Reactive rapid-hardening high-strength recycled asphalt cold patch material as well as preparation method and application thereof
By combining the recovered milling material with ore powder and reactive adhesive mother liquor, a reactive fast-condensing high-strength regenerated asphalt cold feed with high stability and water stability was prepared, and the aging and utilization of asphalt materials in the prior art were solved. The problem of low rate has achieved efficient road surface material recycling and harsh environment adaptability.
Patent Information
- Application Number
- CN202411373177.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-29
- Publication Date
- 2024-12-24
- Estimated Expiration
- 2044-09-29
AI Technical Summary
Among the existing asphalt pavement recycling technology, the factory mixing and heat regeneration technology leads to aging of asphalt materials, reducing the reuse rate of old road materials, and the utilization rate of waste asphalt mixture is low, making it difficult to adapt to harsh repairing operating environments.
Reactive fast-condensing high-strength regenerated asphalt cold feed is used to combine the recycled milling material with ore powder and reactive adhesive mother liquor to prepare materials with high stability and water stability, and restore them with light oil and lubricants. Asphalt performance, achieves 100% recycling of milling materials.
Improve the stability and recycling rate of asphalt materials, and are suitable for harsh environments such as high altitude, large temperature difference, low temperature rain and snow weather, and pit water accumulation, alleviate the problems of solid waste accumulation and shortage of high-quality stone resources, and significantly improve the economy. benefit.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of road surface layer reuse, and in particular to a reactive quick-setting high-strength recycled asphalt cold patch material, a preparation method and an application thereof. Background Art
[0002] The reduction and resource utilization of solid waste has always been a difficult problem that has troubled governments and researchers around the world. In a circular economy, materials circulate in the economy for as long as possible at the highest value, which is achieved through upgrading, reuse, recycling and manufacturing.
[0003] The recycling of asphalt pavement is a common practice at home and abroad, and a complete set of asphalt recycling technology has been formed, reaching the level of normalization and standardization. However, when the factory-mixed hot recycling technology is currently used to recycle asphalt, the secondary high-temperature heating and mixing of the mixture (150-170°C) will cause the asphalt material to age again, reducing the reuse rate of old road materials. In addition, the test roads for recycling waste asphalt mixtures to different degrees are only used as waste materials, generally only for light traffic roads, sidewalks or road cushions, occupying and wasting limited high-quality stone and asphalt resources, and the economic benefits are poor.
[0004] Based on the above-mentioned existing technologies, there are technical problems that need to be solved urgently, such as low utilization rate and poor utilization effect of waste asphalt mixtures, poor performance of cold patch materials prepared after recycling, and difficulty in adapting to harsh repair working environments such as high altitudes, large temperature differences, low temperature rain and snow weather, and water accumulation in potholes. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a reactive quick-setting high-strength recycled asphalt cold patch material, wherein the cold patch material is prepared with recycled milling material as aggregate, mineral powder and reactive adhesive mother liquid; By weight, the components and proportions of the reactive quick-setting high-strength recycled asphalt cold patch material are as follows: Recycled milling material as aggregate: 90-96%; Mineral powder: 4-7%; Reactive adhesive masterbatch: 3-6%; The stability of the reactive quick-setting high-strength recycled asphalt cold patch material is 28.6-31.2 kN, and the dynamic stability is 10000-12000 times•mm -1 , the low temperature strain is 2401-3015με, the freeze-thaw strength ratio is 84-89%, and the flying loss is 4.8-7.2%.
[0006] Furthermore, the recycled milling material is asphalt pavement surface milling material.
[0007] Furthermore, the recycled milling material includes one or more of old asphalt and old aggregate.
[0008] Furthermore, the old asphalt includes one or more of road petroleum asphalt and modified asphalt; The old aggregate includes one or more of basalt crushed stone, diabase crushed stone and limestone crushed stone.
[0009] Furthermore, the recycled milling materials are divided into three types: particle sizes of 0-5mm, 5-10mm, and 10-15mm.
[0010] Furthermore, the moisture content of the recovered milling material is less than or equal to 0.5%.
[0011] Furthermore, the recycled milling material is recycled and pretreated according to the T0727 method in JTGE20-2011 "Test Procedures for Asphalt and Asphalt Mixtures in Highway Engineering" to separate the old asphalt and old aggregate in the recycled asphalt mixture (RAP material).
[0012] Furthermore, the needle penetration of the old asphalt is 24-25 0.1 mm, the softening point is 55-60°C, the elongation at 5°C is 8-9 cm, and the viscosity at 135°C is 2.5-3.5 Pa•s.
[0013] Furthermore, the mineral powder is obtained by grinding limestone or strong basic rock.
[0014] Furthermore, the reactive adhesive mother solution is prepared from liquid polyester polyol, diisocyanate, chain extender crosslinking agent, tackifying resin, defoamer and regeneration liquid.
[0015] Furthermore, the components and proportions of the reactive adhesive master solution are as follows: Liquid polyester polyol: 30-50%; Diisocyanate: 10-40%; Chain extender crosslinker: 1-3%; Tackifying resin: 3-6%; Defoaming agent: 1-2%; The mass of the regeneration fluid is 8-15% of the old asphalt in the recovered milling material.
[0016] Furthermore, the liquid polyester polyol is a polymer formed by polycondensation of one or more combinations of polyoxypropylene glycol, polyoxyethylene glycol, polytetrahydrofuran diol, 4-cyclohexanedicarboxylic acid-3methyl-1,5-pentanediol, and ester diol.
[0017] Furthermore, the molecular weight of the liquid polyester polyol is 2000-7000.
[0018] Furthermore, the diisocyanate is one or more of diphenylmethane diisocyanate, 1,5-naphthalene diisocyanate, polymethylene polyphenyl polyisocyanate, 1,6-diisocyanato, hexamethylene diisocyanate, isophorone diisocyanate, and 3,3'-dimethyldiphenylmethane-4,4' diisocyanate.
[0019] Furthermore, the chain extending cross-linking agent is one or more of diethylene glycol, neopentyl glycol, 1,4-butanediol, and 2-hydroxypropyl 2-acrylate.
[0020] Furthermore, the tackifying resin is one or more of terpene phenol resin, petroleum resin C5 or its hydrogenated product, rosin glycerol ester, and polyvinyl acetate.
[0021] Furthermore, the defoaming agent is one or more of an organic silicon defoaming agent, an organic fluorine defoaming agent, a non-silicon defoaming agent, and a mineral oil defoaming agent.
[0022] Furthermore, the regeneration liquid is a composite solvent obtained by mixing light oil, lubricant and stabilizer.
[0023] Furthermore, the components and proportions of the regeneration solution are as follows: Light oil: 80-100%; Lubricant: 30-50%; Stabilizer: 2-5%.
[0024] Furthermore, the light oil is one or more of cycloparaffinic oil and dearomatized alkane solvent oil.
[0025] Furthermore, the lubricant is 6-hexanediol diglycidyl ether.
[0026] Furthermore, the stabilizer is one or more of lauric acid, dianhydride, and caprylic acid.
[0027] The present invention also provides a method for preparing a reactive quick-setting high-strength recycled asphalt cold patch material, comprising the following steps: Step 1: Get the recycled milling material: Step 2, preparing a reactive adhesive mother solution; Step 3: stir the milling material recovered in step 1, the reactive adhesive mother liquor in step 2 and the mineral powder at a speed of 40-60 r / min for 60-70 s to prepare a reactive quick-setting high-strength recycled asphalt cold patch material.
[0028] Furthermore, in step 1, the milling material is crushed into fine particles with a maximum nominal particle size of 19.5 mm, and then sieved to separate the milling material into three types: 0-5 mm, 5-10 mm, and 10-15 mm.
[0029] Furthermore, the method for preparing the reactive adhesive mother solution in step 2 comprises the following steps: Step 2-1, polyol dehydration: weigh each component by mass, add liquid polyester polyol and regeneration liquid into the reaction kettle and stir to mix, heat to 120-130°C with a temperature-controlled heating jacket, use a vacuum pump to reduce the system pressure by 0.67±0.03Kpa to evacuate and dehydrate for 2-3h, cool to 60-70°C and wait for use; Step 2-2, preparation of prepolymer: adding the melted diisocyanate into a reaction kettle, slowly heating to 120-130° C., stirring at a speed of 400-600 r / min under a nitrogen atmosphere for 1-2 h to obtain a prepolymer; Step 2-3, synthesizing mother liquor: add chain extender crosslinking agent, tackifying resin and defoaming agent to the prepolymer in sequence, keep stirring at high speed under vacuum conditions for 2-3 hours, cool to 70-80°C and then quickly discharge and package in an aluminum foil bag to obtain a reactive adhesive mother liquor.
[0030] A curing material is obtained by curing the above-mentioned reactive quick-setting high-strength recycled asphalt cold patch material.
[0031] Furthermore, the Marshall stability of the solidified material at 1d age is greater than 30kN, which is 8-10 times that of traditional cold patch materials; the dynamic stability index is ≥6000 times / mm, the high temperature stability is significantly better than that of hot mix asphalt mixture, the residual stability is ≥85%, the freeze-thaw splitting strength ratio is ≥80%, and the water stability is excellent.
[0032] The beneficial effects of the present invention are: 1. The main polymer of the reactive adhesive mother solution in the present invention is an isocyanate-terminated prepolymer synthesized from a liquid polyester polyol and an isocyanate, which can realize the transformation from a thermoplastic binder to a thermosetting binder. The occurrence process is mainly divided into initial curing and final curing. The initial curing is a physical process, which will undergo crystallization, solvent volatilization, and preliminary cross-linking of the adhesive polymer, mainly involving adsorption and diffusion theory; the final curing is a chemical process, involving chemical bond bonding, and the -NCO at the end of the active terminal molecular chain is cured and cross-linked with active hydrogen such as water adsorbed on the surface of the substrate and water (-OH) in the air to generate a urea bond structure. At this time, the polymer contains a large number of carbamic acid groups (-NH-COO-), which makes the material properties stable, does not have the ability to flow and deform after heating, cannot be softened and repeatedly molded, and cannot be dissolved in a solvent, and the curing process is completely completed; 2. In the present invention, light oil, lubricant and stabilizer are used as composite regeneration components to restore and strengthen the attenuation performance of the recycled milling material. One or two of cycloparaffinic oil, dearomatized alkane solvent oil and styrene-butadiene block copolymer are mixed in any proportion as light oil, which is a good asphalt regeneration material. It can soften and adjust the problem of material hardening and brittleness caused by serious loss of saturated components during asphalt aging, and adjust the migration change ratio of the four components of asphalt; 6-hexanediol diglycidyl ether is used as a lubricant to reduce the macromolecular polymers of old asphalt to small molecular compounds. When asphalt is acted upon by light and oxygen, the unsaturated functional groups are unstable during the aging process, and are prone to oxidation, dehydrogenation, condensation, addition, cross-linking and other reactions to produce carbon-based, sulfoxide-based and other macromolecular polymers. The lubricant component can degrade and reduce them to olefin compounds, further restoring the elasticity and low-temperature ductility of asphalt; 3. Combining the room temperature regeneration technology with the reactive cold patch material technology, the recycled milling material is used as aggregate, achieving 100% recycling of road milling materials, alleviating the dual problems of solid waste accumulation and shortage of high-quality stone resources, and solving the problem that RAP materials were previously only used for light traffic and downgrading and downgrading of the middle and lower layers; at the same time, the fatal disadvantage of traditional diluted cold patch materials is poor water resistance. Even with the addition of anti-stripping agents and other polymer materials, it is difficult to resist the damage of water to the oil film; the reactive fast-setting high-strength recycled asphalt cold patch material prepared by the present invention uses water as an activator to promote the chemical gel curing of the binder, turning the disadvantages of traditional cold patch materials into advantages, and can be better applied to harsh repair work environments such as high altitude, large temperature difference, low temperature rain and snow weather, and water accumulation in potholes; 4. Compared with the traditional cold patching technology, in order to ensure the workability of the mixture and reserve pores for the volatilization of the solvent in the later stage, the grading of the mineral material is mainly based on single-size aggregate, the amount of machine-made sand powder is small, the void ratio of the final mixture is large, and the density is difficult to ensure; the present invention has developed a grading of cold patching special recycled mixture with extremely low porosity and low compaction work requirements, and the grading pass rate range is as follows: 16mm sieve pass rate 100%, 13.2mm sieve pass rate 90-100%, 9.5mm sieve pass rate 68-82%, 4.75mm sieve pass rate 38-55%, 4.75mm sieve pass rate 21-32%, 2.36mm sieve pass rate 15-23%, 0.6mm sieve pass rate 12-19%, 0.3mm sieve pass rate 9-14%, 0.15mm sieve pass rate 8-13%, 0.075 sieve pass rate 8-12%; 5. The strength of the present invention is improved through a chemical curing process with a fast reaction speed. The initial strength can be quickly formed within 10 minutes to achieve surface hardening. And with a special dense gradation, after complete curing, the Marshall stability of the mixture (1d age) is greater than 30kN, which is 8-10 times that of traditional cold patch materials; the dynamic stability index is ≥6000 times / mm, the high temperature stability is significantly better than that of hot mix asphalt mixture, the residual stability is ≥85%, the freeze-thaw splitting strength ratio is ≥80%, and the water stability is excellent. DETAILED DESCRIPTION
[0033] The milling materials recovered in the following examples are from the asphalt mixture of the middle surface layer of the Shanxi secondary highway. Example 1
[0034] This embodiment provides a reactive quick-setting high-strength recycled asphalt cold patch material, which is prepared with recycled milling material as aggregate, mineral powder and reactive adhesive mother liquid; By weight, the components and proportions of the reactive quick-setting high-strength recycled asphalt cold patch material are as follows: Recycled milling material as aggregate: 96%; Mineral powder: 7%; Reactive adhesive mother solution: 3.311%; The stability of the reactive quick-setting high-strength recycled asphalt cold patch material is 31.2 kN, and the dynamic stability is 11000 times•mm -1 , the low temperature strain is 2741με, the freeze-thaw strength ratio is 87%, and the flying loss is 5.4%.
[0035] The recycled milling material is asphalt pavement surface milling material, including old asphalt and old aggregate.
[0036] The recycled milling materials are divided into three types: particle sizes of 0-5mm, 5-10mm, and 10-15mm, and the moisture content is less than or equal to 0.5%.
[0037] In this embodiment, the recycled milling material is recycled and pretreated according to the T0727 method in JTGE20-2011 "Test Procedures for Asphalt and Asphalt Mixtures in Highway Engineering" to separate the old asphalt and old aggregate in the recycled asphalt mixture (RAP material).
[0038] The oil-to-stone ratio in RAP was calculated to be 2.2%, and the performance of the old asphalt was tested. The test results are shown in Table 1 below.
[0039] Table 1 Performance indexes of old asphalt in RAP
[0040] The dense EA-13 gradation specially used for road pothole repair was used as the target mix ratio. The milling material was graded and screened to determine the gradation of the mineral material to be 10-15mm: 5-10mm: 0-5mm: mineral powder = 21:40:32:7. The oil-stone ratio was determined to be 5.6% through the Marshall test. The mineral material gradation table is shown in Table 2 below.
[0041] Table 2 Grading of reactive quick-setting high-strength recycled asphalt cold patch material
[0042] In this embodiment, the mineral powder is the mineral powder obtained by grinding limestone.
[0043] In this embodiment, the reactive adhesive mother solution is prepared from liquid polyester polyol, diisocyanate, chain extender cross-linking agent, tackifier resin, defoamer, and regeneration liquid.
[0044] By weight, the components and proportions for preparing the reactive adhesive mother solution are as follows: Liquid polyester polyol, polyoxypropylene glycol: 40%; Diisocyanate, diphenylmethane diisocyanate: 30%; Chain extender, diethylene glycol: 2%; Tackifying resin, which is terpene phenol resin: 5%; Defoaming agent, which is a silicone defoaming agent: 1%; The mass of the regeneration fluid is 9% of the old asphalt in the recovered milling material.
[0045] According to the dense gradation as the target mix ratio, the gradation design is carried out to determine the amount of each grade of material, and the mixed milling material is prepared. The amount of reactive adhesive mother liquid is determined by Marshall test. In this embodiment, according to the above-determined mineral grading of 10-15mm: 5-10mm: 0-5mm: mineral powder = 21: 40: 32: 7, the oil-stone ratio is 5.6%. The oil-stone ratio in the RAP material was tested to be 2.2%, and the penetration of the aged asphalt after extraction treatment was 24.6dmm. The test showed that the aged asphalt of the RAP material was added with regeneration liquid at a ratio of 9%, which can better restore and improve the attenuation performance of the aged asphalt. Therefore, the proportion of aged asphalt is 96×2.2%=2.1%, and the corresponding regeneration liquid ratio is 2.1%×9%=0.189%, and the addition ratio of the reactive adhesive mother liquid is 5.6-2.1-0.189=3.311%.
[0046] In this embodiment, the regeneration liquid is a composite solvent obtained by mixing light oil, lubricant and stabilizer.
[0047] In terms of weight, the components and proportions for preparing the regeneration solution are as follows: Light oil, naphthenic oil: 90%; Lubricant, 6-hexanediol diglycidyl ether: 50%; Stabilizer, lauric acid: 3%.
[0048] In this embodiment, the preparation method of the above-mentioned reactive quick-setting high-strength recycled asphalt cold patch material comprises the following steps: Step 1: Get the recycled milling material, crush it into fine particles with a maximum nominal particle size of 19.5 mm, and then screen it to divide it into three types: 0-5 mm, 5-10 mm, and 10-15 mm: Step 2, preparing a reactive adhesive mother solution, specifically comprising the following steps: Step 2-1, polyol dehydration: weigh each component by mass, add liquid polyester polyol and regeneration liquid into the reaction kettle and stir to mix, heat to 120°C with a temperature-controlled heating jacket, use a vacuum pump to reduce the system pressure by 0.67±0.03Kpa to evacuate and dehydrate for 2h, cool to 70°C and wait for use; Step 2-2, preparation of prepolymer: adding the melted diisocyanate into a reaction kettle, slowly heating to 125° C., stirring at a speed of 400 r / min under a nitrogen atmosphere for 1 h to obtain a prepolymer; Step 2-3, synthesizing mother liquor: add chain extender, crosslinking agent, tackifying resin and defoaming agent to the prepolymer in sequence, keep stirring at high speed for 2 hours under vacuum, cool to 80°C, quickly discharge and package in aluminum foil bag to obtain reactive adhesive mother liquor; Step 3: stir the milling material recovered in step 1, the reactive adhesive mother liquor in step 2 and the mineral powder at a speed of 40 r / min for 60 seconds to prepare a reactive quick-setting high-strength recycled asphalt cold patch material. Example 2
[0049] This embodiment provides a reactive quick-setting high-strength recycled asphalt cold patch material, which is prepared with recycled milling material as aggregate, mineral powder and reactive adhesive mother liquid; By weight, the components and proportions of the reactive quick-setting high-strength recycled asphalt cold patch material are as follows: Recycled milling material as aggregate: 94%; Mineral powder: 7%; Reactive adhesive mother liquor: 3.348%; The stability of the reactive quick-setting high-strength recycled asphalt cold patch material is 28.6 kN, and the dynamic stability is 12000 times•mm -1 , the low temperature strain is 3015με, the freeze-thaw strength ratio is 85%, and the flying loss is 6.1%.
[0050] The recycled milling material is asphalt pavement surface milling material, including old asphalt and old aggregate.
[0051] The recycled milling materials are divided into three types: particle sizes of 0-5mm, 5-10mm, and 10-15mm, and the moisture content is less than or equal to 0.5%.
[0052] In this embodiment, the recycled milling material is recycled and pretreated according to the T0727 method in JTGE20-2011 "Testing Procedures for Asphalt and Asphalt Mixtures in Highway Engineering" to separate the old asphalt and old aggregate in the recycled asphalt mixture (RAP material). The performance indicators of the old asphalt are the same as those in Example 1.
[0053] In this embodiment, the mineral powder is obtained by grinding limestone. The mineral material grading step is the same as that in Example 1.
[0054] In this embodiment, the reactive adhesive mother solution is prepared from liquid polyester polyol, diisocyanate, chain extender cross-linking agent, tackifier resin, defoamer, and regeneration liquid.
[0055] By weight, the components and proportions for preparing the reactive adhesive mother solution are as follows: Liquid polyester polyol, which is polyethylene oxide glycol: 30%; Diisocyanate, 1,5-naphthalene diisocyanate: 10%; Chain extender, neopentyl glycol: 1%; Tackifying resin, petroleum resin C5: 6%; Defoaming agent, which is an organic fluorine defoaming agent: 2%; The mass of the regeneration fluid is 12% of the old asphalt in the recovered milling material.
[0056] The amount of each grade of material is determined by gradation design according to the dense gradation as the target mix ratio, and the mixed milling material is prepared. The amount of reactive adhesive mother liquid is determined by Marshall test, and the determination method is the same as that in Example 1.
[0057] In this embodiment, the regeneration liquid is a composite solvent obtained by mixing light oil, lubricant and stabilizer.
[0058] In terms of weight, the components and proportions for preparing the regeneration solution are as follows: Light oil, which is dearomatized alkane solvent oil: 80%; Lubricant, 6-hexanediol diglycidyl ether: 35%; Stabilizer, dianhydride: 5%.
[0059] In this embodiment, the preparation method of the above-mentioned reactive quick-setting high-strength recycled asphalt cold patch material comprises the following steps: Step 1: Get the recycled milling material, crush it into fine particles with a maximum nominal particle size of 19.5 mm, and then screen it to divide it into three types: 0-5 mm, 5-10 mm, and 10-15 mm: Step 2, preparing a reactive adhesive mother solution, specifically comprising the following steps: Step 2-1, polyol dehydration: weigh each component by mass, add liquid polyester polyol and regeneration liquid into the reaction kettle and stir to mix, heat to 120°C with a temperature-controlled heating jacket, use a vacuum pump to reduce the system pressure by 0.67±0.03Kpa to evacuate and dehydrate for 2h, cool to 70°C and wait for use; Step 2-2, preparation of prepolymer: adding the melted diisocyanate into a reaction kettle, slowly heating to 125° C., stirring at a speed of 400 r / min under a nitrogen atmosphere for 1 h to obtain a prepolymer; Step 2-3, synthesizing mother liquor: add chain extender, crosslinking agent, tackifying resin and defoaming agent to the prepolymer in sequence, keep stirring at high speed for 2 hours under vacuum, cool to 80°C, quickly discharge and package in aluminum foil bag to obtain reactive adhesive mother liquor; Step 3: stir the milling material recovered in step 1, the reactive adhesive mother liquor in step 2 and the mineral powder at a speed of 40 r / min for 60 seconds to prepare a reactive quick-setting high-strength recycled asphalt cold patch material. Example 3
[0060] This embodiment provides a reactive quick-setting high-strength recycled asphalt cold patch material, which is prepared with recycled milling material as aggregate, mineral powder and reactive adhesive mother liquid; By weight, the components and proportions of the reactive quick-setting high-strength recycled asphalt cold patch material are as follows: Recycled milling material as aggregate: 92%; Mineral powder: 7%; Reactive adhesive masterbatch: 3.3%; The stability of the reactive quick-setting high-strength recycled asphalt cold patch material is 30.2 kN, and the dynamic stability is 10,000 times•mm -1 , the low temperature strain is 2898με, the freeze-thaw strength ratio is 89%, and the flying loss is 4.8%.
[0061] The recycled milling material is asphalt pavement surface milling material, including old asphalt and old aggregate.
[0062] The recycled milling materials are divided into three types: particle sizes of 0-5mm, 5-10mm, and 10-15mm, and the moisture content is less than or equal to 0.5%.
[0063] In this embodiment, the recycled milling material is recycled and pretreated according to the T0727 method in JTGE20-2011 "Testing Procedures for Asphalt and Asphalt Mixtures in Highway Engineering" to separate the old asphalt and old aggregate in the recycled asphalt mixture (RAP material). The performance indicators of the old asphalt are the same as those in Example 1.
[0064] In this embodiment, the mineral powder is obtained by grinding strong basic rock. The mineral material grading step is the same as that in embodiment 1.
[0065] In this embodiment, the reactive adhesive mother solution is prepared from liquid polyester polyol, diisocyanate, chain extender cross-linking agent, tackifier resin, defoamer, and regeneration liquid.
[0066] By weight, the components and proportions for preparing the reactive adhesive mother solution are as follows: Liquid polyester polyol, polytetramethylene glycol: 50%; Diisocyanate, 1,6-diisocyanate: 40%; Chain extender crosslinker, 1,4-butanediol: 3%; Tackifying resin, rosin glycerol ester: 6%; Defoamer, non-silicon defoamer: 2%; The mass of the regeneration fluid is 15% of the old asphalt in the recovered milling material.
[0067] The amount of each grade of material is determined by gradation design according to the dense gradation as the target mix ratio, and the mixed milling material is prepared. The amount of reactive adhesive mother liquid is determined by Marshall test, and the determination method is the same as that in Example 1.
[0068] In this embodiment, the regeneration liquid is a composite solvent obtained by mixing light oil, lubricant and stabilizer.
[0069] In terms of weight, the components and proportions for preparing the regeneration solution are as follows: Light oil, naphthenic oil: 90%; Lubricant, 6-hexanediol diglycidyl ether: 40%; Stabilizer, octanoic acid: 5%.
[0070] In this embodiment, the preparation method of the above-mentioned reactive quick-setting high-strength recycled asphalt cold patch material comprises the following steps: Step 1: Get the recycled milling material, crush it into fine particles with a maximum nominal particle size of 19.5 mm, and then screen it to divide it into three types: 0-5 mm, 5-10 mm, and 10-15 mm: Step 2, preparing a reactive adhesive mother solution, specifically comprising the following steps: Step 2-1, polyol dehydration: weigh each component by mass, add liquid polyester polyol and regeneration liquid into the reaction kettle and stir to mix, heat to 120°C with a temperature-controlled heating jacket, use a vacuum pump to reduce the system pressure by 0.67±0.03Kpa to evacuate and dehydrate for 2h, cool to 70°C and wait for use; Step 2-2, preparation of prepolymer: adding the melted diisocyanate into a reaction kettle, slowly heating to 125° C., stirring at a speed of 400 r / min under a nitrogen atmosphere for 1 h to obtain a prepolymer; Step 2-3, synthesizing mother liquor: add chain extender, crosslinking agent, tackifying resin and defoaming agent to the prepolymer in sequence, keep stirring at high speed for 2 hours under vacuum, cool to 80°C, quickly discharge and package in aluminum foil bag to obtain reactive adhesive mother liquor; Step 3: stir the milling material recovered in step 1, the reactive adhesive mother liquor in step 2 and the mineral powder at a speed of 40 r / min for 60 seconds to prepare a reactive quick-setting high-strength recycled asphalt cold patch material. Example 4
[0071] This embodiment provides a reactive quick-setting high-strength recycled asphalt cold patch material, which is prepared with recycled milling material as aggregate, mineral powder and reactive adhesive mother liquid; By weight, the components and proportions of the reactive quick-setting high-strength recycled asphalt cold patch material are as follows: Recycled milling material as aggregate: 90%; Mineral powder: 7%; Reactive adhesive mother liquor: 3.46%; The stability of the reactive quick-setting high-strength recycled asphalt cold patch material is 29.8 kN, and the dynamic stability is 11500 times•mm -1 , the low temperature strain is 2401με, the freeze-thaw strength ratio is 84%, and the flying loss is 7.2%.
[0072] The recycled milling material is asphalt pavement surface milling material, including old asphalt and old aggregate.
[0073] The recycled milling materials are divided into three types: particle sizes of 0-5mm, 5-10mm, and 10-15mm, and the moisture content is less than or equal to 0.5%.
[0074] In this embodiment, the recycled milling material is recycled and pretreated according to the T0727 method in JTGE20-2011 "Testing Procedures for Asphalt and Asphalt Mixtures in Highway Engineering" to separate the old asphalt and old aggregate in the recycled asphalt mixture (RAP material). The performance indicators of the old asphalt are the same as those in Example 1.
[0075] In this embodiment, the mineral powder is obtained by grinding strong basic rock. The mineral material grading step is the same as that in embodiment 1.
[0076] In this embodiment, the reactive adhesive mother solution is prepared from liquid polyester polyol, diisocyanate, chain extender cross-linking agent, tackifier resin, defoamer, and regeneration liquid.
[0077] By weight, the components and proportions for preparing the reactive adhesive mother solution are as follows: Liquid polyester polyol, polyoxypropylene glycol: 40%; Diisocyanate, hexamethylene diisocyanate: 40%; Chain extender crosslinker, 2-hydroxypropyl acrylate: 3%; Tackifying resin, polyvinyl acetate: 5%; Defoamer, which is a mineral oil defoamer: 2%; The mass of the regeneration fluid is 8% of the old asphalt in the recovered milling material.
[0078] The amount of each grade of material is determined by gradation design according to the dense gradation as the target mix ratio, and the mixed milling material is prepared. The amount of reactive adhesive mother liquid is determined by Marshall test, and the determination method is the same as that in Example 1.
[0079] In this embodiment, the regeneration liquid is a composite solvent obtained by mixing light oil, lubricant and stabilizer.
[0080] In terms of weight, the components and proportions for preparing the regeneration solution are as follows: Light oil, dearomatized alkane solvent oil: 90%; Lubricant, 6-hexanediol diglycidyl ether: 40%; Stabilizer, lauric acid: 5%.
[0081] In this embodiment, the preparation method of the above-mentioned reactive quick-setting high-strength recycled asphalt cold patch material comprises the following steps: Step 1: Get the recycled milling material, crush it into fine particles with a maximum nominal particle size of 19.5 mm, and then screen it to divide it into three types: 0-5 mm, 5-10 mm, and 10-15 mm: Step 2, preparing a reactive adhesive mother solution, specifically comprising the following steps: Step 2-1, polyol dehydration: weigh each component by mass, add liquid polyester polyol and regeneration liquid into the reaction kettle and stir to mix, heat to 120°C with a temperature-controlled heating jacket, use a vacuum pump to reduce the system pressure by 0.67±0.03Kpa to evacuate and dehydrate for 2h, cool to 70°C and wait for use; Step 2-2, preparation of prepolymer: adding the melted diisocyanate into a reaction kettle, slowly heating to 125° C., stirring at a speed of 400 r / min under a nitrogen atmosphere for 1 h to obtain a prepolymer; Step 2-3, synthesizing mother liquor: add chain extender, crosslinking agent, tackifying resin and defoaming agent to the prepolymer in sequence, keep stirring at high speed for 2 hours under vacuum, cool to 80°C, quickly discharge and package in aluminum foil bag to obtain reactive adhesive mother liquor; Step 3: stir the milling material recovered in step 1, the reactive adhesive mother liquor in step 2 and the mineral powder at a speed of 40 r / min for 60 seconds to prepare a reactive quick-setting high-strength recycled asphalt cold patch material.
[0082] Comparative Example 1 Hot mix asphalt mixture, that is, hot mix AC-13 asphalt mixture. Comparative Example 2
[0083] A commodity cold patch material with high market sales.
[0084] In the above embodiments and comparative examples, test specimens were formed in accordance with JTG E20-2011 "Test Procedures for Asphalt and Asphalt Mixtures in Highway Engineering", and their strength indicators were tested by stability test, their high and low temperature performance were tested by rutting test and bending creep test, and their water stability was tested by freeze-thaw splitting test and Kentburg scattering test. The specific test results are shown in Table 3 below.
[0085] Table 3 Performance indexes of asphalt mixture materials
[0086] It can be seen from Table 3 that the stability of the four embodiments is greater than 28 kN, the dynamic stability is greater than 10,000 times, the low-temperature strain is greater than 2500 με, the freeze-thaw strength ratio is greater than 85%, and the flying loss is less than 10%. Compared with hot-mix asphalt mixture and commercial cold patch material, the reactive quick-setting high-strength recycled asphalt cold patch material prepared by the present invention has excellent performance.
[0087] Comprehensive preparation process and properties of each component show that reactive quick-setting high-strength recycled asphalt cold patch material has excellent high temperature stability, water stability, and low temperature crack resistance. The utilization rate of RAP material in the present invention is 90-96%, which greatly improves the reuse rate of milling materials, alleviates the dual problems of solid waste accumulation and shortage of high-quality stone resources, and the application of RAP material in cold patch material enables it to be efficiently and high-quality regenerated. The combination of the two technologies achieves the effect of 1+1>2, which has good application value and economic benefits.
[0088] It should be understood that the present invention is not limited to what has been described above and that various modifications and changes may be made without departing from its scope. The scope of the present invention is limited only by the appended claims.
Claims
1. A reactive quick-setting high-strength recycled asphalt cold patch material, characterized in that: The cold patch material is prepared with recycled milling material as aggregate, mineral powder and reactive adhesive mother liquid; By weight, the components and proportions of the reactive quick-setting high-strength recycled asphalt cold patch material are as follows: Recycled milling material as aggregate: 90-96%; Mineral powder: 4-7%; Reactive adhesive masterbatch: 3-6%; The stability of the reactive quick-setting high-strength recycled asphalt cold patch material is 28.6-31.2 kN, and the dynamic stability is 10000-12000 times•mm -1 , the low temperature strain is 2401-3015με, the freeze-thaw strength ratio is 84-89%, and the flying loss is 4.8-7.2%.
2. The reactive quick-setting high-strength recycled asphalt cold patch material according to claim 1, characterized in that: The recycled milling material includes one or more of old asphalt and old aggregate.
3. The reactive quick-setting high-strength recycled asphalt cold patch material according to claim 1, characterized in that: The mineral powder is obtained by grinding limestone or strong basic rock.
4. The reactive quick-setting high-strength recycled asphalt cold patch material according to claim 2, characterized in that: The reactive adhesive mother solution is prepared from liquid polyester polyol, diisocyanate, chain extender crosslinking agent, tackifying resin, defoamer and regeneration liquid.
5. The reactive quick-setting high-strength recycled asphalt cold patch material according to claim 4, characterized in that: By weight, the components and proportions for preparing the reactive adhesive mother solution are as follows: Liquid polyester polyol: 30-50%; Diisocyanate: 10-40%; Chain extender crosslinker: 1-3%; Tackifying resin: 3-6%; Defoaming agent: 1-2%; The mass of the regeneration fluid is 8-15% of the old asphalt in the recovered milling material.
6. The reactive quick-setting high-strength recycled asphalt cold patch material according to claim 5, characterized in that: The liquid polyester polyol is a polymer formed by polycondensation of one or more combinations of polyoxypropylene glycol, polyoxyethylene glycol, polytetrahydrofuran diol, 4-cyclohexanedicarboxylic acid-3-methyl-1,5-pentanediol, and ester diol; The diisocyanate is one or more of diphenylmethane diisocyanate, 1,5-naphthalene diisocyanate, polymethylene polyphenyl polyisocyanate, 1,6-diisocyanato, hexamethylene diisocyanate, isophorone diisocyanate, and 3,3'-dimethyldiphenylmethane-4,4' diisocyanate; The chain extending cross-linking agent is one or more of diethylene glycol, neopentyl glycol, 1,4-butanediol, and 2-hydroxypropyl 2-acrylate; The tackifying resin is one or more of terpene phenol resin, petroleum resin C5 or its hydrogenated product, rosin glycerol ester, and polyvinyl acetate; The defoamer is one or more of an organosilicon defoamer, an organofluorine defoamer, a non-silicon defoamer, and a mineral oil defoamer; The regeneration liquid is a composite solvent obtained by mixing light oil, lubricant and stabilizer.
7. The reactive quick-setting high-strength recycled asphalt cold patch material according to claim 6, characterized in that: In terms of weight, the components and proportions for preparing the regeneration solution are as follows: Light oil: 80-100%; Lubricant: 30-50%; Stabilizer: 2-5%.
8. A method for preparing the reactive quick-setting high-strength recycled asphalt cold patch material according to any one of claims 1 to 7, characterized in that: The steps include: Step 1: Get the recycled milling material: Step 2, preparing a reactive adhesive mother solution; Step 3: stir the milling material recovered in step 1, the reactive adhesive mother liquor in step 2 and the mineral powder at a speed of 40-60 r / min for 60-70 s to prepare a reactive quick-setting high-strength recycled asphalt cold patch material.
9. The method for preparing the reactive quick-setting high-strength recycled asphalt cold patch material according to claim 8, characterized in that: In step 1, the milling material is crushed into fine particles with a maximum nominal particle size of 19.5 mm, and then sieved to separate the milling material into three types: 0-5 mm, 5-10 mm, and 10-15 mm; The method for preparing the reactive adhesive mother solution in step 2 comprises the following steps: Step 2-1, polyol dehydration: weigh each component by mass, add liquid polyester polyol and regeneration liquid into the reaction kettle and stir to mix, heat to 120-130°C with a temperature-controlled heating jacket, use a vacuum pump to reduce the system pressure by 0.67±0.03Kpa to evacuate and dehydrate for 2-3h, cool to 60-70°C and wait for use; Step 2-2, preparation of prepolymer: adding the melted diisocyanate into a reaction kettle, slowly heating to 120-130° C., stirring at a speed of 400-600 r / min under a nitrogen atmosphere for 1-2 h to obtain a prepolymer; Step 2-3, synthesizing mother liquor: add chain extender crosslinking agent, tackifying resin and defoaming agent to the prepolymer in sequence, keep stirring at high speed under vacuum conditions for 2-3 hours, cool to 70-80°C and then quickly discharge and package in an aluminum foil bag to obtain a reactive adhesive mother liquor.
10. A curing material, characterized in that: The solidified material is obtained by solidifying the reactive quick-setting high-strength recycled asphalt cold patch material according to any one of claims 1 to 7.
Citation Information
Patent Citations
Crumb rubber powder composited regenerated all-weather road cold-patch material and production method thereof
CN103145376A
Efficient recycled asphalt mixture and preparation process thereof
CN112125575A
Composite regenerant, warm-mixing recycled asphalt mixture and preparation method of warm-mixing recycled asphalt mixture
CN115418081A
Cold-in-place recycling mixture and road surface recycling method
CN115677271A
In-situ temperature mixed polyurethane modified asphalt fully-recycled mixture and design method thereof
CN115925325A
Cited By
A bio-based toughened asphalt cold patch material, and a preparation method and application thereof
CN122789663A