Lightweight extrusion blow molding product and preparation method thereof
By using hollow glass microbeads modified by coupling agent in blow molding, the difficulty of lightening blow molded products in the prior art is solved, the lightening effect on existing equipment is achieved, and the strength and appearance of the product are maintained. Quality, suitable for a variety of packaging products.
Patent Information
- Application Number
- CN202411308659.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-11-29
AI Technical Summary
The existing technology is difficult to effectively realize the lightweight of blow-molded products. The traditional chemical foaming method has excessively affected the appearance and mechanical properties. The supercritical gas foaming method has high equipment costs, and the existing foaming agent is under the shearing effect of screws. It is prone to cracking and leaking, and cannot meet the use requirements of the daily chemical and food industries.
In the extrusion blow molding, hollow glass microbeads modified by coupling agent are introduced, and their compressive strength and compatibility are improved by silane coupling agent treatment. The matrix resin and paraffin oil are mixed and then blow molded to achieve In-situ bubbles reduce density and achieve lightweight effect.
It realizes the preparation of lightweight blow molded products without modification on existing equipment, maintains the strength and appearance quality of the products, reduces the use of plastic materials, reduces the cost of products, and is suitable for hollows such as blow molding barrels, bottles, boxes, etc. Production of products.
Smart Images

Figure CN119039685A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of packaging materials, and in particular to a lightweight extrusion blow molding product and a preparation method thereof. Background Art
[0002] After waste plastics enter the environment, they are difficult to degrade and are likely to cause long-term and deep-seated ecological and environmental problems. Packaging is the main area of plastic consumption, accounting for about 40% of the total plastic consumption. Therefore, it is a general trend to design lightweight plastic hard packaging materials, which account for the largest proportion of packaging materials, and extrusion blow molding products account for the largest proportion of hard packaging. The simplest way to lightweight extrusion blow molding products is to reduce the use of plastic materials by changing the structural design, but this method is limited to reducing the use of plastic materials. When the thinning reaches a certain level, the performance of the blow molding products will not meet the use requirements. Compared with pure plastics, foam plastics have the advantages of low density and high specific strength. Therefore, it is a good choice to introduce air or other gases into the product by foaming to achieve the purpose of reducing the amount of plastic materials.
[0003] For the foaming of injection molded parts, there are relatively mature solutions on the market. For blow molded products, there is currently no mature foaming solution in the industry. The foam cells of products prepared by the traditional chemical foaming method are too large, which has a great impact on the appearance quality and mechanical properties of blow molded products, and the residual chemical reagents may have an adverse effect on the product contents, which cannot meet the use requirements of daily chemical and food industries. It is currently commonly used in the preparation of automobile air intake ducts or air ducts (Chinese patent CN113896973A, Chinese patent CN114379061A, Chinese patent CN 114425895A). Another method is supercritical gas foaming, which requires a substantial transformation of traditional blow molding processing equipment (such as Chinese patent CN109955493A), and the equipment cost is high. In addition, Chinese patent CN117209809A mentions a core-shell microsphere foaming agent masterbatch that can be used for blow molding foaming. The shell of this foaming agent softens during heating, and the internal low-boiling hydrocarbons gasify to promote the expansion of the shell, thereby playing a foaming role. However, the shell polymer of such polymer microspheres is easily broken at high temperatures, especially under the shearing action of the screw, causing leakage of low-boiling hydrocarbon foaming agents. Therefore, such foaming agents are more often used in situations such as compression molding where screw shearing is not required. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a lightweight extrusion blow-molded product and a preparation method thereof, wherein hollow glass microspheres modified by a coupling agent are introduced into the extrusion blow-molding process to obtain a lightweight blow-molded product.
[0005] The specific technical solutions include the following:
[0006] In a first aspect, a lightweight extrusion blow-molded product is provided, comprising hollow glass microspheres modified by a coupling agent.
[0007] Furthermore, the weight portion of the coupling agent-modified hollow glass microspheres is 10-20 parts.
[0008] Furthermore, the lightweight extrusion blow-molded product also includes the following components in parts by weight: 75-85 parts of base resin, 1-2 parts of paraffin oil and 3-4 parts of masterbatch.
[0009] Furthermore, the density of the hollow glass microspheres modified by the coupling agent is 0.4-0.6 g / cm 3 .
[0010] Furthermore, the compressive strength of the coupling agent-modified hollow glass microspheres is greater than or equal to 42 MPa.
[0011] Furthermore, the coupling agent-modified hollow glass microspheres are prepared by hollow glass microspheres being modified with a silane coupling agent.
[0012] Furthermore, the silane coupling agent is one or more of 3-aminopropyltriethoxysilane, γ-mercaptopropyltriethoxysilane, and γ-mercaptopropyltrimethoxysilane.
[0013] Furthermore, the method for preparing the coupling agent-modified hollow glass microspheres comprises the following steps:
[0014] Take the hollow glass microspheres for later use, add the silane coupling agent to the mixture of ethanol and pure water, add acetic acid to adjust the pH to 3-5, hydrolyze for 5-8 minutes to obtain a mixed liquid, add the mixed liquid to the hollow glass microspheres, stir evenly in a high-speed mixer, and finally dry in an oven at 60-70°C for 8-9 hours, cool and set aside, and obtain the hollow glass microspheres modified by the coupling agent.
[0015] In a second aspect, a method for preparing a lightweight extrusion blow molded product as described in the first aspect is provided, comprising the following steps:
[0016] S1. Mixing: Adding a base resin and paraffin oil in a high-speed mixer and stirring so that the plastic particles of the base resin are fully wetted by the paraffin oil, and then adding the coupling agent-modified hollow glass microspheres and masterbatch, mixing evenly, to obtain a uniformly mixed material;
[0017] S2. Blow molding: The evenly mixed material is blow molded through an extrusion blow molding machine to obtain a lightweight extrusion blow molded product.
[0018] Furthermore, in step S2, the extrusion temperature of the blow molding machine is 160-180°C, and the blow molding pressure is 0.5-0.8 MPa.
[0019] In a third aspect, there is provided application of the method for preparing a lightweight extrusion blow-molded product as described in the second aspect in preparing a hollow blow-molded product.
[0020] The present invention introduces hollow glass microspheres modified by coupling agents during blow molding, that is, introduces in-situ bubbles during the molding process, reduces the density of the product, achieves lightweight blow-molded products, and reduces the use of plastic materials. Compared with the prior art, the lightweight extrusion blow-molded products and the preparation method thereof provided by the present invention have the following beneficial effects:
[0021] 1. No equipment modification is required, and the lightweight of blow-molded products can be achieved directly on the existing extrusion blow molding machine.
[0022] 2. Hollow glass microspheres have bubbles in them, and the molding process does not involve the foaming process, does not require complex process control, and is simple and easy.
[0023] 3. The hollow glass microspheres themselves have a certain strength. After being modified with coupling agents, their compatibility with the matrix resin is improved, so that the strength of the material is maintained well, so that the compressive strength of the product can be maintained at more than 85% of the matrix resin product, ensuring that the drop performance of the product meets the use requirements.
[0024] 4. Without affecting the performance of the product, the apparent density of the product is reduced by 10%, which can reduce the use of plastic raw materials and reduce the overall cost of the product.
[0025] 5. This method is universal and can be used for the production of hollow products such as blow-molded barrels, bottles, and boxes. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying any creative work.
[0027] Figure 1 This is a micrograph of the hollow glass microspheres modified by the coupling agent used in Examples 1-3 of the present invention;
[0028] Figure 2 The hollow blow-molded bottle prepared in Example 3 of the present invention (left) and the hollow blow-molded bottle prepared in Comparative Example 1 (right);
[0029] Figure 3 This is a SEM image of the tensile section of Example 3 of the present invention;
[0030] Figure 4 This is the SEM image of the tensile section of comparative example 6 of the present invention. DETAILED DESCRIPTION
[0031] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] It should be understood that when used in this specification and the appended claims, the terms "include" and "comprises" indicate the presence of described features, integers, steps, operations, elements and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components and / or combinations thereof.
[0033] It should also be understood that the terms used in this specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. As used in the specification of the present invention and the appended claims, unless the context clearly indicates otherwise, the singular forms "a", "an" and "the" are intended to include plural forms.
[0034] It should be further understood that the term "and / or" used in the present description and the appended claims refers to any and all possible combinations of one or more of the associated listed items, and includes these combinations.
[0035] In order to more fully understand the technical content of the present invention, the technical solution of the present invention is further introduced and illustrated in conjunction with specific embodiments below.
[0036] Unless otherwise specified, the parts described in the present invention are all parts by weight.
[0037] Among them, the compressive strength (90% retention) of the coupling agent modified hollow glass microspheres described in the present invention refers to the isostatic strength of the coupling agent modified hollow glass microspheres measured by the water pressure method specified in JC / T2284-2014. 90% retention refers to the compressive strength when the volume breakage rate of the coupling agent modified hollow glass microspheres is 10%.
[0038] Preparation method of hollow glass microspheres modified by coupling agent:
[0039] Take the hollow glass microspheres for later use, add the silane coupling agent to the mixture of ethanol and pure water, add acetic acid to adjust the pH to 3-5, hydrolyze for 5-8 minutes to obtain a mixed liquid, add the mixed liquid to the hollow glass microspheres, stir evenly in a high-speed mixer, and finally dry in an oven at 60-70°C for 8-9 hours, cool and set aside, and obtain the hollow glass microspheres modified by the coupling agent.
[0040] Preparation method of lightweight extrusion blow molding products:
[0041] S1. Mixing: Adding a base resin and paraffin oil in a high-speed mixer and stirring so that the plastic particles of the base resin are fully wetted by the paraffin oil, and then adding the coupling agent-modified hollow glass microspheres and masterbatch, mixing evenly, to obtain a uniformly mixed material;
[0042] S2. Blow molding: The uniformly mixed material is blow molded through an extrusion blow molding machine to obtain a lightweight extrusion blow molded product. The extrusion temperature of the blow molding machine is 160-180°C, and the blow molding pressure is 0.5-0.8MPa.
[0043] Performance Testing
[0044] 1. Apparent density and weight test of blow molded products
[0045] In order to characterize the effect of adding hollow glass microspheres on the "lightweight" of blow-molded products, the apparent density of the blow-molded products and the weight of the blow-molded bottles of the embodiments and comparative examples were tested. The specimens were cut from the blow-molded bottles, and the apparent density of each sample was tested with a densitometer (AR-120-4S, Guangdong Qiya Testing Equipment Co., Ltd.), and 5 different positions were taken to calculate the average value. The weight test of the blow-molded bottles was carried out on an electronic balance (PL3002-1C Mettler-Toledo Instruments (Shanghai) Co., Ltd.), and 10 samples of each type were taken and the average value was taken. During the blow-molding process, the average thickness of the bottle body was controlled to keep the average thickness of the bottle body at 1.0-1.3mm, ensuring that the volume of the bottle body in each embodiment and comparative example was similar, so that its apparent density was proportional to the weight of the bottle. Therefore, when the apparent density is reduced by more than 10% compared with the density of pure resin, it can be judged that the purpose of "lightweight" has been achieved. When the apparent density or bottle weight is reduced too little, the plastic material reduced is very limited.
[0046] 2. Strength test of blow molded products
[0047] In order to test the effect of adding hollow glass microspheres on the strength of blow-molded products, we tested the compressive strength and drop performance of blow-molded bottles. The compressive strength test was carried out by placing an empty bottle with a cap vertically on a universal testing machine (AGS-J, Shimadzu Instruments (Suzhou) Co., Ltd.), with a compression speed of 100mm / min. The maximum pressure was taken as its compressive strength. Ten bottles of each type were tested and the average value was taken. The drop test was to add a nominal weight (1kg) of water to the bottle, and then drop it at a height of 1.2m for a total of 3 times, namely vertical drop, plane drop and side drop. Ten samples of each type were made, and the number of broken or leaking bottles was recorded and the breakage rate was calculated. The drop breakage rate was required to be 0%. If damage or leakage was found in the drop test, the test was judged to be unsuccessful. Generally, when the compressive strength can be maintained at 85% of that of pure resin products, the drop strength of the product can meet the requirements.
[0048] The drop performance of blow-molded products is closely related to the tensile strength of the material. In order to further characterize the effect of the addition of hollow glass microspheres on the strength of the material, we tested the tensile properties of the material and used a scanning electron microscope to observe the morphology of the tensile section to further analyze the reasons for the strength change, because generally the better the compatibility of the filler with the resin, the higher the strength of the material, and accordingly, the higher the strength of the product. The specific test method is as follows: Use a punching machine to cut the blow-molded bottle body into dumbbell-shaped strips with a thickness of about 1.2mm, a length of 10cm, and a width of 10mm. Use an AGS-J universal testing machine (Shimadzu Instruments (Suzhou) Co., Ltd.) to test the tensile strength of the strips, and the tensile rate is 50mm / min. After the tensile section is sprayed with gold, it is observed with a Phenom ProX scanning electron microscope (Themo Scientific).
[0049] 3. Appearance inspection of hollow glass microspheres and blow-molded bottles
[0050] In order to characterize the effect of adding hollow glass microspheres on the apparent quality of the product, we used a microscope (OLYMPUSBX53) to observe the morphology of the hollow glass microspheres and test their size, and conducted an appearance inspection on the prepared blow-molded bottles. For plastic products, usually when the filler size is small, it has no effect on the appearance quality of the product. When the filler size is large, the filler will protrude from the surface, making the surface of the product rough.
[0051] Raw materials used in the embodiments and comparative examples:
[0052] Coupling agent modified hollow glass microspheres: density 0.3-0.6g / cm 3 , average diameter is 30-35μm, and compressive strength (90% retention) is 18-83MPa.
[0053] Silane coupling agent: 3-aminopropyltriethoxysilane (KH550), γ-mercaptopropyltriethoxysilane (KH580).
[0054] Base resin (high-density polyethylene): brand number is 5502s, melt index is 0.18g / 10min.
[0055] Masterbatch: Yellow masterbatch with PE carrier, the effective substance is cadmium yellow, and the effective content is 64%.
[0056] Paraffin oil: density is 0.845-0.890g / cm 3 , the distillation temperature is above 300°C.
[0057] Example 1
[0058] A lightweight extrusion blow molding product, comprising the following components in parts by weight:
[0059] 10 parts of hollow glass microspheres modified by coupling agent, 85 parts of matrix resin, 1 part of paraffin oil and 4 parts of masterbatch. The density of the hollow glass microspheres modified by coupling agent is 0.4g / cm 3 , the compressive strength (90% retention) is 42MPa.
[0060] The coupling agent-modified hollow glass microspheres are prepared by treating hollow glass microspheres with a silane coupling agent. The silane coupling agent is 3-aminopropyltriethoxysilane (KH550).
[0061] Specifically, the method for preparing the coupling agent-modified hollow glass microspheres comprises the following steps (parts are by weight):
[0062] Take hollow glass microspheres for later use, add 2 parts of silane coupling agent (3-aminopropyltriethoxysilane) to a mixture of 7.2 parts of ethanol and 0.8 parts of pure water, add acetic acid to adjust the pH to 4, hydrolyze for 5 minutes to obtain a mixed liquid, add the mixed liquid to 100 parts of hollow glass microspheres, stir evenly in a high-speed mixer, and finally dry in an oven at 60°C for 8 hours, cool and set aside to obtain hollow glass microspheres modified by coupling agent.
[0063] The method for preparing the lightweight extrusion blow molded product comprises the following steps:
[0064] S1. Mixing: Add a base resin (high-density polyethylene 5502s) and paraffin oil in a high-speed mixer and stir to make the plastic particles of the base resin fully wetted by the paraffin oil, then add the coupling agent-modified hollow glass microspheres and masterbatch, mix well, and obtain a uniformly mixed material;
[0065] S2. Blow molding: The uniformly mixed material is blow molded by an extrusion blow molding machine to obtain a lightweight extrusion blow molded product; the extrusion temperature of the blow molding machine is 160°C and the blow molding pressure is 0.5MPa.
[0066] Example 2
[0067] The difference between Example 2 and Example 1 is that the weight portion of the hollow glass microspheres modified by the coupling agent added to the lightweight extrusion blow molded product is 15 parts, and the other formulas and process conditions are the same as those in Example 1.
[0068] Example 3
[0069] The difference between Example 3 and Example 1 is that the weight proportion of the hollow glass microspheres modified by the coupling agent added to the lightweight extrusion blow molded product is 20 parts, and the other formulas and process conditions are the same as those in Example 1.
[0070] Example 4
[0071] The difference between Example 4 and Example 3 is that the density of the hollow glass microspheres modified by the coupling agent used is 0.46 g / cm 3 The compressive strength (90% retention) is 69 MPa. The silane coupling agent used is γ-mercaptopropyltriethoxysilane (KH580). Other formulas and process conditions are the same as those in Example 3.
[0072] Example 5
[0073] The difference between Example 5 and Example 1 is that the density of the hollow glass microspheres modified by the coupling agent used is 0.6 g / cm 3 , the compressive strength (90% retention) is 83 MPa, the weight portion of the hollow glass microspheres modified by the coupling agent is 20 parts, the blow molding pressure in the preparation method of the lightweight extrusion blow molding product is 0.8 MPa, and the other formulations and process conditions are the same as those in Example 1.
[0074] Comparative Example 1
[0075] Comparative Example 1 Compared with Example 1, the lightweight extrusion blow molding product of Comparative Example 1 includes the following components in parts by weight: 95 parts of base resin, 1 part of paraffin oil and 4 parts of masterbatch, and other conditions are the same.
[0076] Comparative Example 2
[0077] The difference between Comparative Example 2 and Example 1 is that the weight portion of the hollow glass microspheres modified by the coupling agent added is 8 parts, and the other formulas and process conditions are the same as those of Example 1.
[0078] Comparative Example 3
[0079] The difference between Comparative Example 3 and Example 1 is that the weight portion of the hollow glass microspheres modified by the coupling agent added is 25 parts, and the other formulas and process conditions are the same as those of Example 1.
[0080] Comparative Example 4
[0081] The difference between Comparative Example 4 and Example 3 is that the density of the hollow glass microspheres modified by the coupling agent used is 0.32 g / cm 3 The compressive strength (90% retention) is 14 MPa. Other formulations and process conditions are the same as those in Example 3.
[0082] Comparative Example 5
[0083] The difference between Comparative Example 5 and Example 3 is that the compressive strength (90% retention) of the hollow glass microspheres modified by the coupling agent used is 30 MPa, and the other formulas and process conditions are the same as those of Example 3.
[0084] Comparative Example 6
[0085] The difference between Comparative Example 6 and Example 3 is that the hollow glass microspheres used are not modified by a coupling agent, and the other formulations and process conditions are the same as those of Example 3.
[0086] The formula compositions (weight percentage, %) of the lightweight extrusion blow molded products of Examples 1-5 and Comparative Examples 1-6 are shown in Table 1 below:
[0087] Table 1 Formula composition of lightweight extrusion blow molded products of Examples 1-5 and Comparative Examples 1-6 (weight percentage, %)
[0088]
[0089] The performance tests were conducted on the lightweight extrusion blow molded products (specifically blow molded bottles) of Examples 1-5 and Comparative Examples 1-6. The test results are shown in Table 2 below:
[0090] Table 2 Performance test results of lightweight extrusion blow molding products of Examples 1-5 and Comparative Examples 1-6
[0091]
[0092]
[0093] Figure 1 The micrographs of hollow glass microspheres modified by coupling agents used in Examples 1-3 of the present invention are shown in FIG. Figure 1 It can be seen that the average diameter of the hollow glass microspheres modified by coupling agents used in Examples 1-3 is 30-35 μm, and the maximum diameter does not exceed 80 μm. The hollow glass microspheres modified by coupling agents used in Examples 4-5 and Comparative Examples 2-6 have similar sizes to those of Examples 1-3. Figure 2 The hollow blow-molded bottle prepared in Example 3 of the present invention (left) and the hollow blow-molded bottle prepared in Comparative Example 1 (right). Figure 2 The lightweight extrusion blow molded product with a capacity of 1L shown in the figure has an average thickness of 1.0-1.3 mm to ensure that the volume of the blow molded bottle body in each embodiment and the comparative example is similar. By inspecting the appearance of the bottle body, it is found that the inside and outside of the bottle body are relatively smooth, indicating that the addition of hollow glass microspheres modified by coupling agents in this size range will not make the product appearance rougher (see Figure 2 ).
[0094] The formulations of the embodiments and comparative examples are shown in Table 1, and the performance test results are shown in Table 2. Combining Table 1 and Table 2, it can be seen that compared with the case where the hollow glass microspheres are not added (Comparative Example 1), the hollow glass microspheres modified by adding 10-20 parts by weight of coupling agent in Examples 1-5 can increase the apparent density of the blow-molded bottle (blow-molded product) from 0.95 g / cm 3 Reduced to 0.80-0.85g / cm 3 . Therefore, when the thickness is similar, the weight of the bottle is reduced from about 80g to 68.3-71.8g, and the reduction rate is more than 10%. Examples 1-3 use the same hollow glass microspheres modified by coupling agents. As the content of microspheres increases, the apparent density and bottle weight decrease. Examples 4 and 5 have the same content of hollow glass microspheres modified by coupling agents as Example 3, and the density and strength are improved, but the goal of reducing weight by 10% can still be achieved. The addition of hollow glass microspheres modified by coupling agents reduces the tensile strength of the spline and the compressive strength of the bottle. The lowest strength is Example 3, whose tensile strength of the spline is 25.8MPa and the compressive strength of the bottle is 534.7N, which are 85.4% and 85.3% of that of Comparative Example 1, respectively, and both exceed 85%. This keeps the anti-drop performance of Examples 1-5 good, and no breakage or leakage occurs in the drop test.
[0095] When the amount of hollow glass microspheres modified by coupling agents is too low (Comparative Example 2), although the strength and anti-drop performance meet the standards, the weight loss is too small and does not reach 10%. When the amount of hollow glass microspheres modified by coupling agents is too high (Comparative Example 3), although the weight loss can reach more than 10%, the excessive addition of hollow glass microspheres will cause great damage to the strength, resulting in a 20% drop breakage rate. When the compressive strength (Comparative Example 5) or density (Comparative Example 4) of the hollow glass microspheres is too low, although the amount added reaches 20 parts by weight, a large part of the hollow glass microspheres modified by coupling agents will be broken during the screw shearing process, so that the weight loss of the final product does not reach 10%. Of course, when the density of the hollow glass microspheres modified by coupling agents is too high, such as exceeding 0.6g / cm 3When the density of the plastic is closer to that of the resin, its weight-reducing effect on the final product will be weakened. Figure 3 This is a SEM image of the tensile section of Example 3 of the present invention; Figure 4 This is a SEM image of the tensile cross section of Comparative Example 6 of the present invention. The hollow glass microspheres in Comparative Example 6 have not been treated with a silane coupling agent, and are poorly bonded to the resin. They are easily detached from the cross section during the stretching process, and only the resin bears the force, resulting in a flat cross section and an obvious brittle fracture state ( Figure 4 ), while the hollow glass microspheres of Example 3 are treated with silane coupling agent and have good compatibility with the matrix. Under stress, the hollow glass microspheres bear the stress together with the matrix resin, and the resin has obvious wire drawing phenomenon in the tensile section, presenting a tough fracture state ( Figure 3 ). It can be seen that the poor compatibility of hollow glass microspheres with resin and the decline in mechanical properties of the material are obviously the reasons why the strength of the product in Example 6 is greatly reduced and the drop breakage rate reaches 80%.
[0096] In general, compared with the products without the solution of the embodiment of the present invention, the apparent density of the lightweight extrusion blow molded products prepared by the solution of the embodiment of the present invention is reduced by more than 10%, the weight reduction is more than 10%, and the strength is still maintained at least 85% of the base resin product. At the same time, since the average diameter of the filler is 30-35μm and the maximum does not exceed 80μm, the surface of the product remains smooth. In addition, the solution of the present invention is versatile and can be used for the production of hollow products such as blow molding barrels, bottles, and boxes.
[0097] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can easily think of various equivalent modifications or replacements within the technical scope disclosed by the present invention, and these modifications or replacements should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be based on the protection scope of the claims.
Claims
1. A lightweight extrusion blow molded product, characterized in that: Includes hollow glass microspheres modified with a coupling agent.
2. The lightweight extrusion blow molded product according to claim 1, characterized in that: The weight portion of the coupling agent-modified hollow glass microspheres is 10-20 parts.
3. The lightweight extrusion blow molded product according to claim 2, characterized in that: The invention also comprises the following components in parts by weight: 75-85 parts of base resin, 1-2 parts of paraffin oil and 3-4 parts of masterbatch.
4. The lightweight extrusion blow molded product according to claim 1, characterized in that: The density of the hollow glass microspheres modified by the coupling agent is 0.4-0.6 g / cm 3 .
5. The lightweight extrusion blow molded product according to claim 1, characterized in that: The compressive strength of the coupling agent-modified hollow glass microspheres is greater than or equal to 42 MPa.
6. The lightweight extrusion blow molded product according to claim 1, characterized in that: The coupling agent-modified hollow glass microspheres are prepared by treating hollow glass microspheres with a silane coupling agent for modification.
7. The lightweight extrusion blow molded product according to claim 6, characterized in that: The silane coupling agent is one or more of 3-aminopropyltriethoxysilane, γ-mercaptopropyltriethoxysilane and γ-mercaptopropyltrimethoxysilane.
8. The lightweight extrusion blow molded product according to claim 1, characterized in that: The method for preparing the coupling agent-modified hollow glass microspheres comprises the following steps: Take the hollow glass microspheres for later use, add the silane coupling agent to the mixture of ethanol and pure water, add acetic acid to adjust the pH to 3-5, hydrolyze for 5-8 minutes to obtain a mixed liquid, add the mixed liquid to the hollow glass microspheres, stir evenly in a high-speed mixer, and finally dry in an oven at 60-70°C for 8-9 hours, cool and set aside, and obtain the hollow glass microspheres modified by the coupling agent.
9. The method for preparing a lightweight extrusion blow molded product according to claim 3, characterized in that: The following steps are involved: S1. Mixing: Adding a base resin and paraffin oil in a high-speed mixer and stirring so that the plastic particles of the base resin are fully wetted by the paraffin oil, and then adding the coupling agent-modified hollow glass microspheres and masterbatch, mixing evenly, to obtain a uniformly mixed material; S2. Blow molding: The evenly mixed material is blow molded through an extrusion blow molding machine to obtain a lightweight extrusion blow molded product.
10. The method for preparing a lightweight extrusion blow molded product according to claim 9, characterized in that: In step S2, the extrusion temperature of the blow molding machine is 160-180°C, and the blow molding pressure is 0.5-0.8 MPa.