Preparation method of methyl phenyl silicone resin
In the preparation process of methylphenyl silicone, solid acid catalyzed hydrolysis and polycondensation reactions are used to solve the complex problems of acid wastewater pollution and by-product treatment, and environmentally friendly and high-performance preparation of methylphenyl silicone is achieved.
Patent Information
- Application Number
- CN202510300250.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-03-14
- Publication Date
- 2025-06-03
AI Technical Summary
The existing preparation methods of methylphenyl silicone resins have problems such as acid wastewater pollution and complicated treatment of by-products, which affect environmental protection and product performance.
The methyl trimethoxysilane with the structural formula CH3Si(OCH3)3, the trimethylmethoxysilane with the structural formula (CH3)3SiOCH3, the diphenyldimethoxysilane with the structural formula (C6H5)2Si(OCH3)2, and the phenyltrimethoxysilane with the structural formula C6H5Si(OCH3)3 were hydrolyzed and polycondensed, and the solvent was added to obtain a methylphenyl silicone resin. Solid acid was used as a catalyst to avoid the generation of acidic wastewater.
It has achieved no acidic wastewater production, reduced environmental pollution, simplified treatment processes, improved product performance, and met green environmental protection requirements.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of silicone resins, and particularly relates to a method for preparing methylphenyl silicone resin. Background Art
[0002] As is well known, the largest use of solvent-based silicone resins is as high-temperature resistant materials such as high-temperature resistant coatings or insulating paints (see Chinese patent documents CN101255312A, CN101054496A, and CN102585696A, etc.). Methylphenyl silicone resin is one of the most representative types of solvent-based silicone resins, and is generally sold as a product with a solid content of 50%.
[0003] Currently, there are mainly two categories of silane monomers used for preparing methylphenyl silicone resin: methyl / phenyl chlorosilane monomers (see Chinese patent documents CN101508776A and CN105111440A) and methyl / phenyl alkoxysilane monomers (see Chinese patent documents CN1810858A, CN101875724A, and CN103755960A, etc.).
[0004] The hydrolysis of the former type of methyl / phenyl chlorosilane monomers will produce a large amount of acidic wastewater, which not only causes relatively large pollution and is not environmentally friendly, but also easily corrodes equipment. In particular, the performance of the prepared methylphenyl silicone resin is not good.
[0005] Although the latter type of methyl / phenyl alkoxysilane monomers solves the problem of acidic wastewater, if the by-products methanol / ethanol produced by hydrolysis are directly used as solvents, the polycondensation reaction temperature will be relatively low, affecting the molecular weight of the methylphenyl silicone resin. Therefore, usually, methanol / ethanol needs to be removed and then high-boiling solvents such as toluene and xylene are introduced for azeotropic reflux dehydration to obtain a high-molecular-weight silicone resin with practical value. This not only makes the operation cumbersome, but also there is still the problem that methanol / ethanol is harmful to the environment.
[0006] In summary, it is urgent to improve the existing method for preparing methylphenyl silicone resin. Summary of the Invention
[0007] (I) Technical Problems to be Solved
[0008] In view of the deficiencies in the prior art, the present invention provides a method for preparing methylphenyl silicone resin, which neither produces acidic wastewater, not only avoids spending a large amount of cost for treatment, but also can reduce the pollution to the natural environment, meeting the current requirements of green environmental protection. Secondly, it can effectively utilize by-products, has good product performance, and meets the market demand.
[0009] (II) Technical Solutions to be Adopted
[0010] To achieve the above object, the technical solution adopted by the present invention is as follows:
[0011] A preparation method of a methylphenyl silicone resin, which is prepared by hydrolyzing and polycondensing methyltrimethoxysilane with the structural formula CH 3 Si(OCH 3 ) 3 , trimethylmethoxysilane with the structural formula (CH 3 ) 3 SiOCH 3 , diphenyldimethoxysilane with the structural formula (C 6 H 5 ) 2 Si(OCH 3 ) 2 , and phenyltrimethoxysilane with the structural formula C 6 H 5 Si(OCH 3 ) 3 , and adding a solvent.
[0012] Preferably, the molar ratio of methyltrimethoxysilane with the structural formula CH 3 Si(OCH 3 ) 3 , trimethylmethoxysilane with the structural formula (CH 3 ) 3 SiOCH 3 , diphenyldimethoxysilane with the structural formula (C 6 H 5 ) 2 Si(OCH 3 ) 2 , and phenyltrimethoxysilane with the structural formula C 6 H 5 Si(OCH 3 ) 3 is 1:0.5 - 2:0.5 - 2:1 - 5, preferably 1:0.5:0.5:2.
[0013] Preferably, methyltrimethoxysilane with the structural formula CH 3 Si(OCH 3 ) 3 , trimethylmethoxysilane with the structural formula (CH 3 ) 3 SiOCH 3 , diphenyldimethoxysilane with the structural formula (C 6 H 5 ) 2 Si(OCH 3 ) 2 , and phenyltrimethoxysilane with the structural formula C 6 H5 Si(OCH 3 ) 3 The ratio of the total molar amount of phenyltrimethoxysilane to the molar amount of deionized water used in hydrolysis is 1:1.5 to 1:2.6, preferably 1:2.2.
[0014] Preferably, the catalyst used in the polycondensation reaction is an acidic catalyst, and the acidic catalyst is any one of hydrochloric acid, acetic acid, sulfuric acid, sulfonic acid, and solid acid, preferably solid acid.
[0015] Preferably, the hydrolysis reaction temperature is 20 to 70 °C, preferably 30 to 60 °C; the hydrolysis reaction time is 3 to 7 hours, preferably 4 to 6 hours.
[0016] Preferably, the polycondensation reaction temperature is 80 to 110 °C, preferably 100 to 110 °C; the polycondensation reaction time is 2 to 6 hours, preferably 3 to 5 hours.
[0017] Preferably, the neutralizing agent used in the hydrolysis is a basic neutralizing agent, and the base used in the basic neutralizing agent is any one of sodium hydroxide, sodium carbonate, potassium hydroxide, and sodium methoxide. Since the acidic catalyst selected for this reaction is a solid acid, there is no need to select a neutralizing agent, and only the solid acid needs to be filtered and recovered after the reaction.
[0018] Preferably, the solvent used is toluene.
[0019] (III) Technical effects to be achieved
[0020] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0021] First, the methylphenyl silicone resin of the present invention is prepared by hydrolysis and polycondensation reaction of siloxane using solid acid as a catalyst. This not only does not produce acidic wastewater, but also does not require neutralization. The recovered solid acid can be recycled, which is economical and environmentally friendly. It not only avoids spending a large amount of costs for treatment, but also can reduce the pollution to the natural environment, meeting the current requirements of green environmental protection. In particular, the prepared methylphenyl silicone resin has good performance and is more conducive to meeting the application requirements.
[0022] Second, the catalyst used in the reaction of the present invention is any one of hydrochloric acid, acetic acid, sulfuric acid, sulfonic acid, and solid acid, providing a large selection range.
[0023] Third, the raw material siloxane used in the present invention has high purity, with a content above 99.5%, and few impurities. The prepared methylphenyl organosilicon resin has good performance and is more conducive to meeting the application requirements. Specific embodiments
[0024] Obviously, based on the above content of the present invention, various other forms of modifications, substitutions or changes can be made without departing from the above basic technical idea of the present invention according to the common general technical knowledge and means in the art.
[0025] The above content of the present invention will be further described in detail below by way of specific embodiments. However, this should not be construed as limiting the scope of the above subject matter of the present invention to the following embodiments. All technologies implemented based on the above content of the present invention fall within the scope of the present invention.
[0026] A preparation method of a methylphenyl silicone resin, which is prepared by hydrolyzing and polycondensing methyltrimethoxysilane with the structural formula CH 3 Si(OCH 3 ) 3 , trimethylmethoxysilane with the structural formula (CH 3 ) 3 SiOCH 3 , diphenyldimethoxysilane with the structural formula (C 6 H 5 ) 2 Si(OCH 3 ) 2 , and phenyltrimethoxysilane with the structural formula C 6 H 5 Si(OCH 3 ) 3 , and adding a solvent. Adding a solvent is beneficial to obtaining a liquid product, which better meets the application requirements.
[0027] Among them, the molar ratio of methyltrimethoxysilane with the structural formula CH 3 Si(OCH 3 ) 3 , trimethylmethoxysilane with the structural formula (CH 3 ) 3 SiOCH 3 , diphenyldimethoxysilane with the structural formula (C 6 H 5 ) 2 Si(OCH 3 ) 2 , and phenyltrimethoxysilane with the structural formula C 6 H 5 Si(OCH 3 ) 3 is 1:0.5 - 2:0.5 - 2:1 - 5, preferably 1:0.5:0.5:2. Such a setting is more conducive to obtaining a good product.
[0028] Among them, methyltrimethoxysilane with the structural formula CH 3 Si(OCH 3) 3 methyltrimethoxysilane and the structural formula is (CH 3 ) 3 SiOCH 3 trimethylmethoxysilane, the structural formula is (C 6 H 5 ) 2 Si(OCH 3 ) 2 diphenyldimethoxysilane, the structural formula is C 6 H 5 Si(OCH 3 ) 3 phenyltrimethoxysilane, the ratio of the total molar amount of phenyltrimethoxysilane to the molar amount of deionized water used for hydrolysis is 1:1.5 to 1:2.6, preferably 1:2.2. Such a setting is more conducive to obtaining good products.
[0029] Among them, the catalyst used for the polycondensation reaction is an acidic catalyst. The acidic catalyst is any one of hydrochloric acid, acetic acid, sulfuric acid, sulfonic acid, and solid acid, preferably solid acid. Therefore, there is no need to select a neutralizing agent. After the reaction is completed, only the solid acid needs to be filtered and recovered, and the operation is also simpler and more convenient.
[0030] Among them, the hydrolysis reaction temperature is 20 - 70 °C, preferably 30 - 60 °C. Such a setting is more conducive to obtaining good products; the hydrolysis reaction time is 3 - 7 hours, preferably 4 - 6 hours. Such a setting is more conducive to obtaining good products.
[0031] Among them, the polycondensation reaction temperature is 80 - 110 °C, preferably 100 - 110 °C. Such a setting is more conducive to obtaining good products; the polycondensation reaction time is 2 - 6 hours, preferably 3 - 5 hours. Such a setting is more conducive to obtaining good products.
[0032] Among them, the neutralizing agent used for hydrolysis is a basic neutralizing agent. The base used for the basic neutralizing agent is any one of sodium hydroxide, sodium carbonate, potassium hydroxide, and sodium methoxide. Since the acidic catalyst selected for this reaction is a solid acid, there is no need to select a neutralizing agent. After the reaction is completed, only the solid acid needs to be filtered and recovered, and the operation is also simpler and more convenient.
[0033] Among them, the solvent used is toluene. Through good solubility, liquid products can be obtained, which is more conducive to meeting the application requirements.
[0034] Examples
[0035] The preparation method of the methylphenyl silicone resin in this embodiment is as follows: Put 245.2 g (1.8 mol) of methyltrimethoxysilane, 74.2 g (0.7 mol) of trimethylmethoxysilane, 238.0 g (1.2 mol) of phenyltrimethoxysilane, 154.4 g (0.6 mol) of diphenyldimethoxysilane, and 12.6 g of solid acid into a 1000 ml three-necked flask, and dropwise add 186.4 g (4.8 mol) of deionized water, which is dropped within 2 hours. Then stir at 50 ± 2 °C for 4 hours, distill at normal pressure until 72 °C to collect methanol. When the material in the flask becomes slightly viscous, add 800 g of toluene and distill until 115 °C to remove the residual methanol. Cool and filter to obtain a toluene solution of methylphenyl silicone resin with a solid content of 53-60%, and add toluene to adjust the content to 50 ± 0.5%, so as to obtain a liquid product (methylphenyl silicone resin) that meets the application requirements (requirements for use effects).
[0036] It should be noted that although the above embodiments have been described in this article, the patent protection scope of the present invention is not limited thereby. Therefore, based on the innovative concept of the present invention, changes and modifications made to the embodiments described in this article, or equivalent structural or equivalent process transformations made using the content of the specification and drawings of the present invention, and directly or indirectly applying the above technical solutions to other related technical fields are all included in the protection scope of the present invention patent.
Claims
1. A method for preparing a methylphenyl silicone resin, characterized in that The process is carried out according to the following steps: it is prepared by hydrolysis and polycondensation of methyltrimethoxysilane with the structural formula CH3Si(OCH3)3, trimethylmethoxysilane with the structural formula (CH3)3SiOCH3, diphenyldimethoxysilane with the structural formula (C6H5)2Si(OCH3)2, and phenyltrimethoxysilane with the structural formula C6H5Si(OCH3)3, and then adding a solvent.
2. The method for preparing a methylphenyl silicone resin according to claim 1, wherein: The molar ratio of the methyltrimethoxysilane with the structural formula CH3Si(OCH3)3, the trimethylmethoxysilane with the structural formula (CH3)3SiOCH3, the diphenyldimethoxysilane with the structural formula (C6H5)2Si(OCH3)2, and the phenyltrimethoxysilane with the structural formula C6H5Si(OCH3)3 is 1:0.5~2:0.5~2:1~5.
3. The method for preparing a methylphenyl silicone resin according to claim 1 or 2, characterized in that: The ratio of the total molar number of methyltrimethoxysilane with the structural formula CH3Si(OCH3)3, trimethylmethoxysilane with the structural formula (CH3)3SiOCH3, diphenyldimethoxysilane with the structural formula (C6H5)2Si(OCH3)2, and phenyltrimethoxysilane with the structural formula C6H5Si(OCH3)3 to the molar number of deionized water used for hydrolysis is 1:1.5 to 1:2.
6.
4. The method for preparing a methylphenyl silicone resin according to claim 1, wherein: The catalyst used in the polycondensation is an acidic catalyst, and the catalyst used in the acidic catalyst is any one of hydrochloric acid, acetic acid, sulfuric acid, sulfonic acid or solid acid.
5. The method for preparing a methylphenyl silicone resin according to claim 1, wherein: The neutralizing agent used in the hydrolysis is an alkaline neutralizing agent, and the alkali used in the alkaline neutralizing agent is any one of sodium hydroxide, sodium carbonate and potassium hydroxide.
6. The method for preparing a methylphenyl silicone resin according to claim 1, 2, 4 or 5, characterized in that: The hydrolysis reaction temperature is 20 to 70° C., and the hydrolysis reaction time is 3 to 7 hours.
7. The method for preparing a methylphenyl silicone resin according to claim 1, 2, 4 or 5, characterized in that: The polycondensation reaction temperature is 80 to 110° C., and the polycondensation reaction time is 2 to 6 hours.
8. The method for preparing a methylphenyl silicone resin according to claim 1, 2, 4 or 5, characterized in that: The solvent used is toluene.
Citation Information
Patent Citations
Method of producing organosilicon heat-resistant coating
CN101054496A
Solvent type organic silicon thermostable paint and production method thereof
CN101255312A
Method of preparing methyl phenyl polysiloxane
CN101508776A
Preparation method of phenyl silicone resin
CN101875724A
Methyl phenyl silicone resin base high-temperature-resistant coating and preparation method thereof
CN102585696A
Cited By
Preparation method of phenyltrimethoxysilane oligomer
CN121181896A
Protective coating for stone base material as well as preparation method and application of protective coating
CN121851809A