Positive pole piece, secondary battery and electronic device

By setting multiple ripples on the edge area of ​​the positive electrode sheet of the lithium-ion battery, the problems of high scrap rate and uneven electrolyte infiltration caused by the wave edge of the positive electrode sheet are solved, and higher process efficiency and electrolyte infiltration rate are achieved, improving the electrical and safety performance of the battery.

CN119673956APending Publication Date: 2025-03-21NINGDE AMPEREX TECHNOLOGY LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411754626.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-12-02
Publication Date
2025-03-21

AI Technical Summary

Technical Problem

During the production process, existing lithium-ion batteries have high scrap rate due to the wave edge of the positive electrode plate, which affects efficiency, and the inefficient in the infiltration and transmission of the electrolyte lead to a degradation of safety performance and electrical performance.

Method used

A positive electrode sheet is designed, with a plurality of corrugations in the width direction, and the maximum depth of the corrugations is between 0.1 μm and 100 μm. This structure improves the process advantage of the positive electrode sheet and the wetting rate of the electrolyte.

Benefits of technology

The process efficiency of the positive electrode sheet is improved, the wetting time of the electrolyte on the positive electrode sheet is shortened, and the electrical and safety performance after cycling of the secondary battery is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119673956A_ABST
    Figure CN119673956A_ABST
Patent Text Reader

Abstract

The invention provides a positive pole piece, a secondary battery and an electronic device, the positive pole piece comprises a positive current collector and a positive active material layer arranged on at least one surface of the positive current collector, the width of the positive pole piece is W1, and 30mm < = W1 < = 150mm; along the width direction of the positive pole piece, a plurality of ripples are arranged on the edge area of at least one side of the positive pole piece, the maximum depth D of the ripples is greater than or equal to 0.1 mu m and less than or equal to 100 mu m. Through the arrangement, the process yield of the positive pole piece can be improved, the infiltration time of the electrolyte on the positive pole piece can be shortened, and the electrical performance and the safety performance of the secondary battery after circulation can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of electrochemical technology, and in particular to a positive electrode sheet, a secondary battery and an electronic device. Background Art

[0002] Secondary batteries (such as lithium-ion batteries) are the most researched chemical power source in the current new energy field. Due to its excellent comprehensive performance, its industrialization is the most mature, the research is the most profound, and the application is the most extensive in all new energy fields. However, the scale of lithium-ion battery production industry has reached a certain level. In the future, with the advancement of refined and intelligent manufacturing, rough development will gradually be eliminated, and cost reduction and efficiency improvement will become one of the problems that every company in the industry must face.

[0003] As the blood of lithium-ion batteries, electrolyte has always been one of the bottlenecks that affect the safety and electrical performance of lithium-ion batteries. In order to pursue the ultimate energy density, conventional winding structures, stacked structures, or other types of lithium-ion batteries often make the electrode assembly structure very dense, and subject the pole pieces and diaphragms to hot pressing, bonding, gluing, etc., so that the density of the electrode assembly is close to the compacted state, which greatly affects the infiltration and electrolyte transmission of lithium-ion batteries. At the same time, it may also reduce the electrolyte retention, resulting in uneven electrolyte distribution. Especially for some large-sized lithium-ion battery types, electrolyte infiltration and transmission are particularly critical. In order to improve the infiltration and electrolyte transmission of lithium-ion batteries, one of the solutions in the prior art is to improve it by cutting grooves in the pole pieces, reducing the hot pressing parameters of the electrode assembly, and reducing the viscosity of the electrolyte, but these methods are at the expense of great cost and performance.

[0004] At the same time, due to the extension of the positive electrode under cold pressing pressure, regular wavy edges are inevitable on the edge of the positive electrode, but the wavy edge of the positive electrode is one of the most undesirable factors that cause waste and affect efficiency in the production process of lithium-ion batteries, and it is also the most difficult industry problem to solve. Because more than 40% of the material cost of lithium-ion batteries comes from the positive electrode, improving the process excellence rate of the positive electrode is the most critical link for enterprises to reduce costs and increase efficiency. Summary of the invention

[0005] The purpose of the present application is to provide a positive electrode plate, a secondary battery and an electronic device to improve the process efficiency of the positive electrode plate, shorten the infiltration time of the electrolyte on the positive electrode plate, and improve the electrical performance and safety performance of the secondary battery after cycling.

[0006] It should be noted that in the invention content of this application, lithium-ion batteries are used as an example of secondary batteries to explain this application, but the secondary batteries of this application are not limited to lithium-ion batteries. The specific technical solutions are as follows:

[0007] The first aspect of the present application provides a positive electrode sheet, the positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer arranged on at least one surface of the positive electrode current collector, and the width of the positive electrode sheet is W 1 , 30mm≤W 1 ≤150mm; along the width direction of the positive electrode sheet, a plurality of corrugations are arranged in the edge area of ​​at least one side of the positive electrode sheet, and the maximum depth of the corrugations is D, 0.1μm≤D≤100μm. The positive electrode sheet provided in the first aspect of the present application has a width W 1 Meet 30mm≤W 1 When the positive electrode sheet is ≤150mm, by providing a plurality of corrugations in the edge area of ​​at least one side along the width direction of the positive electrode sheet, and by adjusting the maximum depth D of the corrugations to meet 0.1μm≤D≤100μm, the edge area of ​​the positive electrode sheet provided with corrugations can have a smaller height difference between the peak and the trough, and the overall flatness of the positive electrode sheet is improved, so that the process excellence rate of the positive electrode sheet will be improved. The arrangement of the corrugations in the edge area of ​​the positive electrode sheet along the width direction of the positive electrode sheet can make the edge area of ​​the positive electrode sheet have a larger gap, increase the infiltration rate of the electrolyte on the positive electrode sheet, and shorten the infiltration time of the electrolyte on the positive electrode sheet. The positive electrode sheet provided in the first aspect of the present application is applied to a secondary battery, which has a higher capacity retention rate, and the probability of abnormal phenomena (such as lithium precipitation, purple spots or black spots, etc.) occurring in the interface in the late cycle is reduced, so that the secondary battery has good electrical performance, and can also reduce the probability of the positive electrode sheet breaking due to expansion, so that the secondary battery has good safety performance after the charge and discharge cycle. Thus, through the above arrangement, the process optimization rate of the positive electrode sheet can be improved, the infiltration time of the electrolyte on the positive electrode sheet can be shortened, and the electrical performance and safety performance of the secondary battery after cycling can be improved. The edge area in this application is defined as an area less than or equal to 1 / 3 of the width of the positive electrode sheet from the edge of the positive electrode sheet in the width direction of the positive electrode sheet.

[0008] In one embodiment of the present application, 0.5 μm ≤ D ≤ 20 μm. The maximum depth D of the corrugation is set within the above range, the electrolyte infiltration time on the positive electrode plate is shortened, the safety performance of the secondary battery after cycling is improved, and the process efficiency of the positive electrode plate and the electrical performance of the secondary battery are further improved.

[0009] In one embodiment of the present application, the depth of the corrugations gradually decreases from the edge of the positive electrode sheet to the inside to 0 μm.

[0010] In one embodiment of the present application, a corrugation is provided in the edge area of ​​one side of the positive electrode sheet along the width direction of the positive electrode sheet, and the width of the corrugation is W 2 , W 1 and W 2 Satisfy: 5mm≤W 2≤20mm and W 2 ≤1 / 4W 1 A corrugation is provided at the edge area of ​​one side of the positive electrode plate, and the width of the corrugation is W 2 When set within the above range, the infiltration time of the electrolyte on the positive electrode plate is shortened, the electrical performance and safety performance of the secondary battery after cycle are improved, and the process efficiency of the positive electrode plate is further improved.

[0011] In one embodiment of the present application, along the length direction of the positive electrode sheet, the positive electrode sheet includes a double-sided region provided with a double-layer positive electrode active material layer, and the double-sided region includes a first region provided with corrugations; the length of the double-sided region is L 1 , the length of the first region is L 2 , L 2 =L 1 When the positive electrode sheet is provided with corrugations along the edge area on one side of its width direction, the length L of the double-sided area of ​​the positive electrode sheet is 1 The length L of the first region provided with the corrugations 2 Similarly, on the basis of improving the process efficiency of the positive electrode sheet, the infiltration time of the electrolyte on the positive electrode sheet is further shortened, and the electrical performance and safety performance of the secondary battery after cycling are further improved.

[0012] In one embodiment of the present application, along the width direction of the positive electrode sheet, ripples are respectively provided at the edge regions on both sides of the positive electrode sheet, and the width of the ripples is W. 2 , W 1 and W 2 Satisfy: 3mm≤W 2 ≤20mm and W 2 ≤1 / 3W 1 Corrugations are set on the edge areas on both sides of the positive electrode plate, and the width of the corrugations is W 2 When the above range is set, the process optimization rate of the positive electrode plate is improved, the infiltration time of the electrolyte on the positive electrode plate is further shortened, and the electrical performance and safety performance of the secondary battery after the cycle are further improved.

[0013] In one embodiment of the present application, along the length direction of the positive electrode sheet, the positive electrode sheet includes a double-sided region provided with a double-layer positive electrode active material layer, and the double-sided region includes a second region provided with corrugations; the length of the double-sided region is L 1 , the length of the second region is L 3 , 1 / 3L 1 ≤L 3 ≤L 1 When the positive electrode sheet is provided with corrugations on both sides of the edge area along its width direction, the length L of the double-sided area of ​​the positive electrode sheet is 1The length L of the second region provided with the corrugations 3 When the above relationship is satisfied, the process efficiency of the positive electrode plate is improved, the infiltration time of the electrolyte on the positive electrode plate is shortened, and the electrical performance and safety performance of the secondary battery after cycling are improved.

[0014] In one embodiment of the present application, the spacing between two adjacent corrugations is 3 mm to 20 mm. By adjusting the spacing between two adjacent corrugations within the above range, the process efficiency of the positive electrode sheet can be improved, and the infiltration time of the electrolyte on the positive electrode sheet can be shortened. In addition, the secondary battery using the positive electrode sheet has good electrical performance and safety performance.

[0015] In one embodiment of the present application, the distance between two adjacent corrugations is 3 mm to 12 mm. Adjusting the distance between two adjacent corrugations within the above range is conducive to further improving the process efficiency of the positive electrode sheet, shortening the infiltration time of the electrolyte on the positive electrode sheet, and improving the electrical performance and safety performance of the secondary battery after the charge and discharge cycle.

[0016] In one embodiment of the present application, the angle between the center line of the corrugation and the length direction of the positive electrode sheet is 85° to 95°. By adjusting the angle between the center line of the corrugation and the length direction of the positive electrode sheet within the above range, the process efficiency of the positive electrode sheet is improved, the infiltration time of the electrolyte on the positive electrode sheet is further shortened, and the electrical performance and safety performance of the secondary battery after cycling are further improved.

[0017] The second aspect of the present application provides a secondary battery, which includes the positive electrode sheet described in any of the above embodiments. The secondary battery of the present application has good safety performance and electrical performance.

[0018] The third aspect of the present application provides an electronic device, which comprises the secondary battery described in any one of the above embodiments. Therefore, the electronic device has good performance.

[0019] Beneficial effects of this application:

[0020] The present application provides a positive electrode sheet, a secondary battery and an electronic device. The positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer arranged on at least one surface of the positive electrode current collector. The width of the positive electrode sheet is W 1 , 30mm≤W 1 ≤150mm; along the width direction of the positive electrode sheet, a plurality of corrugations are arranged in the edge area of ​​at least one side of the positive electrode sheet, and the maximum depth of the corrugations is D, 0.1μm≤D≤100μm. Through the above arrangement, the process optimization rate of the positive electrode sheet can be improved, the infiltration time of the electrolyte on the positive electrode sheet can be shortened, and the electrical performance and safety performance of the secondary battery after cycling can be improved.

[0021] Of course, implementing any product or method of the present application does not necessarily require achieving all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application, and for ordinary technicians in this field, other embodiments can also be obtained based on these drawings.

[0023] Figure 1 A schematic diagram of the cross-sectional structure of a positive electrode sheet along its length and width directions according to an embodiment of the present application;

[0024] Figure 2 For along Figure 1 Sectional view along line AA;

[0025] Figure 3 For along Figure 1 Sectional view along the midline BB;

[0026] Figure 4 A schematic diagram of the cross-sectional structure of a positive electrode sheet along its length direction and thickness direction according to an embodiment of the present application;

[0027] Figure 5 It is a schematic diagram of the cross-sectional structure of a positive electrode sheet along its length direction and width direction according to another embodiment;

[0028] Figure 6 This is a schematic diagram of the cross-sectional structure of a positive electrode sheet along its length and thickness directions according to another embodiment of the present application.

[0029] Reference numerals:

[0030] 10 - positive electrode sheet; 11 - positive electrode current collector; 12 - positive electrode active material layer; 20 - edge region; 21 - first region; 22 - second region; 31 - center line; 41 - double-sided region; 42 - single-sided region; 43 - empty foil region. DETAILED DESCRIPTION

[0031] The following will be combined with the embodiments of the present application and the accompanying drawings to clearly and completely describe the technical solutions in the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all the embodiments. All other embodiments obtained by those skilled in the art based on the present application belong to the scope of protection of the present application.

[0032] It should be noted that in the specific implementation manner of the present application, the present application is explained by taking a lithium-ion battery as an example of a secondary battery, but the secondary battery of the present application is not limited to a lithium-ion battery.

[0033] The first aspect of the present application provides a positive electrode sheet, the positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer arranged on at least one surface of the positive electrode current collector, and the width of the positive electrode sheet is W 1 , 30mm≤W 1 ≤150mm; along the width direction of the positive electrode sheet, a plurality of corrugations are arranged in the edge area of ​​at least one side of the positive electrode sheet, and the maximum depth of the corrugations is D, 0.1μm≤D≤100μm.

[0034] For ease of understanding, in this application, the length direction of the positive electrode sheet itself is defined as X, the width direction is defined as Y, and the thickness direction is defined as Z. It should be understood that the above definition of the direction is for the convenience of describing the purpose of this application, and the direction defined in this application can be understood based on the relative positions of the drawings and the actual product elements. In addition, the width direction, length direction and thickness direction of the positive electrode active material layer and the positive electrode current collector themselves are the same as those of the positive electrode sheet. The above-mentioned "the positive electrode active material layer is arranged on at least one surface of the positive electrode current collector" means that the positive electrode active material layer is arranged on one surface or two surfaces of the positive electrode current collector, and the above-mentioned "surface" can be a partial surface of the positive electrode current collector or the entire surface of the positive electrode current collector. The above-mentioned "along the width direction of the positive electrode sheet, a plurality of corrugations are arranged in the edge area of ​​at least one side of the positive electrode sheet" means that along the width direction of the positive electrode sheet, a plurality of corrugations are arranged in the edge area of ​​one side or both sides of the positive electrode sheet. In this application, the "multiple" in "multiple corrugations" refers to two or more. This application does not particularly limit the specific number, as long as the purpose of this application can be achieved. Such as Figures 1 to 4 As shown, the positive electrode sheet 10 includes a positive electrode collector 11 and a positive electrode active material layer 12. Along the length direction X of the positive electrode sheet 10, the positive electrode sheet 10 includes a double-sided region 41 with a double-layer positive electrode active material layer 12 on both sides of the positive electrode collector 11 along its own thickness direction Z, a single-sided region 42 with a single-layer positive electrode active material layer 12 on one side of the positive electrode collector 11 along its own thickness direction Z, and a hollow foil region 43 with no positive electrode active material layer 12 on both sides of the positive electrode collector 11 along its own thickness direction Z. Along the width direction Y of the positive electrode sheet 10, a plurality of corrugations 30 are provided in the edge region 20 on one side of the positive electrode sheet 10. The maximum depth of the corrugation 30 is shown as D, and the width of the corrugation 30 is shown as W. 2 As shown, the width of the positive electrode sheet 10 is W 1 It is understood that, in another embodiment, the corrugation 30 can also be provided at the edge region 20 on the other side of the positive electrode sheet 10 along its width direction Y. Figure 5As shown, along the width direction Y of the positive electrode sheet 10, a plurality of corrugations 30 are respectively provided in the edge regions 20 on both sides of the positive electrode sheet 10. In the present application, the "maximum depth D of the corrugation" refers to the distance between the crest and the trough in the corrugation at the edge of the positive electrode sheet prepared along the same plane. In the present application, the "width of the corrugation" refers to the distance that the center line of the corrugation extends along the width direction of the positive electrode sheet, and the "center line of the corrugation" is a line used to mark the center of the corrugation, that is, a set of line segments marking the midpoint of the corrugation.

[0035] For example, D is 0.1μm, 1μm, 5μm, 10μm, 15μm, 20μm, 25μm, 30μm, 42μm, 50μm, 53μm, 58μm, 65μm, 70μm, 73μm, 76μm, 80μm, 90μm, 92μm, 100μm or any value between any two of the above numerical ranges. The maximum depth D of the corrugation is less than 0.1μm. The maximum depth of the corrugation is too small, the effect of the corrugation is difficult to play, the probability of shortening the infiltration time of the electrolyte on the positive electrode plate is small, the liquid retention amount of the positive electrode plate is small, and problems such as interface abnormalities will occur more frequently in the secondary battery using this positive electrode plate; the maximum depth D of the corrugation is greater than 100μm. The maximum depth of the corrugation is too large, and the height difference between the crest and trough of the corrugation in the edge area of ​​the positive electrode plate will be too large, resulting in poor flatness of the positive electrode plate. The secondary battery using this positive electrode plate has a large precision deviation and difficulty in adjustment, which makes the production of secondary batteries more difficult and increases the scrap rate of secondary batteries.

[0036] For example, W 1 30mm, 40mm, 56mm, 60mm, 70mm, 82mm, 90mm, 100mm, 110mm, 116mm, 123mm, 130mm, 141mm, 150mm or any value between any two of the above ranges. 1 If the width is less than 30mm or greater than 150mm, the width of the positive electrode plate is too small or too large and does not meet normal production requirements.

[0037] In general, the positive electrode sheet provided in the first aspect of the present application has a width W 1 Meet 30mm≤W 1When the positive electrode sheet is ≤150mm, by providing a plurality of corrugations in the edge area of ​​at least one side along the width direction of the positive electrode sheet, and by adjusting the maximum depth D of the corrugations to meet 0.1μm≤D≤100μm, the edge area of ​​the positive electrode sheet provided with corrugations can have a smaller height difference between the peak and the trough, and the overall flatness of the positive electrode sheet is improved, so that the process excellence rate of the positive electrode sheet will be improved. The positive electrode sheet provided in the first aspect of the present application is applied to a secondary battery, and the secondary battery has a higher capacity retention rate during the charge and discharge cycle, and the probability of abnormal phenomena (such as lithium precipitation, purple spots or black spots, etc.) in the interface in the late cycle is reduced, so that the secondary battery has good electrical performance, and can also reduce the probability of the positive electrode sheet breaking due to expansion, so that the secondary battery has good safety performance after the charge and discharge cycle. Therefore, through the above arrangement, the process efficiency of the positive electrode plate can be improved, the infiltration time of the electrolyte on the positive electrode plate can be shortened, and the electrical performance and safety performance of the secondary battery after cycling can be improved.

[0038] In one embodiment of the present application, 0.5μm≤D≤20μm. For example, D is 0.5μm, 1μm, 5μm, 7μm, 10μm, 13μm, 16μm, 20μm or any value between any two of the above numerical ranges. Setting the maximum depth D of the corrugation within the above range is more conducive to making the edge area of ​​the positive electrode sheet have a small height difference between the peak and the trough, and the overall flatness of the positive electrode sheet is further improved. In this way, the process excellence rate of the positive electrode sheet will be further improved. As a result, the infiltration time of the electrolyte on the positive electrode sheet is shortened, the safety performance of the secondary battery after cycling is improved, and the process excellence rate of the positive electrode sheet and the electrical performance of the secondary battery are further improved.

[0039] In one embodiment of the present application, the depth of the corrugations gradually decreases from the edge of the positive electrode sheet to the inner side to 0 μm. Figure 3 As shown, the depth of the corrugation 30 gradually decreases from the edge of the positive electrode sheet 10 to the inside to 0 μm, that is, gradually decreases to be flush with the surface of the positive electrode sheet 10 where the corrugation 30 is not provided. The above-mentioned corrugation is conducive to controlling the flatness of the edge of the positive electrode sheet, and is also conducive to the transmission of the electrolyte on the positive electrode sheet, which is conducive to making the positive electrode sheet have a good process quality rate, the electrolyte has a shorter infiltration time on the positive electrode sheet, and the secondary battery using the positive electrode sheet has good electrical performance and safety performance after cycling.

[0040] In one embodiment of the present application, a corrugation is provided in the edge area of ​​one side of the positive electrode sheet along the width direction of the positive electrode sheet, and the width of the corrugation is W2 , W 1 and W 2 Satisfy: 5mm≤W 2 ≤20mm and W 2 ≤1 / 4W 1 For example, W 2 5mm, 8mm, 9mm, 10mm, 12mm, 15mm, 17mm, 19mm, 20mm or any value between any two of the above ranges. Figure 1 As shown, along the width direction Y of the positive electrode sheet 10, the corrugation 30 is provided in the edge region 20 on one side of the positive electrode sheet 10. It is understandable that the corrugation 30 can also be provided in the edge region 20 on the other side of the positive electrode sheet 10 along its own width direction Y. The corrugation is provided in the edge region on one side of the positive electrode sheet, and the width W of the corrugation is set to 2 When set within the above range, the flatness consistency between the edge area of ​​the positive electrode sheet and the main body is more stable, and the shaping effect will not be poor and the wetting effect will not be improved significantly due to the fact that the edge area of ​​the corrugated plate does not account for the overall width of the positive electrode sheet, nor will the flatness be damaged due to the fact that the edge area of ​​the corrugated plate accounts for too much of the overall positive electrode sheet, resulting in large fluctuations in the process. It is more conducive to further improving the overall flatness of the positive electrode sheet, so that the process excellence rate of the positive electrode sheet will be further improved. As a result, the infiltration time of the electrolyte on the positive electrode sheet is shortened, the electrical performance and safety performance of the secondary battery after the cycle are improved, and the process excellence rate of the positive electrode sheet is further improved.

[0041] In one embodiment of the present application, when a corrugation is provided in an edge region on one side of the positive electrode sheet along the width direction of the positive electrode sheet, along the length direction of the positive electrode sheet, the positive electrode sheet includes a double-sided region provided with a double-layer positive electrode active material layer, and the double-sided region includes a first region provided with corrugations; the length of the double-sided region is L 1 , the length of the first region is L 2 , L 2 =L 1 When the corrugation is provided in the edge area of ​​one side of the positive electrode sheet along the width direction of the positive electrode sheet, such as Figure 4As shown, along the length direction X of the positive electrode sheet 10, the positive electrode sheet 10 includes a double-sided region 41 provided with a double-layer positive electrode active material layer 12, and also includes a single-sided region 42 provided with a single-layer positive electrode active material layer 12 and an empty foil region 43 without a positive electrode active material layer 12. It can be understood that the above-mentioned "double-sided region 41" refers to the positive electrode active material layer 12 is coated on the two surfaces of the positive electrode collector 11 along its own thickness direction Z, that is, the region where two layers of positive electrode active material layer 12 are provided on the two surfaces of the positive electrode collector 11; the above-mentioned "single-sided region 42" refers to the positive electrode active material layer 12 is coated on one of the surfaces of the positive electrode collector 11 along its own thickness direction Z, that is, the region where a layer of positive electrode active material layer 12 is provided on any surface of the positive electrode collector 11; the above-mentioned "empty foil region 43" refers to the region where no positive electrode active material layer 12 is provided on both surfaces of the positive electrode collector 11 along its own thickness direction Z. The double-sided area 41 includes a first area 21 provided with corrugations 30, and the length of the double-sided area 41 is L 1 , the length of the first region 21 is L 2 , L 2 =L 1 When the positive electrode sheet is provided with corrugations along the edge area on one side of its width direction, the length L of the double-sided area of ​​the positive electrode sheet is 1 The length L of the first region provided with the corrugations 2 Similarly, the gap at the edge of the positive electrode sheet can be made larger, the electrolyte can infiltrate and diffuse faster on the positive electrode sheet, the positive electrode sheet can retain more liquid, and the transmission channel of the electrolyte on the positive electrode sheet is smoother. In this way, the infiltration time of the electrolyte on the positive electrode sheet is shortened, which is beneficial to improving the performance of the secondary battery, such as cycle performance, rate performance, and safety performance. Therefore, on the basis of improving the process excellence rate of the positive electrode sheet, the infiltration time of the electrolyte on the positive electrode sheet is further shortened, and the electrical performance and safety performance of the secondary battery after cycling are further improved.

[0042] In one embodiment of the present application, along the width direction of the positive electrode sheet, ripples are respectively provided at the edge regions on both sides of the positive electrode sheet, and the width of the ripples is W. 2 , W 1 and W 2 Satisfy: 3mm≤W 2 ≤20mm and W 2 ≤1 / 3W 1 For example, W 2 3mm, 5mm, 8mm, 9mm, 10mm, 12mm, 15mm, 17mm, 19mm, 20mm or any value between any two of the above ranges. Figure 5As shown, along the width direction Y of the positive electrode sheet 10, the edge regions 20 on both sides of the positive electrode sheet 10 are provided with corrugations 30. The edge regions on both sides of the positive electrode sheet are provided with corrugations, and the width W of the corrugations is set to 2 When it is set within the above range, the edge areas on both sides of the positive electrode sheet can have a larger gap, the electrolyte diffuses and infiltrates faster from the edge to the inside along the width direction of the positive electrode sheet, the positive electrode sheet retains more liquid, and the transmission channel of the electrolyte on the positive electrode sheet is smoother. In this way, the infiltration time of the electrolyte on the positive electrode sheet is shortened, which is beneficial to improving the performance of the secondary battery, such as cycle performance, rate performance, and safety performance. Therefore, on the basis of improving the process excellence rate of the positive electrode sheet, the infiltration time of the electrolyte on the positive electrode sheet is further shortened, and the electrical performance and safety performance of the secondary battery after cycling are further improved.

[0043] In one embodiment of the present application, when corrugations are respectively provided at the edge regions on both sides of the positive electrode sheet along the width direction of the positive electrode sheet, along the length direction of the positive electrode sheet, the positive electrode sheet includes a double-sided region provided with a double-layer positive electrode active material layer, and the double-sided region includes a second region provided with corrugations; the length of the double-sided region is L 1 , the length of the second region is L 3 , 1 / 3L 1 ≤L 3 ≤L 1 When corrugations are respectively provided at the edge regions on both sides of the positive electrode sheet along the width direction of the positive electrode sheet, in some embodiments, such as Figure 6 As shown, along the length direction X of the positive electrode sheet 10, the positive electrode sheet 10 includes a double-sided region 41 provided with a double-layer positive electrode active material layer 12, a single-sided region 42 provided with a single-layer positive electrode active material layer 12, and an empty foil region 43 without a positive electrode active material layer 12. The double-sided region 41 includes a second region 22 provided with corrugations 30, and the length of the double-sided region 41 is L. 1 , the length of the second region 22 is L 3 , L 3 <L 1 It is understood that, in other embodiments, the length L of the second region 22 provided with the corrugations 30 is 3 The length L of the double-sided area 41 1 The same, that is, both sides of the positive electrode sheet are provided with corrugations 30. When the positive electrode sheet is provided with corrugations on both sides of the edge area along its width direction, the length L of the positive electrode sheet double-sided area is 1 The length L of the second region provided with the corrugations 3The above relationship is satisfied, and the edge areas on both sides of the positive electrode sheet along its width direction have a large gap, the electrolyte infiltrates and diffuses faster on the positive electrode sheet, and the positive electrode sheet has a high liquid retention capacity, so that the electrolyte is transmitted smoothly on the positive electrode sheet. And the positive electrode sheet has a high flatness, so that the positive electrode sheet has a high process excellence rate. The positive electrode sheet is applied to the secondary battery, and it has a high capacity retention rate during the charge and discharge cycle of the secondary battery. The probability of abnormal phenomena (such as lithium precipitation, purple spots or black spots, etc.) in the interface in the late cycle is reduced, so that the secondary battery has good electrical performance, and can also reduce the probability of the positive electrode sheet breaking due to expansion, so that the secondary battery has good safety performance after the charge and discharge cycle. Therefore, through the above arrangement, the process excellence rate of the positive electrode sheet can be improved, the infiltration time of the electrolyte on the positive electrode sheet can be shortened, and the electrical performance and safety performance of the secondary battery after the cycle can be improved.

[0044] In one embodiment of the present application, the distance between two adjacent corrugations is 3 mm to 20 mm. For example, the distance between two adjacent corrugations is 3 mm, 5 mm, 7 mm, 10 mm, 13 mm, 15 mm, 18 mm, 20 mm, or any value between any two of the above ranges. Figure 4 As shown, the spacing between two adjacent corrugations 30 is shown as σ. In the present application, "the spacing between two adjacent corrugations" refers to the distance between the center lines of two adjacent corrugations. By regulating the spacing between two adjacent corrugations within the above range, the area provided with the corrugations has a suitable number of corrugations, which can make the positive electrode plate have a higher flatness to improve its process excellence. At the same time, the corrugations provide more gaps, so that the electrolyte can quickly diffuse and infiltrate from the edge of the positive electrode plate to the inside. The positive electrode plate also has a higher liquid retention capacity, and the electrolyte infiltration time on the positive electrode plate is shortened. In addition, the secondary battery using the positive electrode plate has good electrical performance and safety performance.

[0045] In one embodiment of the present application, the spacing between two adjacent corrugations is 3 mm to 12 mm. For example, the spacing between two adjacent corrugations is 3 mm, 5 mm, 6 mm, 8 mm, 10 mm, 11 mm, 12 mm, or any value between any two of the above ranges. Regulating the spacing between two adjacent corrugations within the above range is conducive to shortening the infiltration time of the electrolyte on the positive electrode sheet, further improving the process excellence rate of the positive electrode sheet, and further improving the electrical performance and safety performance of the secondary battery after the charge and discharge cycle.

[0046] In one embodiment of the present application, the angle between the center line of the corrugation and the length direction of the positive electrode sheet is 85°C to 95°C. For example, the angle between the center line of the corrugation and the length direction of the positive electrode sheet is 85°C, 86°C, 88°C, 89°C, 90°C, 92°C, 94°C, 95°C or any value between any two of the above ranges. Figure 1 As shown, the angle between the center line 31 of the corrugation 30 and the length direction X of the positive electrode sheet 10 is shown as θ. It should be noted that "the angle between the center line of the corrugation and the length direction of the positive electrode sheet" refers to the maximum value of the angle formed by the center line of the corrugation and the extension lines on both sides of the length direction of the positive electrode sheet. By regulating the angle between the center line of the corrugation and the length direction of the positive electrode sheet within the above range, it is beneficial for the electrolyte to infiltrate and diffuse faster on the positive electrode sheet, and the positive electrode sheet has more liquid retention. In this way, the infiltration time of the electrolyte on the positive electrode sheet is shortened, which is beneficial to improving the performance of the secondary battery, such as cycle performance, rate performance, and safety performance. As a result, on the basis of improving the process excellence rate of the positive electrode sheet, the infiltration time of the electrolyte on the positive electrode sheet is further shortened, and the safety performance of the secondary battery after cycling is further improved.

[0047] The present application has no particular restrictions on the positive electrode current collector, as long as the purpose of the present application can be achieved. For example, the positive electrode current collector may include aluminum foil or aluminum alloy foil, etc. The positive electrode active material layer of the present application includes a positive electrode active material. The present application has no particular restrictions on the type of positive electrode active material, as long as the purpose of the present application can be achieved. For example, the positive electrode active material may include at least one of lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium iron phosphate, lithium-rich manganese-based materials, lithium cobalt oxide, lithium manganese oxide, lithium iron manganese phosphate or lithium titanate, etc. In the present application, the positive electrode active material may also include non-metallic elements, which may include at least one of fluorine, phosphorus, boron, chlorine, silicon or sulfur, which can further improve the stability of the positive electrode active material. In the present application, there is no particular restriction on the thickness of the positive electrode current collector and the positive electrode active material layer, as long as the purpose of the present application can be achieved. For example, the thickness of the positive electrode current collector is 5μm to 20μm. The thickness of the single-layer positive electrode active material layer is 30μm to 80μm. Optionally, the positive electrode active material layer may also include at least one of a positive electrode conductor or a positive electrode binder. The present application does not particularly limit the types of positive electrode conductors and positive electrode binders in the positive electrode active material layer, as long as the purpose of the present application can be achieved. The present application does not particularly limit the mass ratio of the positive electrode active material, the positive electrode conductor, and the positive electrode binder in the positive electrode active material layer. Those skilled in the art can choose according to actual needs, as long as the purpose of the present application can be achieved. For example, the mass ratio of the positive electrode active material, the positive electrode conductor, and the positive electrode binder in the positive electrode active material layer is (97.5~97.9):(0.8~1.7):(1.0~2.0).

[0048] The present application does not particularly limit the method for preparing the positive electrode sheet, as long as the object of the present application can be achieved. For example, in one embodiment, the method for preparing the positive electrode sheet includes but is not limited to the following steps: (1) Coating the positive electrode slurry on one surface of the positive electrode current collector, and drying to form a positive electrode active material layer; (2) Repeating step (1) on the other surface of the positive electrode current collector, and obtaining the positive electrode sheet with the positive electrode active material layer provided on both sides after cold pressing and slitting; (3) Performing corrugation treatment on the edge region of one side or both sides of the positive electrode sheet. The present application does not particularly limit the solid content of the positive electrode slurry, as long as the object of the present application can be achieved. For example, the solid content of the positive electrode slurry is 50 wt% to 80 wt%. The present application does not particularly limit the manner of corrugation treatment, as long as the object of the present application can be achieved. For example, the corrugation treatment can be performed by means of gradient rolling.

[0049] The second aspect of the present application provides a secondary battery, which includes the positive electrode sheet described in any of the foregoing embodiments. Therefore, the secondary battery has good safety performance, rate performance, and cycle performance.

[0050] In one embodiment of the present application, the secondary battery of the present application further includes a negative electrode sheet. The present application does not particularly limit the negative electrode sheet, as long as the object of the present application can be achieved. The negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer. The negative electrode active material layer is provided on one surface or two surfaces of the negative electrode current collector. The above "surface" can be a partial surface of the negative electrode current collector or the entire surface of the negative electrode current collector. The present application does not particularly limit the negative electrode current collector, as long as the object of the present application can be achieved. For example, the negative electrode current collector can include copper foil, copper alloy foil, nickel foil, stainless steel foil, titanium foil, nickel foam, or copper foam, etc. The negative electrode active material layer of the present application contains a negative electrode active material. The present application does not particularly limit the type of the negative electrode active material, as long as the object of the present application can be achieved. For example, the negative electrode active material can include natural graphite, artificial graphite, mesocarbon microbeads (MCMB), hard carbon, soft carbon, silicon, silicon-carbon composite, SiO x (0 < x < 2), Li-Sn alloy, Li-Sn-O alloy, Sn, SnO, SnO 2 、spinel-structured lithium titanate Li 4 Ti 5 O 12, Li-Al alloy or metallic lithium. In the present application, there is no particular restriction on the thickness of the negative electrode current collector and the negative electrode active material layer, as long as the purpose of the present application can be achieved. For example, the thickness of the negative electrode current collector is 6μm to 10μm, and the thickness of the negative electrode active material layer is 30μm to 130μm. Optionally, the negative electrode active material layer may also include at least one of a negative electrode conductor, a dispersant or a negative electrode binder. The present application does not particularly limit the types of negative electrode conductors, dispersants and negative electrode binders in the negative electrode active material layer, as long as the purpose of the present application can be achieved. The present application does not particularly limit the mass ratio of negative electrode active materials, negative electrode conductors, dispersants and negative electrode binders in the negative electrode active material layer, as long as the purpose of the present application can be achieved. For example, the mass ratio of negative electrode active materials, negative electrode conductors, dispersants and negative electrode binders in the negative electrode active material layer is (97~98):(0.5~1.5):(0~1.5):(1.0~1.9).

[0051] In one embodiment of the present application, the secondary battery of the present application further includes a diaphragm, which is disposed between the positive electrode sheet and the negative electrode sheet. The present application has no particular restrictions on the diaphragm, as long as the purpose of the present application can be achieved. For example, the material of the diaphragm may include, but is not limited to, at least one of polyethylene (PE), polypropylene (PP)-based polyolefins (PO), polyesters (e.g., polyethylene terephthalate (PET) films), cellulose, polyimide (PI), polyamide (PA), spandex or aramid. The type of diaphragm may include at least one of a woven membrane, a non-woven membrane, a microporous membrane, a composite membrane, a rolled membrane or a spun membrane. The present application has no particular restrictions on the thickness of the diaphragm, as long as the purpose of the present application can be achieved.

[0052] In one embodiment of the present application, the secondary battery further comprises an electrolyte, and the electrolyte comprises a lithium salt and a non-aqueous solvent. The present application has no particular restrictions on the lithium salt and the non-aqueous solvent, as long as the purpose of the present application can be achieved. For example, the lithium salt can be selected from LiPF 6, because it can give high ionic conductivity and improve cycle characteristics. Lithium salts include but are not limited to at least one of lithium hexafluorophosphate, lithium difluorophosphate, lithium tetrafluoroborate, lithium hexafluoroarsenate, lithium perchlorate, lithium bisfluorosulfonyl imide, lithium bistrifluoromethanesulfonyl imide, lithium bisoxalate borate or lithium difluorooxalate borate. For example, the non-aqueous solvent may be at least one of a carbonate compound, a carboxylate compound, an ether compound or other organic solvents. The above-mentioned carbonate compound may be at least one of a chain carbonate compound, a cyclic carbonate compound or a fluorocarbonate compound. The above-mentioned chain carbonate compound may include but is not limited to at least one of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC) or methyl ethyl carbonate (MEC). The cyclic carbonate compound may include but is not limited to at least one of ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC) or vinyl ethylene carbonate (VEC). The fluorinated carbonate compound may include, but is not limited to, at least one of fluoroethylene carbonate (FEC), 1,2-difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate, or trifluoromethylethylene carbonate. The above-mentioned carboxylate compound may include, but is not limited to, at least one of methyl formate, methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, decalactone, valerolactone, mevalonolactone, or caprolactone. The above-mentioned ether compound may include but is not limited to at least one of dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, 1,2-dimethoxyethane, 1,2-diethoxyethane, ethoxymethoxyethane, 2-methyltetrahydrofuran or tetrahydrofuran. The above-mentioned other organic solvents may include but are not limited to at least one of dimethyl sulfoxide, 1,2-dioxolane, cyclopentane, methyl cyclopentane, 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, formamide, dimethylformamide, acetonitrile, trimethyl phosphate, triethyl phosphate, trioctyl phosphate or phosphate.

[0053] In one embodiment of the present application, the secondary battery further comprises a packaging bag, wherein the positive electrode sheet, the separator, the negative electrode sheet and the electrolyte are contained in the packaging bag. The present application has no particular limitation on the type and shape of the packaging bag, as long as the purpose of the present application can be achieved.

[0054] The secondary battery of the present application is not particularly limited, and may include any device that undergoes an electrochemical reaction. For example, the secondary battery may include, but is not limited to: a lithium metal secondary battery, a lithium ion secondary battery (lithium ion battery), a lithium polymer secondary battery, or a lithium ion polymer secondary battery.

[0055] The present application does not particularly limit the preparation method of the secondary battery, and any preparation method known in the art can be selected as long as the purpose of the present application can be achieved. For example, the preparation method of the secondary battery includes but is not limited to the following steps: stacking the separator, the positive electrode sheet, the separator and the negative electrode sheet in order, and winding, folding and other operations as needed to obtain an electrode assembly with a wound structure, placing the electrode assembly in a packaging bag, injecting the electrolyte into the packaging bag and sealing it to obtain a secondary battery.

[0056] The third aspect of the present application provides an electronic device, which comprises the secondary battery described in any one of the above embodiments. Therefore, the electronic device has good performance.

[0057] The electronic device of the present application is not particularly limited, and it can be any electronic device known in the prior art. For example, the electronic device can include, but is not limited to: a laptop computer, a pen-input computer, a mobile computer, an electronic book player, a portable phone, a portable fax machine, a portable copier, a portable printer, a head-mounted stereo headset, a video recorder, an LCD television, a portable cleaner, a portable CD player, a mini-disc, a transceiver, an electronic notepad, a calculator, a memory card, a portable recorder, a radio, a backup power supply, a motor, a car, a motorcycle, a power-assisted bicycle, a bicycle, a lighting fixture, a toy, a game console, a clock, an electric tool, a flashlight, a camera, a large household battery, and a lithium-ion capacitor.

[0058] Example

[0059] Hereinafter, the embodiments of the present application will be described in more detail with reference to Examples and Comparative Examples. Various tests and evaluations were performed according to the following methods.

[0060] Test methods and equipment:

[0061] Test of process quality of positive electrode:

[0062] (1) Take a number of rolls of positive electrode sheets prepared in each embodiment and comparative example, a total of N rolls (N ≥ 1000);

[0063] (2) Take enough corresponding separators and negative electrode sheets of each embodiment and comparative example, the number of which is much greater than N;

[0064] (3) Assembling and producing the lithium-ion batteries according to the winding method of each embodiment and comparative example;

[0065] (4) Record the total scrap quantity M of positive electrode sheets during the production process;

[0066] (5) Process excellence rate of positive electrode (%) = (1-M / N) × 100%.

[0067] Test of electrolyte wetting time on positive electrode:

[0068] (1) The electrode assembly assembled with the positive electrode sheets to be tested in each embodiment and comparative example is placed in an aluminum-plastic film packaging bag through a top and side sealing process, and then vacuum-baked at 80° C. for 4 hours to remove moisture;

[0069] (2) Inject 5.95 g of electrolyte into the packaging bag containing the electrode assembly from the unsealed side of the packaging bag;

[0070] (3) Stand still at 60℃ for a period of time t, where the values ​​of t are 0.5h, 1h, 2h, 4h, 6h, 8h, 10h, 12h, 16h, and 24h;

[0071] (4) Charge the lithium-ion batteries at different rest times to 4.5V at 0.5C;

[0072] (5) Take the lithium-ion batteries charged at different time periods, disassemble them, and observe whether there are black spots on the negative electrode in the center area of ​​the lithium-ion battery to determine whether there is electrolyte deficiency in the center area;

[0073] (6) The minimum static time without black spots in the central area is recorded as the wetting time of the positive electrode.

[0074] Electrical performance and safety performance tests:

[0075] The lithium-ion batteries prepared in the examples and comparative examples were placed in a 25°C constant temperature test box and left to stand for 30 minutes to allow the lithium-ion batteries to reach a constant temperature. They were charged to 4.5V at a constant current of 0.5C, charged to a current of 0.025C at a constant voltage of 4.5V, left to stand for 5 minutes, and discharged to 3.0V at a constant current of 0.5C, which was recorded as the initial discharge capacity C. 0 Repeat this procedure for 800 cycles and record the discharge capacity C after 800 cycles. 1 , calculate the capacity retention rate of lithium-ion batteries after 800 cycles, cycle capacity retention rate (%) = C 1 / C 0 ×100%. At the same time, the lithium-ion battery after the cycle was fully charged (charged to 4.5V at a constant current of 0.5C) and disassembled to analyze and confirm the interface conditions in the later stage of the cycle and the actual conditions of the positive electrode current collectors in each layer, and confirm the differences.

[0076] The electrical performance of lithium-ion batteries is characterized by capacity retention rate and interface conditions. Specifically, if there is no abnormality in the interface and the capacity retention rate is higher, the electrical performance of the lithium-ion battery is better; if there is an abnormality in the interface and the capacity retention rate is lower, the electrical performance of the lithium-ion battery is worse. Among them, "interface condition" refers to the condition of the surface of the negative electrode after the lithium-ion battery is disassembled under full charge after cycling; "no abnormality in the interface" means that there are no black spots, lithium deposition, purple spots and other phenomena on the surface of the negative electrode; "abnormality in the interface" means that at least one of the following phenomena, such as black spots, lithium deposition or purple spots, appears on the surface of the negative electrode.

[0077] The actual conditions of the positive electrode current collectors at each layer are used to characterize the safety performance of the lithium-ion battery. Specifically, the actual conditions of the positive electrode current collectors refer to whether the positive electrode current collectors have cracks or breaks.

[0078] Example 1-1

[0079] <Preparation of positive electrode sheet>

[0080] The positive electrode active material is lithium cobalt oxide, the positive electrode conductive agent is acetylene black, and the positive electrode binder is polyvinylidene fluoride (PVDF, with a weight average molecular weight of 5×10 5 ) are mixed in a mass ratio of 96:2:2, N-methylpyrrolidone (NMP) is added as a solvent, and stirred under the action of a vacuum mixer until the solid content is 75wt% and the system is uniform. The positive electrode slurry is evenly coated on one surface of the positive electrode current collector aluminum foil with a thickness of 8μm, and dried at 90°C to obtain a positive electrode sheet with a single-sided positive electrode active material layer (thickness 60μm). Thereafter, the above steps are repeated on the other surface of the aluminum foil to obtain a positive electrode sheet with a double-sided positive electrode active material layer. After cold pressing and slitting, a positive electrode sheet with a specification of 74mm×888mm is obtained for standby use. Among them, the positive electrode sheet includes a double-sided area provided with a double-layer positive electrode active material layer and a single-sided area provided with a single-layer positive electrode active material layer. Along the length direction of the positive electrode sheet, the length L of the double-sided area 1 =633mm, the length of the single-sided area is 162mm, and the length of the empty foil area is 93mm. Along the width of the positive electrode sheet, the edge area on one side of the positive electrode sheet is subjected to a single-side corrugation process by a gradual rolling method from the edge to the inside, forming multiple corrugations. Along the length direction of the positive electrode sheet, the area with corrugations is the first area, and the length of the first area is L 2 =L 1 Among them, the width of the corrugation W 2 =12mm, the maximum depth of the corrugation D=10μm, the angle θ between the center line of the corrugation and the length direction of the positive electrode sheet is 90°, and the spacing σ between two adjacent corrugations is 7mm.

[0081] <Preparation of negative electrode sheet>

[0082] The negative electrode active material artificial graphite, the negative electrode conductive agent acetylene black, and the negative electrode binder styrene butadiene rubber (SBR, weight average molecular weight 5×10 6 ), dispersant carboxymethyl cellulose (CMC) are mixed in a mass ratio of 96:2:1:1, and then deionized water is added as a solvent, and stirred under the action of a vacuum mixer until the solid content is 50wt% and the system is uniform. The negative electrode slurry is evenly coated on one surface of a negative electrode current collector copper foil with a thickness of 6μm, and dried at 90°C to obtain a negative electrode sheet with a single-sided negative electrode active material layer (thickness 130μm). After that, the above steps are repeated on the other surface of the copper foil to obtain a negative electrode sheet with a double-sided negative electrode active material layer. After cold pressing and slitting, a negative electrode sheet with a specification of 76mm×873mm is obtained for standby use, wherein the double-sided area length of the negative electrode sheet is 640mm, the single-sided area length is 158mm, and the empty foil area length is 75mm.

[0083] <Preparation of Separator>

[0084] The substrate of the diaphragm is a polyethylene (PE) film with a thickness of 8μm and a width of 78mm. An alumina ceramic coating with a thickness of 4μm is coated on each of the two surfaces of the substrate along its thickness direction, and then 2.5mg of a binder polyvinylidene fluoride is coated on each of the two surfaces of the ceramic coating along its thickness direction. The diaphragm is obtained by drying.

[0085] <Preparation of Electrolyte>

[0086] In a dry argon atmosphere, organic solvents ethylene carbonate, ethyl methyl carbonate and diethyl carbonate were mixed in a mass ratio of 30:50:20 to obtain an organic solution, and then lithium salt lithium hexafluorophosphate was added to the organic solvent to dissolve and mix evenly to obtain an electrolyte with a lithium salt concentration of 1.15 mol / L.

[0087] <Preparation of lithium-ion batteries>

[0088] The prepared separator, positive electrode sheet, separator and negative electrode sheet are stacked in order and wound to obtain an electrode assembly. The electrode assembly is placed in an aluminum-plastic film packaging bag, and after drying, an electrolyte is injected, and a lithium-ion battery is obtained through vacuum packaging, standing, formation, degassing, trimming and other processes.

[0089] Example 1-2 to Example 1-6

[0090] Except for adjusting the parameters according to Table 1, the rest is the same as Example 1-1.

[0091] Examples 1-7

[0092] Except that the specifications of the positive electrode sheet in <Preparation of Positive Electrode Sheet> are adjusted to 100mm×888mm and the specifications of the negative electrode sheet in <Preparation of Negative Electrode Sheet> are adjusted to 102mm×873mm, the rest are the same as Example 1-5.

[0093] Examples 1-8

[0094] Except that the specifications of the positive electrode sheet in <Preparation of Positive Electrode Sheet> are adjusted to 30mm×888mm and the specifications of the negative electrode sheet in <Preparation of Negative Electrode Sheet> are adjusted to 32mm×873mm, the rest are the same as Example 1-2.

[0095] Examples 1-9

[0096] Except for adjusting the parameters according to Table 1, the rest is the same as Example 1-8.

[0097] Examples 1-10

[0098] Except that the specifications of the positive electrode sheet in <Preparation of Positive Electrode Sheet> are adjusted to 150mm×888mm and the specifications of the negative electrode sheet in <Preparation of Negative Electrode Sheet> are adjusted to 152mm×873mm, the rest are the same as Example 1-7.

[0099] Embodiment 1-11

[0100] Except that the specifications of the positive electrode sheet in <Preparation of Positive Electrode Sheet> are adjusted to 120mm×888mm and the specifications of the negative electrode sheet in <Preparation of Negative Electrode Sheet> are adjusted to 122mm×873mm, the rest are the same as Example 1-7.

[0101] Examples 1-12

[0102] Except that the specifications of the positive electrode sheet in <Preparation of Positive Electrode Sheet> are adjusted to 130 mm×888 mm and the specifications of the negative electrode sheet in <Preparation of Negative Electrode Sheet> are adjusted to 132 mm×873 mm, the rest are the same as Example 1-7.

[0103] Examples 1-13

[0104] <Preparation of positive electrode sheet>

[0105] The positive electrode active material is lithium cobalt oxide, the positive electrode conductive agent is acetylene black, and the positive electrode binder is polyvinylidene fluoride (PVDF, with a weight average molecular weight of 5×10 5) are mixed in a mass ratio of 96:2:2, N-methylpyrrolidone (NMP) is added as a solvent, and stirred under the action of a vacuum mixer until the solid content is 75wt% and the system is uniform. The positive electrode slurry is evenly coated on one surface of the positive electrode current collector aluminum foil with a thickness of 8μm, and dried at 90°C to obtain a positive electrode sheet with a single-sided positive electrode active material layer (thickness 60μm). Thereafter, the above steps are repeated on the other surface of the aluminum foil to obtain a positive electrode sheet with a double-sided positive electrode active material layer. After cold pressing and slitting, a positive electrode sheet with a specification of 74mm×888mm is obtained for standby use. Among them, the positive electrode sheet includes a double-sided area with a double-layer positive electrode active material layer, a single-sided area with a single-layer positive electrode active material layer, and an empty foil area without a positive electrode active material layer. Along the length direction of the positive electrode sheet, the length L of the double-sided area 1 =633mm, the length of the single-sided area is 162mm, and the length of the empty foil area is 93mm. Along the width of the positive electrode sheet, the edge areas on both sides of the positive electrode sheet are subjected to double-sided corrugation processing by gradual rolling from the edge to the inside, forming multiple corrugations. Along the length direction of the positive electrode sheet, the area with corrugations is the second area, and the length of the second area is L 3 =L 1 Among them, the width of the corrugation W 2 =3mm, the maximum depth of the corrugation D=10μm, the angle θ between the center line of the corrugation and the length direction of the positive electrode sheet is 90°, and the spacing σ between two adjacent corrugations is 7mm.

[0106] The rest is the same as Example 1-1.

[0107] Example 1-14 to Example 1-21

[0108] Except for adjusting the relevant parameters according to Table 1, the rest is the same as Example 1-13.

[0109] Example 1-22 to Example 1-28

[0110] Except for adjusting the relevant parameters according to Table 1, the rest is the same as Example 1-1.

[0111] Example 1-29 to Example 1-35

[0112] Except for adjusting the relevant parameters according to Table 1, the rest is the same as Example 1-13.

[0113] Example 1-36 and Example 1-37

[0114] Except for adjusting the relevant parameters according to Table 1, the rest is the same as Example 1-1.

[0115] Example 2-1 to Example 2-6

[0116] Except for adjusting the distance between two adjacent corrugations according to Table 2, the rest is the same as Example 1-15.

[0117] Example 2-7 to Example 2-10

[0118] Except for adjusting the angle between the center line of the corrugation and the length direction of the positive electrode sheet according to Table 2, the rest is the same as Example 1-15.

[0119] Comparative Example 1 and Comparative Example 2

[0120] Except for adjusting the relevant parameters according to Table 1, the rest is the same as Example 1-1.

[0121] Comparative Example 3

[0122] Except that the specifications of the positive electrode sheet in <Preparation of positive electrode sheet> are adjusted to 160mm×888mm and the specifications of the negative electrode sheet in <Preparation of negative electrode sheet> are adjusted to 162mm×873mm, the rest are the same as Example 1-1.

[0123] Comparative Example 4

[0124] Except for adjusting the relevant parameters according to Table 1, the rest is the same as Example 1-1.

[0125] Comparative Example 5

[0126] Except that the specifications of the positive electrode sheet in <Preparation of positive electrode sheet> are adjusted to 20mm×888mm and the specifications of the negative electrode sheet in <Preparation of negative electrode sheet> are adjusted to 22mm×873mm, the rest are the same as Example 1-1.

[0127] Comparative Example 6

[0128] Except for adjusting relevant parameters according to Table 1, the rest is the same as Comparative Example 3.

[0129] Comparative Example 7

[0130] Except for adjusting relevant parameters according to Table 1, the rest is the same as Comparative Example 5.

[0131] Comparative Example 8 and Comparative Example 9

[0132] Except for adjusting relevant parameters according to Table 1, the rest is the same as Example 1-15.

[0133] Comparative Example 10

[0134] Except that the specifications of the positive electrode sheet in <Preparation of Positive Electrode Sheet> are adjusted to 160mm×888mm and the specifications of the negative electrode sheet in <Preparation of Negative Electrode Sheet> are adjusted to 162mm×873mm, the rest are the same as Example 1-15.

[0135] Comparative Example 11

[0136] Except for adjusting relevant parameters according to Table 1, the rest is the same as Example 1-15.

[0137] Comparative Example 12

[0138] Except that the specifications of the positive electrode sheet in <Preparation of Positive Electrode Sheet> are adjusted to 20mm×888mm and the specifications of the negative electrode sheet in <Preparation of Negative Electrode Sheet> are adjusted to 22mm×873mm, the rest are the same as Example 1-15.

[0139] Comparative Example 13

[0140] Except for adjusting the relevant parameters according to Table 1, the rest is the same as Comparative Example 10.

[0141] Comparative Example 14

[0142] Except for adjusting the relevant parameters according to Table 1, the rest is the same as Comparative Example 12.

[0143] The preparation parameters and performance parameters of each embodiment and comparative example are shown in Table 1 and Table 2.

[0144] Table 1

[0145] Note: “\” in Table 1 means there is no corresponding parameter.

[0146] It can be seen from Examples 1-1 to 1-37 and Comparative Examples 1 to 14 that the positive electrode sheet width W of the embodiments of the present application is 1 Meet 30mm≤W 1When the positive electrode sheet is ≤150mm, a plurality of corrugations are provided on the edge area on one side or both sides along the width direction of the positive electrode sheet, and the maximum depth D of the corrugations satisfies 0.1μm≤D≤100μm, the positive electrode sheet has a good process excellence rate, and the electrolyte has a short infiltration time on the positive electrode sheet. The positive electrode sheet of the embodiment is applied to a secondary battery, and the secondary battery has a higher capacity retention rate after cycling, no abnormal interface conditions, and no fracture of the positive electrode collector, indicating that the secondary battery of the embodiment of the present application has improved electrical performance and safety performance after cycling based on the good process excellence rate of the positive electrode sheet and the short infiltration time of the electrolyte on the positive electrode sheet. However, the width of the positive electrode plate of the comparative example is not within the scope of the present application, the positive electrode plate is not provided with the corrugations of the present application or the maximum depth D of the corrugations is not within the scope of the present application, the capacity retention rate of the secondary battery of the comparative example after cycling is lower, black spots appear on the interface, and cracks or fractures appear on some positive electrode current collectors, indicating that the secondary battery of the comparative example cannot take into account the process excellence rate of the positive electrode plate, the infiltration time of the electrolyte on the positive electrode plate, and its electrical properties and safety performance.

[0147] The width of the corrugation W 2 It usually affects the process quality rate of the positive electrode sheet, the infiltration time of the electrolyte on the positive electrode sheet, and the electrical performance and safety performance of the secondary battery after cycling. From Examples 1-1 to 1-19, and Examples 1-36 to 1-37, it can be seen that the width W of the corrugation is selected. 2 The positive electrode plate within the scope of the present application has a higher process efficiency and a shorter electrolyte infiltration time, and the secondary battery using the positive electrode plate has good electrical performance and safety performance after cycling.

[0148] The length L of the second region 3 It usually affects the process quality rate of the positive electrode sheet, the infiltration time of the electrolyte on the positive electrode sheet, and the electrical performance and safety performance of the secondary battery after cycling. It can be seen from Examples 1-15, 1-20 and 1-21 that the length L of the second region is selected 3 The positive electrode plate within the scope of the present application has a higher process efficiency and a shorter electrolyte infiltration time, and the secondary battery using the positive electrode plate has good electrical performance and safety performance after cycling.

[0149] The maximum depth D of the corrugation usually affects the process excellence of the positive electrode sheet, the electrolyte infiltration time on the positive electrode sheet, and the electrical performance and safety performance of the secondary battery after cycling. It can be seen from Examples 1-1 and 1-22 to 1-28, 1-15 and 1-29 to 1-37 that the positive electrode sheet with the maximum depth D of the corrugation within the scope of the present application has a higher process excellence rate, a shorter electrolyte infiltration time, and the secondary battery using the positive electrode sheet has good electrical performance and safety performance after cycling.

[0150] Table 2

[0151] The spacing σ of the corrugations usually affects the process excellence of the positive electrode sheet, the electrolyte infiltration time on the positive electrode sheet, and the electrical performance and safety performance of the secondary battery after cycling. It can be seen from Examples 1-15 and 2-1 to 2-6 that the positive electrode sheet with the corrugation spacing σ within the range of the present application has a higher process excellence rate, a shorter electrolyte infiltration time, and the secondary battery using the positive electrode sheet has good electrical performance and safety performance after cycling.

[0152] The angle θ between the center line of the corrugation and the length direction of the positive electrode sheet usually affects the process excellence of the positive electrode sheet, the electrolyte infiltration time on the positive electrode sheet, and the electrical performance and safety performance of the secondary battery after cycling. From Examples 1-15, 2-7 to 2-10, it can be seen that the positive electrode sheet in which the angle θ between the center line of the corrugation and the length direction of the positive electrode sheet is within the range of the present application has a higher process excellence rate, a shorter electrolyte infiltration time, and the secondary battery using the positive electrode sheet has good electrical performance and safety performance after cycling.

[0153] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0154] Each embodiment in this specification is described in a related manner, and the same or similar parts between the embodiments can be referenced to each other, and each embodiment focuses on the differences from other embodiments.

[0155] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application shall be included in the scope of protection of the present application.

Claims

1. A positive electrode sheet, comprising a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector, wherein the width of the positive electrode sheet is W1, 30 mm ≤ W1 ≤ 150 mm; Along the width direction of the positive electrode sheet, a plurality of corrugations are arranged in the edge region of at least one side of the positive electrode sheet, and the maximum depth of the corrugations is D, 0.1 μm≤D≤100 μm.

2. The positive electrode sheet according to claim 1, wherein: 0.5μm≤D≤20μm.

3. The positive electrode sheet according to claim 1, wherein: The depth of the corrugations gradually decreases from the edge of the positive electrode sheet to the inside to 0 μm.

4. The positive electrode sheet according to claim 1, wherein: The corrugation is arranged at an edge region on one side of the positive electrode sheet along the width direction of the positive electrode sheet, and the width of the corrugation is W2, and W1 and W2 satisfy: 5mm≤W2≤20mm and W2≤1 / 4W1.

5. The positive electrode sheet according to claim 4, wherein: Along the length direction of the positive electrode sheet, the positive electrode sheet includes a double-sided area provided with a double layer of the positive electrode active material layer, and the double-sided area includes a first area provided with the corrugations; The length of the double-sided area is L1, the length of the first area is L2, and L2=L1.

6. The positive electrode sheet according to claim 1, wherein: Along the width direction of the positive electrode sheet, the corrugations are respectively arranged at the edge regions on both sides of the positive electrode sheet, the width of the corrugations is W2, and W1 and W2 satisfy: 3mm≤W2≤20mm and W2≤1 / 3W1.

7. The positive electrode sheet according to claim 6, wherein: Along the length direction of the positive electrode sheet, the positive electrode sheet includes a double-sided region provided with a double layer of the positive electrode active material layer, and the double-sided region includes a second region provided with the corrugations; The length of the double-sided area is L1, the length of the second area is L3, and 1 / 3L1≤L3≤L1.

8. The positive electrode sheet according to claim 1, wherein: The distance between two adjacent corrugations is 3 mm to 20 mm.

9. The positive electrode sheet according to claim 1, wherein: The distance between two adjacent corrugations is 3 mm to 12 mm.

10. The positive electrode sheet according to claim 1, wherein: The angle between the center line of the corrugation and the length direction of the positive electrode sheet is 85° to 95°.

11. A secondary battery, wherein: The secondary battery comprises the positive electrode sheet according to any one of claims 1 to 10.

12. An electronic device, wherein: The electronic device includes the secondary battery according to claim 11.