Niobium-tungsten alloy for rare earth molten salt electrolytic furnace metal receiver and preparation method of niobium-tungsten alloy

By using specific components of niobium tungsten alloy and preparation process in rare earth molten salt electrolytic furnaces, the problems of high temperature resistance and insufficient processing performance of tungsten metal are solved, and the high temperature mechanical properties and processing performance are improved. It is suitable for rare earth molten salt electrolytic furnaces. Metal receiver.

CN119040716APending Publication Date: 2024-11-29BAIYIN NEW MATERIALS RES INST OF LANZHOU UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411177962.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The metal receiver materials in existing rare earth molten salt electrolytic furnaces, especially tungsten metal, have problems with insufficient resistance to high temperature and heat corrosion, which leads to the impact of the quality of rare earth metals and the reduction of the life of the electrolytic cell, and poor processing performance and difficult to form. .

Method used

Develop a niobium tungsten alloy containing specific proportions of W, Mo, Zr, C, Si, Fe and Al elements, and is subjected to vacuum sintering, vacuum electron beam smelting, vacuum consumable arc smelting, extrusion, forging, solid-dissolving Processing and aging treatment process are prepared to form a niobium tungsten alloy with excellent mechanical properties and processing properties.

Benefits of technology

It realizes excellent mechanical properties and processing performance of niobium tungsten alloy at room temperature and high temperatures, with a maximum service temperature of more than 1900℃, solving the problem of difficult processing deformation of tungsten metal receivers, and improving the quality of rare earth metals and electrolytic cell life. .

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the technical field of niobium-tungsten alloys, and provides a niobium-tungsten alloy for a rare earth molten salt electrolytic furnace metal receiver and a preparation method of the niobium-tungsten alloy. The niobium-tungsten alloy comprises the following components in percentage by mass: 6.7-7.5% of W, 2.0-2.5% of Mo, 1.0-1.5% of Zr, 0.09-0.11% of C, less than or equal to 0.05% of the total amount of Si, Fe and Al, less than or equal to 0.05% of the total amount of non-metal impurity elements and the balance of Nb. According to the method, the proportion of all the element components is reasonably controlled, vacuum electron beam melting is combined with two times of vacuum consumable electric arc melting, and the alloy cast ingot which is low in impurity element content, small and uniform in original crystal grain and good in structure property can be obtained; the alloy cast ingot is subjected to solution treatment and aging treatment after being extruded and forged, transverse and longitudinal grain structures of the cast ingot can be fully damaged, and bars, plates and the like with uniform structure components are obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of niobium-tungsten alloys, and in particular to a niobium-tungsten alloy used for a metal receiver of a rare earth molten salt electrolysis furnace and a preparation method thereof. Background Art

[0002] Rare earth materials have unique physical, chemical and magnetic properties. Among the preparation methods of rare earth metals, molten salt electrolysis is currently the main industrial method for producing single light rare earth metals, mixed rare earth metals and rare earth alloys. Among them, the cell type, distance between electrodes, current density, etc. of the electrolytic cell will affect the production efficiency and quality of rare earth metals. At present, the metal and alloy receivers used in rare earth molten salt electrolytic furnaces are mainly tungsten metal. After numerical simulation of the electric field, the current flowing through the metal receiver area is very small, which means that the electric field force of the liquid metal element leaving the cathode and entering this area is very small. The weak electric field force will not cause violent flow circulation of the melt in this area, which is conducive to its smooth sedimentation into the receiver. After numerical simulation of the temperature field, the potential gradient in the metal receiving area is smaller than that in the cathode area and has an irregular distribution state, and the current density here is lower. In actual production, due to the low temperature at the bottom of the cell, metal solidification is prone to occur, which is also the reason for the nodule phenomenon in the electrolytic cell.

[0003] Generally speaking, there should be basically no high potential area in the metal receiving area at the bottom of the electrolytic cell, that is, the potential gradient is almost unchanged, which is more conducive to the deposition and collection of rare earth metals in actual working conditions. With the increase of the anode insertion depth, the low potential area of ​​the melt decreases. The deeper the anode insertion depth, the smaller the low potential area affected by the cathode. From the perspective of potential distribution, increasing the anode insertion depth is conducive to the deposition and collection of rare earth metals. The equipotential surface distribution in the metal receiving area is sparse, and the electrolyte in this area hardly participates in the electrolysis reaction, and the temperature of the metal receiving area is the lowest. The temperature in the electrolytic cell is the highest overall, especially near the cathode, where the temperature reaches about 1630K, and the local temperature of the metal receiver is about 1250K. Excessive electrolysis temperature will lead to violent electrolysis reaction. The praseodymium and neodymium elements precipitated at the cathode are easily melted in the molten salt electrolyte, affecting the quality of rare earth metals, and easily aggravating the corrosion of the cathode and anode, resulting in a decrease in the life of the electrolytic cell. Since the metal receiver area is far away from the main area where the electrolysis reaction occurs, the temperature is relatively low and constant, but there are also differences in various areas within the metal receiver area. The side and bottom areas of the metal receiver are far away from the lower surface of the cathode rod, where the current density is low and the circulation of the electrolyte solution is weak. In this area, the praseodymium-neodymium metal is easily solidified due to the lower temperature, resulting in nodule formation in the electrolytic cell.

[0004] The melting point of pure tungsten is 3410℃, and it still has high strength at about 1300℃, while niobium tungsten alloy still has high strength at about 1800℃ and has good resistance to thermal shock. Tungsten is an effective strengthening element of niobium to maintain the high strength of the alloy and reduce the plastic-brittle transition temperature. At the same time, among refractory metals, tungsten and tungsten alloys have the highest plastic-brittle transition temperature. Tungsten has poor oxidation resistance and its oxidation characteristics are similar to those of molybdenum. Tungsten trioxide will volatilize above 1000℃, resulting in "catastrophic" oxidation. Therefore, tungsten materials must be protected under vacuum or inert atmosphere when used at high temperatures. If used in a high-temperature oxidizing atmosphere, a protective coating must be added. The high-temperature resistance and heat-corrosion resistance of the pure tungsten rare earth metal receiver currently used still have room for improvement. Some molten impurities enter the rare earth metal, which will affect the purity of the rare earth metal to a certain extent. Especially in a high-temperature carbon-containing environment, a tungsten carbide structure with better heat resistance will be formed, which will adhere to the metal receiver, affecting the use and service life of the receiver. More importantly, tungsten metal has poor processing performance and can only be prepared through casting process, resulting in poor forming ability of the prepared metal receiver.

[0005] Based on this, the development of niobium tungsten alloy suitable for metal receivers in rare earth molten salt electrolysis furnaces has better high temperature resistance and processing performance, which is of great significance. Summary of the invention

[0006] The purpose of the present invention is to provide a niobium-tungsten alloy for a metal receiver of a rare earth molten salt electrolysis furnace and a preparation method thereof in view of the deficiencies in the prior art.

[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0008] The present invention provides a niobium-tungsten alloy for a metal receiver of a rare earth molten salt electrolysis furnace. The niobium-tungsten alloy comprises the following components in mass fraction:

[0009] W 6.7~7.5%, Mo 2.0~2.5%, Zr 1.0~1.5%, C 0.09~0.11%, the total amount of Si, Fe and Al ≤0.05%, the total amount of non-metallic impurity elements ≤0.05%, and the balance is Nb.

[0010] Preferably, the non-metallic impurity elements include O, N and H.

[0011] Preferably, the niobium tungsten alloy contains the following components by mass fraction: W 7-7.2%, Mo 2.2-2.3%, Zr 1.4-1.5%, C 0.1%, the total amount of Si, Fe and Al is 0.03-0.05%, the total amount of non-metallic impurity elements is ≤0.03%, and the balance is Nb.

[0012] The present invention also provides a method for preparing the niobium-tungsten alloy for a metal receiver of a rare earth molten salt electrolysis furnace, comprising the following steps:

[0013] 1) mixing niobium powder, tungsten powder, molybdenum powder, zirconium powder and carbon powder, and sequentially performing vacuum sintering, vacuum electron beam melting and vacuum consumable arc melting to obtain an alloy ingot;

[0014] 2) The alloy ingot is sequentially subjected to extrusion, forging, solution treatment and aging treatment to obtain niobium tungsten alloy.

[0015] Preferably, the vacuum degree of the vacuum sintering in step 1) is 0.03-0.08 Pa, the temperature is 1400-1500° C., and the time is 1-2 h.

[0016] Preferably, the vacuum degree of the vacuum electron beam melting in step 1) is 0.01-0.03Pa.

[0017] Preferably, the vacuum consumable arc melting in step 1) is performed twice, the vacuum degree of the first vacuum consumable arc melting is 0.6-0.8Pa, the melting current is 4-4.5kA, and the voltage is 30-35V; the vacuum degree of the second vacuum consumable arc melting is 0.5-0.6Pa, the melting current is 5.5-6kA, and the voltage is 32-37V.

[0018] Preferably, in step 2), the extrusion temperature is 1300-1400° C. and the time is 1-2 h; the forging temperature is 1250-1300° C. and the time is 0.5-1 h.

[0019] Preferably, in step 2), the temperature of the solution treatment is 1270-1330° C., and the time is 1.5-2.5 h; the temperature of the aging treatment is 1030-1080° C., and the time is 7-9 h.

[0020] The beneficial effects of the present invention include:

[0021] The present invention reasonably controls the proportion of each element and adopts vacuum electron beam melting combined with two vacuum consumable arc melting to obtain a niobium tungsten alloy ingot with low impurity element content, small and uniform original grains, and good organizational properties; the alloy ingot is subjected to solid solution treatment and aging treatment after extrusion and forging, which can fully destroy the transverse and longitudinal grain structure of the ingot to obtain rods, plates, etc. with uniform organizational composition. The niobium tungsten alloy of the present invention is used for metal receivers of rare earth molten salt electrolysis furnaces, and has excellent mechanical properties and processing properties at room temperature and high temperatures, and the maximum operating temperature is above 1900°C. The niobium tungsten alloy of the present invention has low tensile strength at room temperature, good plasticity and toughness, can be formed by plastic processing methods such as forging and upsetting, has good plasticity and deep processing performance at room temperature, and has high strength at high temperatures, which solves the problem of difficult processing and deformation of tungsten metal receivers. DETAILED DESCRIPTION

[0022] The present invention provides a niobium-tungsten alloy for a metal receiver of a rare earth molten salt electrolysis furnace. The niobium-tungsten alloy comprises the following components in mass fraction:

[0023] W 6.7~7.5%, Mo 2.0~2.5%, Zr 1.0~1.5%, C 0.09~0.11%, the total amount of Si, Fe and Al ≤0.05%, the total amount of non-metallic impurity elements ≤0.05%, and the balance is Nb.

[0024] In the present invention, the non-metallic impurity elements preferably include O, N and H.

[0025] The mass fraction of W in the niobium tungsten alloy of the present invention is 6.7-7.5%, preferably 6.8-7.3%, and more preferably 7-7.2%; the mass fraction of Mo is 2.0-2.5%, preferably 2.1-2.4%, and more preferably 2.2-2.3%; the mass fraction of Zr is 1.0-1.5%, preferably 1.2-1.5%, and more preferably 1.4-1.5%; the mass fraction of C is 0.09-0.11%, preferably 0.1%, the total amount of Si, Fe and Al is preferably ≤0.05%, more preferably 0.03-0.05%, and more preferably 0.03-0.04%; the total amount of non-metallic impurity elements is preferably ≤0.05%, and more preferably ≤0.03%, and the balance is Nb.

[0026] Adding tungsten, molybdenum and zirconium to the niobium matrix will form a variety of solid solution strengthening phases and precipitation strengthening phases with niobium, improving the room temperature and high temperature mechanical properties of the alloy. After adding tungsten and molybdenum to the alloy, due to the high melting point of these two elements and the close atomic radius to niobium, it is easy to form a substitution solid solution, thereby improving the high temperature strength and creep properties of the niobium matrix. The addition of molybdenum can improve the high temperature strength and hot corrosion resistance of the alloy, and moderately improve the mechanical properties such as toughness of the alloy. Adding zirconium plays a precipitation strengthening role, has a significant deoxidation, denitrification and desulfurization effect, reduces the content of non-metallic elements in the alloy, purifies the alloy, and further improves the matrix strength of the alloy. Al has a strong affinity with oxygen and nitrogen, and can be used as a deoxidation and nitrogen fixation agent for alloy smelting; at the same time, aluminum can significantly reduce the austenite phase area and improve the uniformity of the alloy structure. Si can form compounds with carbon, molybdenum and other elements in the alloy, making the alloy lattice structure more compact, thereby improving the strength and hardness of the alloy; at the same time, Si can also improve the wear resistance and fatigue resistance of the alloy and extend the service life of the alloy. The Fe element can improve the wear resistance and thermal stability of the alloy.

[0027] The present invention also provides a method for preparing the niobium-tungsten alloy for a metal receiver of a rare earth molten salt electrolysis furnace, comprising the following steps:

[0028] 1) mixing niobium powder, tungsten powder, molybdenum powder, zirconium powder and carbon powder, and sequentially performing vacuum sintering, vacuum electron beam melting and vacuum consumable arc melting to obtain an alloy ingot;

[0029] 2) The alloy ingot is sequentially subjected to extrusion, forging, solution treatment and aging treatment to obtain niobium tungsten alloy.

[0030] In the present invention, the vacuum degree of the vacuum sintering in step 1) is preferably 0.03-0.08 Pa, more preferably 0.04-0.07 Pa, and more preferably 0.05-0.06 Pa; the temperature of the vacuum sintering is preferably 1400-1500°C, more preferably 1420-1480°C, and more preferably 1440-1450°C; the time of the vacuum sintering is preferably 1-2 h, and more preferably 1.5 h.

[0031] In the present invention, the vacuum degree of the vacuum electron beam melting in step 1) is preferably 0.01-0.03Pa, and more preferably 0.02Pa.

[0032] In the present invention, the number of vacuum consumable arc melting in step 1) is preferably twice, the vacuum degree of the first vacuum consumable arc melting is preferably 0.6-0.8Pa, more preferably 0.65-0.75Pa, more preferably 0.7Pa; the melting current is preferably 4-4.5kA, more preferably 4.1-4.4kA, more preferably 4.2-4.3kA, and the voltage is preferably 30-35V, more preferably 31-34V, more preferably 32-33V; the vacuum degree of the second vacuum consumable arc melting is preferably 0.5-0.6Pa, more preferably 0.52-0.58Pa, more preferably 0.54-0.55Pa; the melting current is preferably 5.5-6kA, more preferably 5.6-5.9kA, more preferably 5.7-5.8kA, and the voltage is preferably 32-37V, more preferably 33-36V, more preferably 34-35V.

[0033] In the present invention, vacuum electron beam melting can fully remove metallic impurity elements and non-metallic impurity elements in the alloy under high vacuum, and the purification effect is good; however, due to the solid solubility of niobium in zirconium and the difference in density between zirconium and niobium, the use of a single electron beam melting method results in coarse grain structure of the ingot, and poor uniformity and performance of the alloy structure; vacuum electron beam melting purification combined with vacuum consumable arc melting to enlarge the ingot, the ingot has good grain size and uniformity, and is easy to prepare niobium tungsten alloy with uniform structure and performance.

[0034] In the present invention, the extrusion temperature in step 2) is preferably 1300-1400°C, more preferably 1320-1380°C, and more preferably 1340-1350°C; the extrusion time is preferably 1-2h, and more preferably 1.5h; the forging temperature is preferably 1250-1300°C, more preferably 1260-1290°C, and more preferably 1270-1280°C, and the forging time is preferably 0.5-1h, and more preferably 0.7-0.8h.

[0035] The purpose of alloy ingot extrusion is to fill the tiny pores in the ingot, refine and homogenize the grain structure, and improve the mechanical properties of the ingot; extrusion can obtain a billet with good surface quality and uniform transverse structure. During forging, the metal plastically deforms in a direction perpendicular to the axial direction, and the grain boundaries are repeatedly bent, resulting in a large number of nucleation zones, which can further refine the longitudinal structure.

[0036] In the present invention, the temperature of the solution treatment in step 2) is preferably 1270-1330°C, more preferably 1280-1320°C, and more preferably 1300°C; the time of the solution treatment is preferably 1.5-2.5h, and more preferably 2h; the temperature of the aging treatment is preferably 1030-1080°C, more preferably 1040-1070°C, and more preferably 1050-1060°C; the time of the aging treatment is preferably 7-9h, and more preferably 8h.

[0037] In the present invention, the forged alloy is subjected to solution treatment and aging treatment, so as to eliminate ingot segregation, refine grains, improve organizational uniformity, and reduce coarse grains and brittle cracking.

[0038] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0039] Example 1

[0040] Tungsten powder, molybdenum powder, zirconium powder, carbon powder and niobium powder with mass fractions of 6.8% respectively, are mixed evenly, and the uniform mixture is vacuum sintered at 0.04Pa and 1420℃ for 2h. The sintered product is vacuum electron beam melted at 0.01Pa to obtain a primary ingot with a diameter of 40mm. The primary ingot is subjected to vacuum consumable arc melting twice, the vacuum degree of the first vacuum consumable arc melting is 0.65Pa, the melting current is 4.5kA, and the voltage is 35V to obtain an ingot with a diameter of 50mm. The vacuum degree of the second vacuum consumable arc melting is 0.52Pa, the melting current is 6kA, and the voltage is 37V to obtain an alloy ingot with a diameter of 60mm. After each vacuum consumable arc melting, the foreign matter on the surface of the ingot after melting is treated with an ingot cleaning machine and dried.

[0041] The alloy ingots were extruded and forged in sequence, with the extrusion temperature being 1320°C for 2 hours, the forging temperature being 1250°C for 1 hour; the forged product was solution treated at 1280°C for 2.5 hours, and then aged at 1030°C for 9 hours to obtain niobium tungsten alloy rods with a diameter of 55 mm and a length of 100 mm.

[0042] The mass fractions of the components in the niobium tungsten alloy obtained in this embodiment are: W 6.78%, Mo 2.1%, Zr 1.05%, C 0.09%, Nb 89.91%, Si 0.02%, Fe 0.01%, and the total amount of non-metallic impurity elements O, H, and N is 0.04%.

[0043] Example 2

[0044] Tungsten powder, molybdenum powder, zirconium powder, carbon powder and niobium powder with mass fractions of 7.3%, 2.5%, 1.5%, 0.11% and 88.59% respectively are mixed uniformly, and the uniform mixture is vacuum sintered at 0.07Pa and 1480℃ for 1h. The sintered product is vacuum electron beam melted at 0.03Pa to obtain a primary ingot with a diameter of 40mm. The primary ingot is subjected to vacuum consumable arc melting twice, the vacuum degree of the first vacuum consumable arc melting is 0.75Pa, the melting current is 4kA, and the voltage is 30V to obtain an ingot with a diameter of 50mm, and the vacuum degree of the second vacuum consumable arc melting is 0.58Pa, the melting current is 5.5kA, and the voltage is 32V to obtain an alloy ingot with a diameter of 60mm. After each vacuum consumable arc melting, the foreign matter on the surface of the ingot after melting is treated with an ingot cleaning machine and dried.

[0045] The alloy ingots were extruded and forged in sequence, with the extrusion temperature being 1380°C for 1 hour, the forging temperature being 1300°C for 0.5 hour; the forged product was solution treated at 1320°C for 1.5 hours, and then aged at 1080°C for 7 hours to obtain niobium tungsten alloy rods with a diameter of 54 mm and a length of 95 mm.

[0046] The mass fractions of the components in the niobium tungsten alloy obtained in this embodiment are: W 7.28%, Mo 2.48%, Zr 1.5%, C 0.11%, Nb 88.57%, Si 0.01%, Fe 0.01%, Al 0.01%, and the total amount of non-metallic impurity elements O, H, and N is 0.03%.

[0047] Example 3

[0048] 7% tungsten powder, 2.3% molybdenum powder, 1.3% zirconium powder, 0.1% carbon powder and 89.3% niobium powder with mass fractions are mixed uniformly, the uniform mixture is vacuum sintered at 0.05Pa and 1450℃ for 1.5h, the sintered product is vacuum electron beam melted at 0.02Pa to obtain a primary ingot with a diameter of 40mm; the primary ingot is subjected to vacuum consumable arc melting twice, the vacuum degree of the first vacuum consumable arc melting is 0.7Pa, the melting current is 4.3kA, the voltage is 33V, and an ingot with a diameter of 50mm is obtained; the vacuum degree of the second vacuum consumable arc melting is 0.55Pa, the melting current is 5.7kA, the voltage is 35V, and an alloy ingot with a diameter of 60mm is obtained; after each vacuum consumable arc melting, the foreign matter on the surface of the ingot after melting is treated with an ingot cleaning machine and dried.

[0049] The alloy ingots were extruded and forged in sequence, with the extrusion temperature being 1350°C for 1.5 h, the forging temperature being 1280°C for 0.8 h; the forged product was solution treated at 1300°C for 2 h, and then aged at 1050°C for 8 h to obtain niobium tungsten alloy rods with a diameter of 55 mm and a length of 95 mm.

[0050] The mass fractions of the components in the niobium tungsten alloy obtained in this embodiment are: W 6.99%, Mo 2.28%, Zr 1.3%, C 0.1%, Nb 89.26%, Si 0.02%, Fe 0.02%, and the total amount of non-metallic impurity elements O, H, and N is 0.03%.

[0051] Comparative Example 1

[0052] The vacuum electron beam melting, forging and solution treatment of Example 3 are omitted, and other conditions are the same as those of Example 3.

[0053] Comparative Example 2

[0054] The second vacuum consumable arc melting and aging treatment in Example 3 were omitted, the mass fraction of tungsten powder was changed to 5%, the mass fraction of niobium powder was changed to 87.3%, and other conditions were the same as in Example 3.

[0055] The niobium tungsten alloy rods of Examples 1 to 3 and Comparative Examples 1 to 2 were tested for performance at room temperature and high temperature. The niobium tungsten alloy rod of Example 1 had a tensile strength of 380 MPa, a yield strength of 260 MPa, an elongation of 22%, a hardness of HBW136, a tensile strength of 68 MPa at 1800°C, and an elongation of 25% at room temperature; the niobium tungsten alloy rod of Example 2 had a tensile strength of 388 MPa, a yield strength of 269 MPa, an elongation of 25%, a hardness of HBW134, a tensile strength of 70 MPa at 1800°C, and an elongation of 27%; the niobium tungsten alloy rod of Example 3 had a tensile strength of 375 MPa, a yield strength of 258 MPa, an elongation of 28%, a hardness of HBW130, a tensile strength of 73 MPa at 1800°C, and an elongation of 30%. The niobium tungsten alloy rod of Comparative Example 1 has a tensile strength of 330 MPa at room temperature and an elongation of 15%, a tensile strength of 50 MPa at 1800°C and an elongation of 17%; the niobium tungsten alloy rod of Comparative Example 2 has a tensile strength of 337 MPa at room temperature and an elongation of 18%, a tensile strength of 53 MPa at 1800°C and an elongation of 20%.

[0056] The present invention reasonably controls the proportion of each element and adopts vacuum electron beam melting combined with two vacuum consumable arc melting to obtain a niobium tungsten alloy ingot with low impurity element content, small and uniform original grains, and good organizational properties; the alloy ingot is subjected to solution treatment and aging treatment after extrusion and forging, which can fully destroy the transverse and longitudinal grain structure of the ingot to obtain rods, plates, etc. with uniform organizational composition. The niobium tungsten alloy of the present invention is used for the metal receiver of the rare earth molten salt electrolysis furnace, and has excellent mechanical properties and processing properties at room temperature and high temperature, and the maximum operating temperature is above 1900°C. It can be seen from the embodiments and comparative examples that the present invention improves the room temperature and high temperature performance of the niobium tungsten alloy by reasonably controlling the proportion of each element and combining specific process steps.

[0057] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A niobium-tungsten alloy for a metal receiver of a rare earth molten salt electrolysis furnace, characterized in that: Niobium tungsten alloy contains the following components by mass fraction: W 6.7~7.5%, Mo 2.0~2.5%, Zr 1.0~1.5%, C 0.09~0.11%, the total amount of Si, Fe and Al ≤0.05%, the total amount of non-metallic impurity elements ≤0.05%, and the balance is Nb.

2. The niobium-tungsten alloy according to claim 1, characterized in that: Non-metallic impurity elements include O, N and H.

3. The niobium-tungsten alloy according to claim 1 or 2, characterized in that: Niobium tungsten alloy contains the following components by mass fraction: W 7~7.2%, Mo 2.2~2.3%, Zr 1.4~1.5%, C 0.1%, the total amount of Si, Fe and Al is 0.03~0.05%, the total amount of non-metallic impurity elements is ≤0.03%, and the balance is Nb.

4. The method for preparing the niobium-tungsten alloy for the metal receiver of the rare earth molten salt electrolysis furnace according to any one of claims 1 to 3, characterized in that: The following steps are included: 1) mixing niobium powder, tungsten powder, molybdenum powder, zirconium powder and carbon powder, and sequentially performing vacuum sintering, vacuum electron beam melting and vacuum consumable arc melting to obtain an alloy ingot; 2) The alloy ingot is sequentially subjected to extrusion, forging, solution treatment and aging treatment to obtain niobium tungsten alloy.

5. The preparation method according to claim 4, characterized in that: Step 1) The vacuum degree of the vacuum sintering is 0.03-0.08 Pa, the temperature is 1400-1500° C., and the time is 1-2 hours.

6. The preparation method according to claim 4 or 5, characterized in that: The vacuum degree of the vacuum electron beam melting in step 1) is 0.01-0.03Pa.

7. The preparation method according to claim 4, characterized in that: Step 1) The vacuum consumable arc melting is performed twice, the vacuum degree of the first vacuum consumable arc melting is 0.6-0.8 Pa, the melting current is 4-4.5 kA, and the voltage is 30-35 V; the vacuum degree of the second vacuum consumable arc melting is 0.5-0.6 Pa, the melting current is 5.5-6 kA, and the voltage is 32-37 V.

8. The preparation method according to claim 4 or 7, characterized in that: Step 2) The extrusion temperature is 1300-1400°C for 1-2 hours; the forging temperature is 1250-1300°C for 0.5-1 hour.

9. The preparation method according to claim 8, characterized in that: Step 2) The temperature of the solution treatment is 1270-1330°C, and the time is 1.5-2.5h; the temperature of the aging treatment is 1030-1080°C, and the time is 7-9h.