Method for rapidly preparing lithium-rich spinel positive electrode and application

Lithium-rich spinel Li(Li0.17Mn0.83)2O4 positive electrode material is prepared by the lithium-manganese coordination polymer precursor in a short time and high temperature reaction, which solves the problems of poor cycle life and low production efficiency of the positive electrode material of lithium-ion batteries, and realizes the problem of low cycle life and production efficiency of the positive electrode material of lithium-ion batteries. Highly efficient electrochemical performance and low cost production.

CN119191359APending Publication Date: 2024-12-27CIVIL AVIATION UNIV OF CHINA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410904497.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-12-27

AI Technical Summary

Technical Problem

The cycle life of the positive electrode material of existing lithium-ion battery is affected by the Jahn-Teller distortion of Mn3+, resulting in poor electrochemical performance, and the traditional solid-phase synthesis process is time-consuming and labor-intensive, low production efficiency and high cost.

Method used

Lithium-manganese coordination polymer was used as the precursor, and lithium-manganese coordination polymer was formed by reacting at 140°C for 72 hours, and then nucleating in a short time of 450-550°C to obtain lithium-rich spinel Li (Li0.17Mn0 .83)2O4 positive electrode material.

Benefits of technology

A rapid preparation method with simple operation and strong repeatability is realized. The positive electrode material of lithium-ion battery shows good electrochemical performance after 100 cycles at a current density of 50mA g-1, and the capacity reaches 100.4mAh g-1, reducing production cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119191359A_ABST
    Figure CN119191359A_ABST
Patent Text Reader

Abstract

The invention discloses a method for rapidly and efficiently preparing lithium-rich spinel and application of the lithium-rich spinel in the field of energy storage. The chemical composition of the lithium-rich spinel is Li (Li0. 17Mn0. 83) 2O4. The method comprises the following steps: 1) weighing Li < + >, Mn < 2 + > and HCOOH according to different stoichiometric number ratios, putting the weighed Li < + >, Mn < 2 + > and HCOOH into a lining of a reaction kettle, adding a certain amount of N, N-dimethylformamide (DMF) solution into the lining of the reaction kettle to dissolve the materials, screwing the reaction kettle, putting the reaction kettle into an air dry oven, reacting for 72 hours at 140 DEG C, washing for 3-5 times by using a methanol (CH3OH) solution, and drying to obtain a precursor; drying to obtain a lithium-manganese coordination polymer precursor; and 2) placing the coordination polymer precursor in a porcelain boat of a tubular furnace, and reacting at a certain temperature for a certain time to obtain the lithium-rich spinel material Li (Li0. 17Mn0. 83) 2O4. And 3) Li (Li0. 17Mn0. 83) 2O4 is used as a lithium ion battery positive electrode material and is used in the field of energy storage. The synthesis method disclosed by the invention has the characteristics of simple experimental operation, high repeatability and the like; the lithium-rich spinel material prepared by the invention shows excellent electrochemical performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of energy storage technology and relates to Li(Li 0.17 Mn 0.83 ) 2 O 4 The rapid synthesis method of lithium-rich spinel positive electrode provides new ideas and directions for the development of lithium-ion battery positive electrodes. Background Art

[0002] At present, carbon peak and carbon neutrality have become a global consensus. The new energy industry has developed rapidly in response to the requirements of the times and helped reduce carbon emissions. In the past twenty years, lithium-ion batteries have been widely used in various portable electronic devices and energy vehicles. Researchers have achieved certain results in the research of negative electrode materials for lithium-ion batteries. The lithium storage performance is mainly restricted by the positive electrode materials. At present, the positive electrode materials used in the field of lithium-ion battery positive electrodes include layered LiCoO 2 , spinel structured LiMn 2 O 4 , and olivine structured LiFePO 4 Among them, spinel structured LiMn 2 O 4 With its advantages of good safety performance and low price, it has attracted wide attention in power banks, electric bicycles and power batteries. 2 O 4 The spinel structure of Li + Provides a three-dimensional diffusion channel, Li + The rapid diffusion of LiMn 2 O 4 It has excellent rate performance. But LiMn 2 O 4 The electrochemical performance of the positive electrode is still affected by Mn 3+ The Jahn-Teller distortion of the lithium-rich spinel (Li 1+x Mn 2-x O 4 ) The positive electrode passes through Li + Partially replace Mn 3+ , thereby reducing Mn 3+ concentration, which can effectively improve the electrochemical performance. Usually, the lithium-rich spinel positive electrode is synthesized by a solid phase method, which involves 3 、LiNO 3 , LiOH) and manganese-containing compounds (MnO 2 , Mn 3 O 4 、Mn(NO 3 ) 2、MnCO 3 ) are mixed in a certain proportion and calcined at high temperature. The typical calcination temperature range is 750-800°C, and the calcination time is about 12 hours or more. Obviously, this process is time-consuming and labor-intensive, resulting in low production efficiency and high cost.

[0003] The present invention proposes a method for rapidly preparing a lithium-rich spinel positive electrode using a lithium-manganese coordination polymer as a precursor. + and Mn 2+ The uniform distribution at the microscopic level promotes the lithium-rich spinel Li(Li 0.17 Mn 0.83 ) 2 O 4 Rapid nucleation at a certain temperature. The synthesis method of the invention has the characteristics of simple operation and strong repeatability, and the lithium-rich spinel material prepared by the invention shows excellent electrochemical performance. Summary of the invention

[0004] The present invention aims to provide a method for preparing lithium-rich spinel Li (Li 0.17 Mn 0.83 ) 2 O 4 Positive method.

[0005] The purpose of the present invention is achieved through the following technical solutions:

[0006] Li-rich spinel cathode refers to a cathode in which part of the Li is substituted for the spinel (LiMn 2 O 4 ) 3+ , the formed Li 1+ x Mn 2-x O 4 The positive electrode, the lithium-rich spinel material synthesized by the present invention is Li (Li 0.17 Mn 0.83 ) 2 O 4 .

[0007] The preparation method of the lithium-rich spinel comprises the following steps: 1) weighing Li + , Mn 2+ and HCOOH were placed in the reactor lining, a certain amount of N,N-dimethylformamide solution (DMF) was added to the reactor lining to dissolve it, the reactor was tightened, placed in a forced air drying oven, reacted at 140°C for 72 hours, and methanol (CH 3OH) solution for 3-5 times, and then dried to obtain a lithium-manganese coordination polymer precursor; 2) placing the coordination polymer precursor in a porcelain boat of a tube furnace, and reacting at a certain temperature for a certain time to obtain a lithium-rich spinel material Li (Li 0.17 Mn 0.83 ) 2 O 4 3) Li(Li 0.17 Mn 0.83 ) 2 O 4 As a positive electrode material for lithium-ion batteries, it is used in the field of energy storage.

[0008] Preferably, the positive electrode material of the lithium-ion battery is 50 mA g -1 At the current density of 1.5 Å, good electrochemical performance was obtained after 100 cycles with a capacity of 100.4 mAh g -1 .

[0009] Preferably, in step 1), Mn 2+ From Mn(NO 3 ) 2 ·4H 2 O, Li + It is derived from LiOH, and the molar ratio thereof is between 1:4 and 1:8. The volume of N,N-dimethylformamide is 40% of the volume of the reactor, and the volume of HCOOH is 10% of the volume of N,N-dimethylformamide.

[0010] Preferably, the certain temperature in step 2) is 450-550°C, preferably 500°C.

[0011] Preferably, in step 2), the certain time is 5-8 minutes, preferably 8 minutes.

[0012] Preferably, in step 3), the lithium-rich spinel material Li (Li 0.17 Mn 0.83 ) 2 O 4 The material is used as a positive electrode in lithium-ion battery applications, the electrolyte is 1M LiPF 6 / EC:DEC (v / v=1:1), voltage range is 1.8V-3.6V.

[0013] Compared with the prior art, the present invention has the following beneficial effects:

[0014] (1) The preparation method adopted by the present invention can obtain lithium-rich spinel material Li (Li 0.17 Mn 0.83 ) 2 O 4 positive electrode.

[0015] (2) The positive electrode material of the lithium ion battery prepared by the present invention is -1 At a current density of 1.344 W, good electrochemical performance was obtained after 100 cycles with a capacity of 100.4 mAh g -1 . BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 The lithium-rich spinel material Li(Li 0.17 Mn 0.83 ) 2 O 4 X-ray diffraction (XRD) patterns of the samples.

[0017] Figure 2 The lithium-rich spinel material Li(Li 0.17 Mn 0.83 ) 2 O 4 As a positive electrode material for lithium-ion batteries at 50 mA g -1 Cyclic performance diagram under 24-hour conditions. DETAILED DESCRIPTION

[0018] Embodiment 1:

[0019] Weigh 4 mmol of LiOH and 1 mmol of Mn(NO 3 ) 2 ·4H 2 O, pour it into a 25ml polytetrafluoroethylene reactor liner, add 10ml DMF and 1ml formic acid, stir until completely dissolved, and remove the stirrer. Seal the reactor containing the above reaction raw materials and put it into a 140℃ forced air drying oven for 72h. After the reaction is completed, let the reactor cool to room temperature naturally. Open the reactor, pour out the supernatant, add methanol solution to wash 3-5 times, and dry. Put the dried sample into a tubular furnace at 450℃ for 8 minutes, and test it as a positive electrode material for lithium-ion batteries at 50mA g -1 At the current density of 1.5 Å, good electrochemical performance was obtained after 100 cycles with a capacity of 80.3 mAh g -1 .

[0020] Embodiment 2:

[0021] Weigh 5 mmol of LiOH and 1 mmol of Mn(NO 3 ) 2 ·4H 2O, pour it into a 25ml polytetrafluoroethylene reactor lining, add 10ml DMF and 1ml formic acid, stir until completely dissolved, and remove the stirrer. Seal the reactor containing the above reaction raw materials and place it in a 140℃ forced air drying oven for 72h. After the reaction is completed, allow the reactor to cool to room temperature naturally. Open the reactor, pour out the supernatant, add methanol solution to wash 3-5 times, and dry. Place the dried sample in a tubular furnace at 500℃ for 5 minutes, and test it as a positive electrode material for lithium-ion batteries at 50mA g -1 At the current density of 1.5 Å, good electrochemical performance was obtained after 100 cycles with a capacity of 90.8 mAh g -1 .

[0022] Embodiment 3:

[0023] Weigh 12 mmol of LiOH and 2 mmol of Mn(NO 3 ) 2 ·4H 2 O, pour it into a 50ml polytetrafluoroethylene reactor lining, add 20ml DMF and 2ml formic acid, stir until completely dissolved, and remove the stirrer. Seal the reactor containing the above reaction raw materials and put it into a 140℃ forced air drying oven for 72h. After the reaction is completed, let the reactor cool to room temperature naturally. Open the reactor, pour out the supernatant, add methanol solution to wash 3-5 times, and dry. Put the dried sample into a tubular furnace at 500℃ for 8 minutes, and test it as a positive electrode material for lithium-ion batteries at 50mA g -1 At the current density of 1.5 Å, good electrochemical performance was obtained after 100 cycles with a capacity of 100.4 mAh g -1 .

[0024] Embodiment 4:

[0025] Weigh 28 mmol of LiOH and 4 mmol of Mn(NO 3 ) 2 ·4H 2 O, pour it into a 100ml polytetrafluoroethylene reactor lining, add 40ml DMF and 4ml formic acid, stir until completely dissolved, and remove the stirrer. Seal the reactor containing the above reaction raw materials and put it into a 140℃ forced air drying oven for 72h. After the reaction is completed, let the reactor cool to room temperature naturally. Open the reactor, pour out the supernatant, add methanol solution to wash 3-5 times, and dry. Put the dried sample into a tubular furnace at 550℃ for 5 minutes, and test it as a positive electrode material for lithium-ion batteries at 50mA g -1 At the current density of 1.5 Å, good electrochemical performance was obtained after 100 cycles with a capacity of 85.9 mAh g -1 .

[0026] Embodiment 5:

[0027] Weigh 8 mmol of LiOH and 1 mmol of Mn(NO 3 ) 2 ·4H 2 O, pour it into a 25ml polytetrafluoroethylene reactor liner, add 10ml DMF and 1ml formic acid, stir until completely dissolved, and remove the stirrer. Seal the reactor containing the above reaction raw materials and put it into a 140℃ forced air drying oven for 72h. After the reaction is completed, let the reactor cool to room temperature naturally. Open the reactor, pour out the supernatant, add methanol solution to wash 3-5 times, and dry. Put the dried sample into a tubular furnace at 550℃ for 8 minutes, and test it as a positive electrode material for lithium-ion batteries at 50mA g -1 At the current density of 1.5 Å, good electrochemical performance was obtained after 100 cycles with a capacity of 89.6 mAh g -1 .

[0028] The parts of the embodiments herein that are not exhaustive of the midpoint values ​​of the technical scope claimed for protection by the present invention and the new technical solutions formed by equivalent replacement of single or multiple technical features in the technical solutions of the embodiments are also within the scope claimed for protection by the present invention; at the same time, in all the listed or unlisted embodiments of the scheme of the present invention, each parameter in the same embodiment merely represents an example of its technical solution (i.e., a feasible solution), and there is no strict coordination and limitation relationship between the parameters, wherein the parameters can be replaced with each other without violating the axioms and the claims of the present invention, unless otherwise stated.

[0029] The technical means disclosed in the scheme of the present invention are not limited to the technical means disclosed in the above technical means, but also include technical schemes composed of any combination of the above technical features. The above is a specific implementation of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications are also regarded as the protection scope of the present invention.

[0030] The specific embodiments described herein are merely examples of the spirit of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in similar ways, but they will not deviate from the spirit of the present invention or exceed the scope defined by the appended claims.

Claims

1. A method for preparing a lithium-rich spinel positive electrode material, characterized in that: The following steps are involved: 1) According to different stoichiometric ratios, measure Li + , Mn 2+ and HCOOH into the lining of the reactor, add a certain amount of N,N-dimethylformamide solution (DMF) to the lining of the reactor to dissolve it, tighten the reactor, place it in a forced air drying oven, react at 140°C for 72 hours, wash it with methanol (CH3OH) solution 3-5 times, and dry it to obtain a lithium-manganese coordination polymer precursor; 2) place the coordination polymer precursor in a porcelain boat of a tubular furnace, react at a certain temperature for a certain time, and obtain a lithium-rich spinel material Li (Li 0.17 Mn 0.83 )2O4.3) Li(Li 0.17 Mn 0.83 )2O4 is used as a positive electrode material for lithium-ion batteries and in the field of energy storage.

2. According to the preparation process of the coordination polymer precursor described in claim 1, Mn 2+ With Li + The molar ratio of the substances is between 1:4 and 1:8, the volume of N,N-dimethylformamide is 40% of the volume of the reactor, and the volume of HCOOH is 10% of the volume of N,N-dimethylformamide.

3. The calcination treatment according to claim 1 is specifically: calcination at 450-550°C for 5-8 minutes.

4. The method for preparing the lithium-rich spinel positive electrode material according to claim 1, characterized in that: The calcination treatment is performed in an air atmosphere or an oxygen atmosphere.

5. A lithium-rich spinel battery positive electrode material prepared by the preparation method according to claim 1 or 3.

6. Use of the lithium-rich spinel positive electrode material as claimed in claim 5 in lithium-ion batteries.

7. A method for preparing a battery according to claim 6, characterized in that: The following steps are involved: A slurry obtained by uniformly mixing the lithium-rich spinel positive electrode material, the conductive agent and the binder is coated on the surface of the current collector and dried to obtain a positive electrode; the positive electrode, the negative electrode and the electrolyte are assembled to obtain the battery.

8. Application of the battery as claimed in claim 7 in the fields of power banks, electric bicycles and power batteries.