromagnetic waves in the existing technology is solved, and the efficient electromagnetic wave absorption effect is achieved.
Patent Information
- Application Number
- CN202310615931.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-29
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-05-29
AI Technical Summary
There is a limited EMW attenuation mechanism for electromagnetic wave absorption materials in the GHz frequency range of existing 5G electronic devices, which is difficult to optimize impedance matching and improve electromagnetic response capabilities, especially inadequate absorption performance in the low frequency range.
Cu2O cubes are used as templates, and the Cu2O microcubes are converted into hollow Cu2-xSe microcube boxes at room temperature through the template directional in situ selenization reaction. Self-supported microcubes are constructed using the Kirkendal effect and Ostwald maturation effect. Cubic structure, forming a hollow selenized copper box, combined with paraffin composite material to improve electromagnetic wave absorption performance.
It realizes excellent electromagnetic wave absorption performance of hollow selenized copper boxes in the low frequency range, improves the volume gain and dielectric constant, and provides a lightweight and efficient EMW absorber manufacturing solution, and has good electromagnetic wave low frequency at 40 wt% filling amount. Absorption characteristics.
Smart Images

Figure CN119038499A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of wireless communication technology, and in particular to a hollow copper selenide box and a preparation method and application thereof. Background Art
[0002] The rapid development of 5G electronic devices in wireless communications and military applications has prompted researchers to develop electromagnetic wave absorbing materials in the GHz frequency range. However, challenges remain due to their limited EMW (electromagnetic wave) attenuation mechanism. To this end, people continue to work hard to improve their electromagnetic response capabilities and optimize impedance matching, including the careful design of parameters such as morphology, defect level, electronic conductivity, composition characteristics, and interface structure.
[0003] Copper selenide is a p-type semiconductor with high earth abundance. Due to their complex structure and valence states (such as Cu 0.87 Se, CuSe, Cu3Se2, Cu 1.8 Se, Cu2Se, CuSe2, etc.) lead to some unique optical and electrical properties, which make it widely used in many fields such as sensors, solar cells, electronic switches, etc., and a lot of work has been invested in the synthesis of copper selenide crystals with different morphologies such as nanoparticles, nanowires and nanotubes. Therefore, it is still of great significance to study new copper selenide absorbing materials and improve the electromagnetic wave absorption performance of copper selenide. Summary of the invention
[0004] The purpose of the present invention is to provide a hollow copper selenide box and a preparation method and application thereof. The hollow copper selenide box has excellent electromagnetic wave absorption performance and good low-frequency absorption characteristics.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides a method for preparing a hollow copper selenide box, comprising the following steps:
[0007] Copper salt, alkali, glucose and water are mixed and reduced to obtain Cu2O cubic powder;
[0008] Se powder and alkali solution are mixed and subjected to hydrothermal reaction to obtain a Se ion-containing solution;
[0009] The Cu2O cubic powder is mixed with water, and the obtained suspension is mixed with a Se ion-containing solution to perform a selenization reaction to obtain a hollow selenized copper box.
[0010] Preferably, the copper salt comprises copper sulfate, and the base comprises sodium hydroxide.
[0011] Preferably, the mass ratio of the copper salt, the base and the glucose is 7.5:3.6:4.2.
[0012] Preferably, the reduction temperature is 70° C. and the time is 30 min.
[0013] Preferably, the usage ratio of the Se powder to the alkali solution is 12.66mmol:50mL; and the concentration of the alkali solution is 2.5-10mol / L.
[0014] Preferably, the temperature of the hydrothermal reaction is 120° C. and the time is 4 hours.
[0015] Preferably, the molar ratio of the Cu2O cubic powder to the Se powder is 3.47:12.66.
[0016] Preferably, the temperature of the selenization reaction is room temperature, and the time is 3 to 5 hours.
[0017] The present invention provides a hollow copper selenide box prepared by the preparation method described in the above technical solution, which presents a hollow cubic structure.
[0018] The present invention provides application of the hollow copper selenide box described in the above technical solution in the field of electromagnetic wave absorption.
[0019] The present invention provides a method for preparing a hollow copper selenide box. The present invention uses a Cu2O cube as a sacrificial template, and successfully converts the Cu2O microcube into Cu by a wet chemical method at room temperature through a template-directed in-situ selenization reaction. 2-x Se microcubic box, the present invention realizes a self-supporting microcubic structure hollow Cu under the synergistic effect of Kirkendall effect and Ostwald ripening effect 2-x The construction of Se heterogeneous copper selenide box has rare low-frequency electromagnetic wave absorption performance.
[0020] In addition, the hollow structure in the copper selenide box prepared by the present invention solves the problem of high density of conventional copper selenide. The reduced density makes the hollow powder have a higher filling volume than conventional powder under the same filling mass in the matrix. The increase in filling volume has a certain gain on the dielectric constant (particles contact each other to form a conductive network), so the absorbing material can play a role under a lower filling mass of the absorber, and the hollow structure material provides an effective idea for the manufacture of lightweight and efficient EMW absorbers due to good impedance matching, high loss and adjustable electromagnetic parameters.
[0021] The hollow Cu prepared by the present invention 2-x The composite product of Se selenide copper box and paraffin has excellent electromagnetic wave absorption properties, and has good EMW (electromagnetic wave) low-frequency absorption properties (from 4GHz) when the filling amount is 40wt%. The minimum RL value of T5 / paraffin-40wt% at 2.6mm-5.0mm exceeds -20dB. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 XRD (a), SEM (b) and particle size distribution diagram (c) of Cu2O cubic powder prepared in the present invention;
[0023] Figure 2 XRD patterns of Cu2O cubic templates after different selenization times (T1-T5) from 15 min to 5 h (a) and three Cu 2-x Standard diffraction pattern of Se (b);
[0024] Figure 3 TEM images of Cu2O at different stages during the selenization process;
[0025] Figure 4 Cu prepared at different NaOH concentrations 2-x XRD patterns of Se(N1-N3) (a) and CuO, Cu3Se2 and Cu 0.87 Standard diffraction spectrum of Se (b);
[0026] Figure 5 TEM images of selenization products (N1-N3) of Cu2O cubic powder at different NaOH concentrations;
[0027] Figure 6 The curves of ε′ and ε″ varying with frequency (ab), dielectric loss (c) and Cole-Cole curve (df) of T5 / paraffin with different filling ratios;
[0028] Figure 7 R of T5 / paraffin-30wt%, T5 / paraffin-40wt%, T5 / paraffin-50wt% at 2-18GHz L Change diagram (ac) and two-dimensional R of T5 / paraffin-40wt% L Figure (d). DETAILED DESCRIPTION
[0029] The present invention provides a method for preparing a hollow copper selenide box, comprising the following steps:
[0030] Copper salt, alkali, glucose and water are mixed and reduced to obtain Cu2O cubic powder;
[0031] Se powder and alkali solution are mixed and subjected to hydrothermal reaction to obtain a Se ion-containing solution;
[0032] The Cu2O cubic powder is mixed with water, and the obtained suspension is mixed with a Se ion-containing solution to perform a selenization reaction to obtain a hollow selenized copper box.
[0033] In the present invention, unless otherwise specified, the required reagents are commercially available products well known in the art.
[0034] The invention mixes copper salt, alkali, glucose and water, performs reduction, and obtains Cu2O cubic powder.
[0035] In the present invention, the copper salt preferably includes copper sulfate, more preferably copper sulfate pentahydrate; the alkali preferably includes sodium hydroxide.
[0036] In the present invention, the mass ratio of the copper salt, the base and the glucose is preferably 7.5:3.6:4.2.
[0037] The present invention preferably dissolves the copper salt in part of the water, and under the set reduction temperature condition, the copper salt is completely dissolved by stirring, the alkali is dissolved in the remaining water, the obtained alkali solution is added to the copper salt solution, and the stirring is continued for 5 minutes before adding glucose to carry out reduction.
[0038] In the present invention, the reduction temperature is preferably 70° C., and the time is preferably 30 min; and the reduction is preferably carried out under stirring conditions.
[0039] After the reduction is completed, the present invention preferably collects the obtained product by centrifugation, filters the excess liquid, washes the product with deionized water, and vacuum dries it at 50° C. for 12 h to obtain Cu2O cubic powder.
[0040] The present invention mixes Se powder and alkali solution, performs hydrothermal reaction, and obtains Se ion solution. In the present invention, the usage ratio of Se powder to alkali solution is preferably 12.66mmol:50mL; the concentration of alkali solution is preferably 2.5-10mol / L, more preferably 5-7.5mol / L; the alkali in the alkali solution is preferably sodium hydroxide.
[0041] The present invention has no particular limitation on the process of mixing the Se powder and the alkali solution, and the materials can be mixed uniformly according to a process well known in the art.
[0042] In the present invention, the temperature of the hydrothermal reaction is preferably 120°C, and the time is preferably 4 hours. During the hydrothermal reaction, Se reacts with the alkali solution to form Se 2- , Se is converted into 2 / 3Na2Se and 1 / 3Na2SeO3.
[0043] After the hydrothermal reaction is completed, the present invention preferably cools the obtained system to room temperature naturally, filters and separates excess Se powder, and collects the liquid material, which is an alkaline Se ion solution (containing Na2Se and Na2SeO3).
[0044] After obtaining the Se-containing ion solution, the present invention mixes the Cu2O cubic powder with water, mixes the obtained suspension with the Se-containing ion solution, performs a selenization reaction, and obtains a hollow selenized copper box.
[0045] The present invention has no special limitation on the usage ratio of the Cu2O cubic powder and water, as long as the Cu2O cubic powder is fully dispersed and suspended; in an embodiment of the present invention, specifically 3.47 mmol Cu2O cubic powder is stirred and dispersed in 400 mL deionized water.
[0046] In the present invention, the molar ratio of the Cu2O cubic powder to the Se powder is preferably 3.47:12.66.
[0047] In the present invention, the temperature of the selenization reaction is preferably room temperature, and the time is preferably 3 to 5 hours; the selenization reaction is preferably carried out under stirring conditions; the present invention has no special limitation on the stirring, and the reaction can be carried out smoothly according to the process known in the art. During the selenization reaction, the Cu2O cube acts as a sacrificial template, and the Na2Se in the Se ion solution plays a role in selenizing Cu2O to form copper selenide.
[0048] After the selenization reaction is completed, the present invention preferably collects the product by suction filtration, then washes it with deionized water, and then vacuum dries the obtained product to obtain a hollow selenized copper box. The present invention has no special restrictions on the suction filtration and vacuum drying, and can be carried out according to processes well known in the art.
[0049] The present invention provides a hollow copper selenide box prepared by the preparation method described in the above technical solution, which presents a hollow cubic structure.
[0050] The present invention provides the application of the hollow copper selenide box described in the above technical solution in the field of electromagnetic wave absorption. The present invention has no special limitation on the application method, and the application can be carried out according to methods well known in the art.
[0051] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0052] Examples 1 to 8
[0053] Table 1 Raw material dosage and selenization time in different cases
[0054]
[0055] 7.5 g of CuSO4·5H2O was dissolved in 300 mL of deionized water and completely dissolved under stirring at 70°C. Then, 30 mL of the prepared NaOH solution (containing 3.6 g of NaOH) was added. After continuous stirring for 5 min, 4.2 g of glucose was added and the reaction was continued for 30 min. The product was collected by centrifugation, the excess liquid was filtered, and the product was washed with deionized water and vacuum dried at 50°C for 12 h to obtain Cu2O cubic powder.
[0056] Se powder (amount as shown in Table 1) was dissolved in 50 mL of NaOH solution (concentration as shown in Table 1), kept at 120°C for 4 h, cooled naturally to room temperature, and the excess Se powder was filtered to separate the alkaline aqueous solution containing selenium ions;
[0057] 3.47 mmol of the prepared Cu2O cubic powder was added to 400 mL of deionized water to obtain a Cu2O suspension. The above-mentioned selenium ion-containing aqueous solution was added to the obtained Cu2O suspension under continuous stirring, and selenization was carried out at room temperature with stirring (selenization time is shown in Table 1). The product was collected by filtration, washed with deionized water, and the obtained product was vacuum dried to obtain a hollow selenized copper box.
[0058] Characterization and performance testing
[0059] 1) Scanning electron microscopy (SEM, ZEISS sigma500) and transmission electron microscopy (TEM, FEI-Tecnai G2 F20) were used to observe the surface and internal morphology of the samples prepared in different embodiments. X-ray powder diffraction (XRD, UltimalV, Cu / Kα), TEM-SEAD mode and EDS-Mapping energy spectrum (BRUKER XFlash 6130) were used to analyze the phase and composition of the samples.
[0060] Figure 1 XRD (a), SEM (b) and particle size distribution diagram (c) of the Cu2O cubic powder prepared in the present invention, as shown in FIG. Figure 1 As shown, the prepared Cu2O cubes are completely consistent with the Cu2O crystal standard card PDF#74-1230 (a), and the prepared Cu2O cubes have uniform particle size, smooth surface, and good dispersion (b). The size-frequency distribution of the Cu2O cubes is normally distributed, and the average particle size is about 1μm (c).
[0061] Figure 2 (a) shows the XRD pattern of the Cu2O cubic template after different selenization times (T1-T5) from 15min to 5h, where the solid dots correspond to the diffraction peaks of Cu2O. It can be clearly seen that with the extension of selenization time, the diffraction peak representing the Cu2O{111} plane at 36.46° gradually disappears, indicating that the product is gradually converted from Cu2O to Cu 2-x Se. Figure 2 (b) shows three types of Cu 2-x Standard diffraction patterns of Se, including two types of CuSe (20-1020, hexagonal and 27-0184, orthorhombic) and Cu 0.87 Se. It can be seen that when the Cu 2-xThe main phase of Se is hexagonal CuSe. When the reaction time is 1h, orthorhombic CuSe appears briefly. 2-x CuSe in Se is eventually replaced by Cu 0.87 Se substitution (3h and 5h), which may be the Se in the system 2- After comparing with the standard diffraction spectrum, the main components of T4 and T5 are Cu 0.87 Se.
[0062] Figure 3 TEM images of Cu2O at different stages during the selenization process, where (a) represents the selenization time of 15 min, (b) represents the selenization time of 30 min, (c) represents the selenization time of 1 h, (d) represents the selenization time of 3 h, and (e) represents the selenization time of 5 h. Figure 3 As shown in the figure, the morphology of the products at different stages is very different. In the first 30 minutes, the cubic morphology can be well inherited, but the surface gradually becomes rough and wrinkled, indicating that the surface of the Cu2O cube is converted into Cu 2-x Se(ab). The selenization time was increased to 1h, Cu 2-x Se gradually increased and began to detach from the Cu2O surface, exposing the spherical Cu2O core (c). By 3 h, the internal Cu2O was almost completely consumed, and the free Cu 2-x Se is in the form of tortuous nanoplates, which are aggregated and connected to each other, and the prototype of hollow cubes can be observed (d). When the reaction is carried out for 5 hours, Cu 2-x Se hollow box, the wall of the box is composed of coarse grains, the surface is rough, and there are gaps inside. It is similar to the original Cu2O cube shape, but the size has increased significantly (e). f is the TEM high-resolution mode image of T5. The result of measuring the interplanar spacing in the lattice fringes is 0.32nm, corresponding to Cu 0.87 Se {102} crystal plane (the diffraction peak at 28.1° in the XRD pattern). However, the SEAD electron diffraction inset in f shows both single crystal diffraction spots and polycrystalline diffraction rings, which indicates that T5 is not pure Cu 0.87 Se and possibly Cu 2-x Other varieties of Se.
[0063] In summary, the present invention prepares a copper selenide box through the combined action of the Kirkendall effect and the Ostwald ripening effect: 2-x The solubility of Se in alkaline aqueous solution is much lower than that of Cu2O, so Se 2- ions come into contact with Cu2O. +The chemical valence change of the ions also causes a redox reaction. At this time, the Cu2O particles maintain a cubic morphology, with only a thin layer of Cu formed on the surface. 2-x Se film, this film is composed of many small Cu 2- x Se grains. Then, under the action of Kirkendall effect, Cu in Cu2O + The ions migrate from the inside to the outside and interact with the external Se 2- ions continue to react. 2-x Se grains detach from Cu2O and grow and thicken into shells during Ostwald ripening until Cu2O is completely consumed and the surrounding Cu 2-x Se aggregated into incomplete hollow cubes. Finally, in order to maintain the lowest energy of the system during Ostwald ripening, the smaller Cu 2-x Se fragments will gradually dissolve and re-precipitate on the surface of larger grains. This grain coarsening process makes Cu 2-x The Se shell thickened and eventually developed into a hollow cube with a complete morphology.
[0064] Cu2O-based Cu 2-x The formation of Se hollow boxes can be attributed to chemical reactions (1) and (2):
[0065] 3Se+6NaOH→2Na2Se+Na2SeO3+3H2O (1)
[0066] 2Cu2O+4Na2Se+4H2O+O2→4CuSe+8NaOH (2).
[0067] 2) Se 2- The Se powder is obtained through the disproportionation reaction in the alkaline solution, which shows that the alkaline solution has a great influence on Se 2- The acquisition of Cu plays an important role. This paper studies the effect of different NaOH concentrations on Cu 2-x The influence of Se morphology.
[0068] Figure 4 (a) shows the Cu prepared at different NaOH concentrations. 2-x XRD pattern of Se(N1-N3), solid circles represent the characteristic diffraction peaks of Cu2O. Figure 1 Similar to (a), as the concentration of NaOH increases, the characteristic diffraction peak of Cu2O gradually disappears, and the product is completely converted into Cu 2-x Se. Figure 4 (b) is CuO, Cu3Se2 and Cu 0.87From the standard diffraction spectrum of Se, we can see that when the concentration of NaOH is 2.5M, the product consists of three phases: Cu2O, CuO and Cu3Se2. + The valence of the ions increases, so CuO may be an intermediate product of the selenization reaction of Cu2O. When the NaOH concentration is above 5.0M, the characteristic diffraction peaks of Cu2O and CuO weaken until they disappear, and the diffraction peak at 26.9° gradually becomes stronger (corresponding to Cu 0.87 Se). Until 7.5M, the product does not contain any copper oxides, and Cu 2-x Se is composed of Cu3Se2 and Cu 0.87 In fact, when the NaOH concentration is below 10 M, there is excess Se powder that can be filtered, indicating that Se→Se 2- Therefore, when the NaOH concentration is low, the product contains not only copper oxides but also Cu 2-x The proportion of Cu element in Se is generally higher.
[0069] Figure 5 TEM images of selenization products (N1-N3) of Cu2O cubic powder at different NaOH concentrations, where (a) represents a NaOH concentration of 2.5 M, (b) represents a NaOH concentration of 5 M, and (c) represents a NaOH concentration of 7.5 M; Figure 5 As shown in the figure, when the NaOH concentration is below 5M, it can be observed that the Cu 2-x Se fragments gradually aggregate into Cu 2-x The prototype of Se box (ab). Until the NaOH concentration reaches 7.5M, Cu 2-x Se develops into a complete hollow box (c). However, compared with T5 (NaOH concentration is 10 M), the Cu 2-x The walls of the Se box are thinner because the Se 2- The above experiments confirm the existence of the Kirkendall effect and Ostwald ripening process, and the speed of these reactions is controlled by Se 2- Affected by concentration.
[0070] 3) The complex dielectric constant of the sample at 2-18 GHz was measured using a vector network analyzer (VNA, PNA-N5234A). The sample powder was uniformly mixed with the paraffin matrix at different mass fractions and then pressed into a ring-shaped mold with an inner diameter of 3.04 mm and an outer diameter of 7.00 mm.
[0071] Copper selenide powder (T5) is filled in a paraffin matrix at different ratios to make T5 / paraffin composite materials. Since copper selenide is non-magnetic, the real part (μ′) and imaginary part (μ″) of the complex magnetic permeability can be approximated to 1 and 0, respectively. In non-magnetic media, the complex dielectric constant (ε r =ε′-jε″) determines the electromagnetic wave absorption characteristics. The real part ε′ represents the storage capacity of electrical energy, and the imaginary part ε″ reflects the electrical loss capacity.
[0072] Figure 6 Figures ab are curves of ε′ and ε″ with frequency when T5 is filled at 30wt%, 40wt% and 50wt%, respectively. Obviously, the complex dielectric constant increases with the increase of copper selenide filling ratio, and the increase is more obvious when it increases from 40wt% to 50wt%. When the copper selenide filling ratio is low, the copper selenide particles are isolated by paraffin, and when the filling ratio increases to a certain critical value, the copper selenide particles in the matrix will be connected to each other to form a conductive path. At this time, the conductivity of the copper selenide / paraffin composite material will be greatly increased, thereby significantly improving the complex dielectric constant. Through the dielectric loss tangent value (tanδ E =ε″ / ε′) characterizes the dielectric loss capacity of different filling ratios T5 / paraffin ( Figure 6 c), when the filling ratio reaches 50wt%, tanδ E The values are all above 1 in the range of 2-18 GHz. Although T5 / paraffin-50wt% has extremely strong dielectric loss capacity, its complex dielectric constant is too high, so electromagnetic waves will be strongly reflected and cannot smoothly enter the absorber, so its electromagnetic wave absorption performance is not necessarily good. Figure 6 It was observed that the dielectric loss peaks gradually shifted to lower frequencies with the increase of filling ratio, and these loss peaks may be caused by polarization loss.
[0073] The Debye relaxation effect is described as follows: ∞ and ε s They represent the dielectric constant in the high frequency limit and the static dielectric constant respectively.
[0074]
[0075] If only Debye relaxation occurs, the curves of ε′ and ε″ will form a Cole-Cole semicircle. Figure 6 df represents the Cole-Cole curves of T5 / paraffin with different filling ratios. When the filling amount is 30wt% and 40wt%, as the frequency increases, the corresponding Cole-Cole curves rise in a spiral shape, indicating that they have multiple polarization processes. 0.87 Se, including other Cu 2-xSe species, so the multipolarization process may come from the dipole polarization and interface polarization of these copper selenides. When the filling amount reaches 50wt%, the circular shape is almost unobservable, indicating that the high dielectric loss of T5 / paraffin-50wt% is not dominated by polarization relaxation loss, but is covered by high conductive loss.
[0076] Reflection loss (R L ) can be used to evaluate the absorption characteristics of electromagnetic waves (Formula 4-5):
[0077]
[0078]
[0079] Z0 represents the normalized free space impedance (Z0 = 1), Z in represents input impedance, c is the speed of light, f is the frequency of EM wave, d is the thickness of the absorber, j is an imaginary number, μ r is the complex magnetic permeability. R of T5 / paraffin-30wt% (a), T5 / paraffin-40wt% (b), T5 / paraffin-50wt% (c) at 2-18GHz L Changes such as Figure 7 As shown in the figure, within the absorber thickness range of 0-5mm, the filling mass of 40wt% has the best comprehensive performance. The electromagnetic wave loss capacity caused by low filling amount (30wt%) is too weak, and the electromagnetic wave reflection caused by high filling amount (50wt%) is too strong, which makes the absorber unable to obtain good electromagnetic wave absorption performance. In addition, the absorption peak of T5 / paraffin-40wt% is mainly concentrated in the low frequency range ( Figure 7 In d), the minimum R L The values are all over -20dB, which is equivalent to at least 99% loss of electromagnetic wave energy. When the absorber thickness is 3.8mm, R L The value reaches -35.2dB. Many dielectric lossy electromagnetic wave absorbing materials mainly absorb high frequencies, and the copper selenide box prepared by the present invention has rare low-frequency characteristics.
[0080] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a hollow copper selenide box, characterized in that: The following steps are involved: Copper salt, alkali, glucose and water are mixed and reduced to obtain Cu2O cubic powder; Se powder and alkali solution are mixed and subjected to hydrothermal reaction to obtain a Se ion-containing solution; The Cu2O cubic powder is mixed with water, and the obtained suspension is mixed with a Se ion-containing solution to perform a selenization reaction to obtain a hollow selenized copper box.
2. The preparation method according to claim 1, characterized in that: The copper salt includes copper sulfate, and the base includes sodium hydroxide.
3. The preparation method according to claim 1 or 2, characterized in that: The mass ratio of the copper salt, alkali and glucose is 7.5:3.6:4.
2.
4. The preparation method according to claim 1, characterized in that: The reduction temperature is 70° C. and the time is 30 min.
5. The preparation method according to claim 1, characterized in that: The usage ratio of the Se powder to the alkali solution is 12.66mmol:50mL; the concentration of the alkali solution is 2.5-10mol / L.
6. The preparation method according to claim 1 or 5, characterized in that: The temperature of the hydrothermal reaction is 120° C. and the time is 4 hours.
7. The preparation method according to claim 1, characterized in that: The molar ratio of the Cu2O cubic powder to the Se powder is 3.47:12.
66.
8. The preparation method according to claim 1, characterized in that: The temperature of the selenization reaction is room temperature and the time is 3 to 5 hours.
9. The hollow copper selenide box prepared by the preparation method according to any one of claims 1 to 8, characterized in that: It presents a hollow cube structure.
10. Use of the hollow copper selenide box according to claim 9 in the field of electromagnetic wave absorption.
Citation Information
Patent Citations
Copper selenide hollow tubular multi-stage structure material as well as preparation method and application thereof
CN105513806A
Method for preparing hexagonal copper sulfide nano-sheets
CN108529661A
Controllable preparation method and application of Cu7S4-Cu9S8 heterostructure hollow cube catalyst
CN109465017A
Copper oxide nanoparticle catalyst with large-cavity eggshell structure as well as preparation method and application of copper oxide nanoparticle catalyst
CN113235112A