4D printing hydrogel material as well as preparation method and application thereof
The hydrogel materials prepared through 4D printing technology use copolymerization reaction and charged coordination technology to solve the problems of lithium salt leakage and moisture release inconvenient during the moisture absorption process of existing adsorbent materials, achieving efficient moisture capture and release, and improving atmospheric water collection performance.
Patent Information
- Application Number
- CN202510285563.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-03-11
- Publication Date
- 2025-06-13
AI Technical Summary
The loading method of LiCl in existing porous composite adsorption materials depends on physical force, resulting in leakage easily during the adsorption and desorption of water. The closed single-phase block material is not conducive to the release of moisture, resulting in insufficient stability and water collection performance.
Hydrogel materials were prepared by 4D printing technology, and N-isopropylacrylamide (NIPAM) and [2-(methacryloyloxy)ethyl]dimethyl-(3-sulfonate)ammonium hydroxide (DMAPS) were copolymerized, combining the polyelectrolyte effect of poly[2-(methacryloyloxy)ethyl]dimethyl-(3-sulfonate)ammonium hydroxide (PDMAPS), alleviating the salting out effect of hydrogel, and coordinating with lithium salt through the chargeability of the PDMAPS components, anchoring the lithium salt in the polymer network of the hydrogel.
The volume swelling of hydrogel materials during the hygroscopic process is achieved, with fast hygroscopic kinetics and ultra-high hygroscopic amount, excellent water storage and water collection ability, avoiding the problem of lithium salt leakage, and improving the atmospheric water collection performance.
Smart Images

Figure CN120137212A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of hydrogel materials, and particularly to a 4D printing hydrogel material, a preparation method thereof, and an application thereof. Background Art
[0002] In recent years, solar adsorption atmospheric water collection can effectively alleviate the problem of water resource shortage. It is not restricted by environmental climate and geographical conditions, directly captures water from the air, and the captured water can be released under sunlight irradiation, featuring green environmental protection and sustainability. So far, many kinds of adsorption materials with high water collection performance, fast kinetics, and high regeneration ability have been developed in the field of atmospheric water collection, such as covalent organic frameworks, hygroscopic organic liquids, and base composite materials. Among them, the hygroscopic saline hydrogel composite material, which is characterized by loading lithium chloride in the porous structure of the hydrogel, can effectively solve the problems of lithium chloride agglomeration and deliquescence, and shows good water collection performance, thus attracting more and more attention from researchers. However, the loading method of LiCl in these porous composite adsorption materials is through physical forces such as hydrogen bonds or van der Waals forces, resulting in the easy leakage of LiCl after adsorption and desorption of water, making the stability of the adsorption material relatively weak. In addition, these porous composite adsorption materials are all closed single-phase bulk materials, capturing water in the air starting from the outer layer of the bulk material. When the LiCl in the outer layer reaches saturation, the water adsorption rate will rapidly decline. Secondly, this closed single-phase bulk material is also not conducive to the release of water. Therefore, developing porous composite adsorption materials with high adsorption and desorption efficiency and long-term stability still poses a huge challenge. Summary of the Invention
[0003] Aiming at one or more technical problems existing in the prior art, the present invention provides a 4D printing hydrogel material, a preparation method thereof, and an application thereof. The 4D printing hydrogel material provided by the present invention can exhibit volume swelling during the moisture absorption process and has excellent water storage and water collection capabilities.
[0004] The present invention provides a preparation method of a 4D printing hydrogel material in the first aspect, and the preparation method includes:
[0005] S1. Performing a prepolymerization reaction on N-isopropylacrylamide under the action of a photoinitiator to obtain a prepolymer;
[0006] S2. Mixing the prepolymer, [2-(methacryloyloxy)ethyl]dimethyl-(3-sulfopropyl)ammonium hydroxide, and a crosslinking agent to obtain a printing slurry;
[0007] S3. Performing 3D photocuring printing using the printing slurry to obtain a hydrogel matrix with a porous structure;
[0008] S4. Immerse the hydrogel matrix in a lithium salt solution to obtain a 4D printed hydrogel material.
[0009] Preferably, before step S4, it further includes: immersing the hydrogel matrix in a pyrrole monomer solution for soaking treatment, and then performing oxidative polymerization in an oxidant solution.
[0010] Preferably, the mass ratio of N-isopropylacrylamide to the initiator is 1:0.005 - 0.01; preferably, the photoinitiator is lithium phenyl(2,4,6-trimethylbenzoyl)phosphate;
[0011] The mass ratio of N-isopropylacrylamide to water is 1:0.8 - 0.12.
[0012] The mass ratio of N-isopropylacrylamide to [2-(methacryloyloxy)ethyl]dimethyl-(3-sulfopropyl)ammonium hydroxide is 1:0.2 - 0.3; and / or
[0013] The mass ratio of N-isopropylacrylamide to the crosslinking agent is 1:0.05 - 0.08; preferably, the crosslinking agent is N,N'-methylenebisacrylamide.
[0014] Preferably, the prepolymerization reaction is carried out by irradiating with ultraviolet light at 20 - 30 °C for 1 - 3 min; and / or
[0015] During the photocuring printing process, the thickness of a single layer printing is 50 - 100 μm, and the time for single layer photocuring is 40 - 60 s.
[0016] Preferably, the lithium salt in the lithium salt solution accounts for 5 - 40 wt%, and the lithium salt is preferably lithium chloride; and / or
[0017] The soaking time is 12 - 24 h.
[0018] Preferably, the pyrrole monomer in the pyrrole monomer solution accounts for 2 - 3 wt%; and / or
[0019] The oxidant solution is FeCl 3 solution, preferably, FeCl 3 in the solution FeCl 3 accounts for 1 - 2 wt%.
[0020] Preferably, the soaking treatment time is 1 - 2 h; and / or
[0021] The oxidative polymerization time is 1 - 2 h.
[0022] Preferably, after soaking in the lithium salt solution, it further includes a drying step; the drying is at least one of freeze-drying and atmospheric drying.
[0023] In a second aspect, the present invention provides a 4D printing hydrogel material prepared by the preparation method described in the first aspect.
[0024] In a third aspect, the present invention provides an application of the 4D printing hydrogel material described in the second aspect, which is applied to the field of atmospheric water harvesting.
[0025] Compared with the prior art, the present invention has at least the following beneficial effects:
[0026] First, the present invention pre-polymerizes N-isopropylacrylamide (NIPAM), and mixes the prepolymer, [2-(methacryloyloxy)ethyl]dimethyl-(3-sulfopropyl)ammonium hydroxide (DMAPS) and a cross-linking agent to obtain a printing slurry; then, through photocuring 3D printing, NIPAM and DMAPS are copolymerized, and the anti-polyelectrolyte effect of poly[2-(methacryloyloxy)ethyl]dimethyl-(3-sulfopropyl)ammonium hydroxide (PDMAPS) is used to alleviate the salting-out effect of the hydrogel, so that the copolymer hydrogel can swell during the moisture absorption process, realizing excellent water storage and water harvesting capabilities; at the same time, the macroscopic structure of the hydrogel matrix is designed through 3D printing to enhance the kinetics of water capture and greatly improve the atmospheric water harvesting performance; finally, through the coordination of the charged property of the PDMAPS component and the lithium salt, the lithium salt is anchored in the polymer network of the hydrogel to solve the problem that the lithium salt is prone to leakage during the moisture absorption process of the existing adsorption materials. The 4D printing hydrogel material provided by the present invention can undergo volume swelling during the moisture absorption process, has fast moisture absorption kinetics and ultra-high moisture absorption capacity, and has excellent water storage and water harvesting capabilities. Description of the Drawings
[0027] In order to more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the following will briefly introduce the drawings required for use in the description of the embodiments or the prior art. Obviously, the following drawings are some embodiments of the present invention. For those of ordinary skill in the art, without creative efforts, other drawings can also be obtained based on these drawings.
[0028] Figure 1 It is an infrared spectrum diagram of the 4D printing hydrogel material provided in Example 1 of the present invention;
[0029] Figure 2 It is a differential scanning calorimetry diagram of PNIPAM, PDMAPS and P(NIPAM-co-DMAPS);
[0030] Figure 3 It is a diagram of the atmospheric water harvesting performance test of the hydrogel materials provided in Example 1 and Comparative Examples 1-2 of the present invention at 90% humidity;
[0031] Figure 4 It is the test chart of the atmospheric water collection performance of the hydrogel material provided in Example 2 of the present invention under 90% humidity;
[0032] Figure 5 It is the test chart of the performance of the 4D printed hydrogel material provided in Example 2 of the present invention to release moisture under one-fold sunlight irradiation;
[0033] Figure 6 It is the comparison chart of the moisture absorption performance of the 4D printed hydrogel materials provided in Example 1 and Example 2 of the present invention. Detailed implementation manners
[0034] To make the objectives, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be described clearly and completely below. Apparently, the described embodiments are some, but not all, of the embodiments of the present invention. All other embodiments obtained by those of ordinary skill in the art based on the embodiments of the present invention without creative efforts shall fall within the protection scope of the present invention.
[0035] The present invention provides a preparation method of a 4D printed hydrogel material in the first aspect. The preparation method includes:
[0036] S1. Subject N-isopropylacrylamide to a prepolymerization reaction under the action of a photoinitiator to obtain a prepolymer;
[0037] S2. Mix the prepolymer, [2-(methacryloyloxy)ethyl]dimethyl-(3-sulfopropyl) ammonium hydroxide and a crosslinking agent to obtain a printing slurry;
[0038] S3. Perform 3D photocuring printing using the printing slurry to obtain a hydrogel matrix with a porous structure;
[0039] S4. Immerse the hydrogel matrix in a lithium salt solution to obtain a 4D printed hydrogel material.
[0040] The present invention first pre-polymerizes N-isopropylacrylamide (NIPAM), and mixes the prepolymer, [2-(methacryloyloxy)ethyl]dimethyl-(3-sulfopropyl) ammonium hydroxide (DMAPS) and a cross-linking agent to obtain a printing paste; then, through photocuring 3D printing, NIPAM and DMAPS are copolymerized, and the anti-polyelectrolyte effect of poly[2-(methacryloyloxy)ethyl]dimethyl-(3-sulfopropyl) ammonium hydroxide (PDMAPS) is used to alleviate the salting-out effect of the hydrogel, so that the copolymer hydrogel can swell during the moisture absorption process, achieving excellent water storage and water collection capabilities; at the same time, the macroscopic structure of the hydrogel matrix is designed by 3D printing to enhance the kinetics of water capture and greatly improve the atmospheric water collection performance; finally, through the coordination of the charged property of the PDMAPS component with the lithium salt, the lithium salt is anchored in the polymer network of the hydrogel to solve the problem of easy lithium salt leakage in the existing adsorption materials during the moisture absorption process. The 4D printing hydrogel material provided by the present invention can undergo volume swelling during the moisture absorption process, has fast moisture absorption kinetics and an ultra-high moisture absorption capacity, and has excellent water storage and water collection capabilities.
[0041] According to some preferred embodiments, before step S4, it further includes: soaking the hydrogel matrix in a pyrrole monomer solution, and then performing oxidative polymerization in an oxidant solution.
[0042] Before soaking the lithium salt, the present invention imparts photothermal conversion performance to the copolymer hydrogel by introducing polypyrrole into the hydrogel matrix with a porous structure, so that the hydrogel material can release the adsorbed moisture under light irradiation. The finally prepared hydrogel material exhibits excellent thermosensitive response under one-fold sunlight irradiation, can rapidly undergo structural contraction and rapidly release liquid water. The 4D printing hydrogel material provided by the present invention can undergo swelling during the moisture absorption process, has fast moisture absorption kinetics and an ultra-high moisture absorption capacity, can directly release liquid water during the water release process, realizes the collection of fresh water, avoids the high-energy consumption process of gas-liquid conversion, and has the advantages of environmental friendliness.
[0043] According to some preferred embodiments, the mass ratio of N-isopropylacrylamide to the initiator is 1:0.005 to 0.01; preferably, the photoinitiator is lithium phenyl(2,4,6-trimethylbenzoyl)phosphate.
[0044] According to some preferred embodiments, the mass ratio of N-isopropylacrylamide to water is 1:0.8 to 0.12.
[0045] According to some preferred embodiments, the mass ratio of N-isopropylacrylamide to [2-(methacryloyloxy)ethyl]dimethyl-(3-sulfopropyl) ammonium hydroxide is 1:0.2 to 0.3. In the present invention, the mass ratio of N-isopropylacrylamide to [2-(methacryloyloxy)ethyl]dimethyl-(3-sulfopropyl) ammonium hydroxide is controlled within the above range to ensure the structural strength and water collection performance of the hydrogel material. If the amount of [2-(methacryloyloxy)ethyl]dimethyl-(3-sulfopropyl) ammonium hydroxide is too small, there will be less lithium salt participating in coordination in the later stage, and the water collection performance of the final hydrogel material will be poor; if the amount of [2-(methacryloyloxy)ethyl]dimethyl-(3-sulfopropyl) ammonium hydroxide is too large, the strength of the hydrogel material will be weak, which is not conducive to the 3D printing forming structure of the hydrogel.
[0046] According to some preferred embodiments, the mass ratio of N-isopropylacrylamide to the crosslinking agent is 1:0.05 to 0.08; preferably, the crosslinking agent is N,N'-methylenebisacrylamide.
[0047] According to some preferred embodiments, the prepolymerization reaction is carried out by irradiating with ultraviolet light at 20 to 30 °C for 1 to 3 minutes.
[0048] In the present invention, by strictly controlling the content and temperature of N-isopropylacrylamide (PNIPAM) during the prepolymerization reaction, the subsequent copolymerization reaction can be ensured to proceed smoothly, and thus a hydrogel with better performance can be obtained; if the content of PNIPAM is too high, PNIPAM will aggregate and undergo a phase change during the reaction process, which is not conducive to the subsequent copolymerization reaction. If the temperature is too high, a phase change will also occur, causing the solution to change from transparent to a white emulsion, which is not conducive to the subsequent copolymerization reaction. It should be noted that before the prepolymerization of NIPAM, N 2 is introduced to remove the oxygen in the water in order to carry out the polymerization reaction.
[0049] In the present invention, poly-N-isopropylacrylamide (PNIPAM) with a certain molecular weight is formed by prepolymerization. The molecular weight of PNIPAM will affect the critical transition temperature (the temperature at which water is released) of the hydrogel material. If prepolymerization is not carried out, the number-average molecular weight of PNIPAM is small, and finally there is no obvious critical transition temperature for PNIPAM.
[0050] According to some preferred embodiments, during the photocuring printing process, the thickness of a single layer printing is 50 to 100 μm (for example, it can be 50 μm, 60 μm, 70 μm, 80 μm, 90 μm or 100 μm), and the photocuring time for a single layer is 40 to 60 s (for example, it can be 40 s, 50 s or 60 s).
[0051] The present invention constructs a 3D printing model, then slices the model, and sets the thickness of each layer and the exposure time of each layer. Through a large number of experiments, it is proved that the exposure time of photocuring printing needs to be reasonably set. If the exposure time is too short, the polymerization reaction will be incomplete and printing cannot be carried out. If the exposure time is too long, over-polymerization will occur, affecting the printing quality. Therefore, when the exposure time of photocuring 3D printing is controlled within the above range in the present invention, a 4D printed hydrogel can be obtained.
[0052] According to some preferred embodiments, the concentration of LiCl is 5-40 wt%. The inventors found that if the concentration of the LiCl solution is too small, the LiCl loading will be low, resulting in poor moisture absorption performance of the hydrogel material. If the concentration of the LiCl solution continues to increase, the swelling ratio of the hydrogel will decrease, resulting in a decrease in the LiCl loading and poor moisture absorption performance of the material. Therefore, the content of the lithium salt in the lithium salt solution is controlled within the above range in the present invention.
[0053] According to some preferred embodiments, the soaking time is 12-24 h.
[0054] According to some preferred embodiments, the pyrrole monomer accounts for 2-3 wt% in the pyrrole monomer solution. The inventors found that if the concentration of the pyrrole monomer solution is too large, the structure of the hydrogel will collapse. If the concentration of the pyrrole monomer solution is too small, the loading of polypyrrole is low, and the photothermal conversion effect of the hydrogel material is poor. Therefore, the content of the pyrrole monomer in the pyrrole monomer solution is controlled within the above range in the present invention.
[0055] According to some preferred embodiments, the oxidant solution is FeCl 3 solution. Preferably, FeCl 3 in the solution accounts for 1-2 wt%. 3
[0056] According to some preferred embodiments, the soaking treatment time is 1-2 h.
[0057] According to some preferred embodiments, the oxidation polymerization time is 1-2 h. The present invention does not specifically limit the oxidation polymerization time. When the hydrogel changes from transparent to black, it indicates that the polymerization is complete.
[0058] According to some preferred embodiments, after soaking in the lithium salt solution, a drying step is further included; the drying is at least one of freeze-drying and atmospheric drying.
[0059] The present invention provides a 4D printed hydrogel material in a second aspect, which is prepared by using the preparation method described in the first aspect.
[0060] According to some preferred embodiments, the 4D printed hydrogel material has a honeycomb structure.
[0061] In a third aspect, the present invention provides an application of the 4D printing hydrogel material described in the second aspect, which is applied to the field of atmospheric water harvesting.
[0062] In order to more clearly illustrate the technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with embodiments. The present invention does not specifically limit the sources of the various reagents used in the examples and comparative examples, and they can be directly purchased or synthesized by themselves.
[0063] Example 1
[0064] S1. Place 15 g of N-isopropylacrylamide (NIPAM) in a flask, add 150 mL of water, then introduce N 2 Remove the oxygen in the water, add 150 mg of lithium phenyl(2,4,6-trimethylbenzoyl)phosphate to the flask, stir and mix evenly, and then irradiate with ultraviolet light at 365 nm for 2 min at 25 °C to obtain a prepolymer (denoted as PNIPAM);
[0065] S2. Add 3.75 g of [2-(methacryloyloxy)ethyl]dimethyl-(3-sulfopropyl)ammonium hydroxide (DMAPS) and 0.8 g of N,N'-methylenebisacrylamide (BIS) to the prepolymer (PNIPAM), stir and mix evenly to obtain a printing slurry;
[0066] S3. Pour the obtained mixture into a stereolithography 3D printer for printing, design the printing model, set the thickness of a single layer of printing to 50 μm, and the time of a single layer of light irradiation to 50 s to obtain a hydrogel matrix with a honeycomb structure (denoted as P(NIPAM-co-DMAPS));
[0067] S4. Immerse the printed hydrogel matrix with a honeycomb structure in a LiCl solution (LiCl concentration is 10 wt%) for 24 h, and dry to remove moisture to obtain a 4D printing hydrogel material (denoted as P(NIPAM-co-DMAPS)-LiCl).
[0068] It can be seen from Figure 1 that in the infrared curve of the 4D printing hydrogel material prepared in Example 1, the presence of the -NH characteristic peak (at 1544 cm -1 in PNIPAM) can be seen in the infrared curve of P(NIPAM-co-DMAPS), indicating that NIPAM and DMAPS have successfully copolymerized. From the infrared curve of P(NIPAM-co-DMAPS)-LiCl, it can be seen that when P(NIPAM-co-DMAPS) coordinates with LiCl, the symmetric stretching vibration peak S=O corresponding to PDMAPS shifts from 1049 cm -1 to 1041 cm -1, indicating the successful coordination of PDMAPS with LiCl. Meanwhile, the peak at 1485 cm -1 is the peak of -N in PDMAPS + (CH 3 ) 2 — functional group, which becomes difficult to identify after coordination with Cl - , proving the existence of the coordination salt state.
[0069] From the differential scanning calorimetry (DSC) curve of Figure 2 , it can be seen that the lower critical solution temperature (LCST) of the pure PNIPAM hydrogel is about 34.2 °C, and the LCST of the P(NIPAM-co-DMAPS) copolymer hydrogel is 41.2 °C, indicating that there is still an LCST peak after copolymerization of the two, showing thermoresponsiveness.
[0070] Comparative Example 1
[0071] S1. Place 15 g of N-isopropylacrylamide (NIAPM) and 0.8 g of N,N'-methylenebisacrylamide (BIS) in a flask, add 150 mL of water, and then introduce N 2 to remove the oxygen in the water; then add 150 mg of lithium phenyl(2,4,6-trimethylbenzoyl)phosphate to the flask, stir and mix evenly, and then irradiate with ultraviolet light at 365 nm for 5 min at 25 °C to obtain a PNIAPM hydrogel;
[0072] S2. Immerse the PNIAPM hydrogel in a LiCl solution (LiCl concentration is 10 wt%) for 24 h, and then dry to remove the water to obtain a hydrogel material.
[0073] Comparative Example 2
[0074] S1. Place 15 g of N-isopropylacrylamide (NIAPM), 3.75 g of [2-(methacryloyloxy)ethyl]dimethyl-(3-sulfopropyl)ammonium hydroxide (DMAPS) and 0.8 g of N,N'-methylenebisacrylamide (BIS) in a flask, add 150 mL of water, and then introduce N 2 to remove the oxygen in the water; then add 150 mg of lithium phenyl(2,4,6-trimethylbenzoyl)phosphate to the flask, stir and mix evenly, and then irradiate with ultraviolet light at 365 nm for 5 min at 25 °C to obtain a copolymer hydrogel;
[0075] S2. Immerse the copolymer hydrogel in a LiCl solution (LiCl concentration is 10 wt%) for 24 h, and then dry to remove the water to obtain a hydrogel material.
[0076] Under the condition of 90% RH, the hygroscopic properties of the hydrogel materials of Example 1, Comparative Example 1 and Comparative Example 2 were tested. From Figure 3 It can be seen that there was no swelling phenomenon during the moisture absorption process of Comparative Example 1, and even volume shrinkage occurred after 12 hours of moisture absorption, indicating that the salting-out effect inhibited its moisture absorption performance. The moisture capture in the structure of Comparative Example 2 was limited to its surface, and the limited air adsorption interface severely restricted the capture efficiency, remaining translucent even after 12 hours of moisture absorption, which confirmed that once the surface LiCl reached saturation, the diffusion of water into the interior would be hindered, resulting in limited moisture absorption performance. In the honeycomb-structured hydrogel material of Example 1, the edges of each millimeter-sized hexagonal unit first became transparent during the moisture absorption process, which strongly proved that they could effectively collect moisture from the air. This structure of Example 1 not only greatly increased the speed of capturing moisture from the air but also significantly shortened the diffusion distance of water within the material. After 4 hours of moisture absorption, Example 1 changed from the original dry white state to a transparent state under humidity stimulation, indicating that water vapor in the air was quickly captured by the 4D-printed hydrogel material. Subsequently, the captured water vapor condensed into liquid water, quickly migrated into the hydrophilic polymer network structure, and underwent volume swelling to store moisture. The structural difference between the two hydrogel materials of Example 1 and Comparative Example 2 resulted in a swelling rate of up to 83% for the hydrogel material of Example 1 after moisture absorption, enabling it to accommodate more water and thus having superior moisture absorption capacity, while the swelling rate of the hydrogel material of Comparative Example 2 was only 25%.
[0077] Comparative Example 3
[0078] It was basically the same as Example 1, except that: in S2, the dosage of [2-(methacryloyloxy)ethyl]dimethyl-(3-sulfopropyl)ammonium hydroxide (DMAPS) was 1.5 g.
[0079] Since the dosage of [2-(methacryloyloxy)ethyl]dimethyl-(3-sulfopropyl)ammonium hydroxide was too small, there would be fewer lithium salts participating in coordination in the later stage, and the water collection performance of the final hydrogel material was poor.
[0080] Comparative Example 4
[0081] It was basically the same as Example 1, except that: in S2, the dosage of [2-(methacryloyloxy)ethyl]dimethyl-(3-sulfopropyl)ammonium hydroxide (DMAPS) was 6 g.
[0082] Since the dosage of [2-(methacryloyloxy)ethyl]dimethyl-(3-sulfopropyl)ammonium hydroxide was too large, the strength of the hydrogel material was weak, which was not conducive to the 3D printing and forming of the hydrogel.
[0083] Example 2
[0084] S1. Place 15 g of N-isopropylacrylamide (NIPAM) in a flask, add 150 mL of water, and then introduce N 2 Remove the oxygen in the water, add 150 mg of lithium phenyl(2,4,6-trimethylbenzoyl)phosphate to the flask, stir and mix evenly, and then irradiate with ultraviolet light at 365 nm for 2 min at 25 °C to obtain a prepolymer (PNIPAM);
[0085] S2. Add 3.75 g of [2-(methacryloyloxy)ethyl]dimethyl-(3-sulfopropyl)ammonium hydroxide (DMAPS) and 0.8 g of N,N'-methylenebisacrylamide (BIS) to the prepolymer (PNIPAM), stir and mix evenly to obtain a printing slurry;
[0086] S3. Pour the obtained mixture into a stereolithography 3D printer for printing, design a printing model, set the thickness of a single-layer printing to 50 μm, and the time of single-layer light irradiation to 50 s to obtain a hydrogel matrix with a honeycomb structure (denoted as P(NIPAM-co-DMAPS));
[0087] S4. Immerse the printed hydrogel matrix in a pyrrole monomer solution with a mass concentration of 2 wt% for 2 h, and then transfer it to a solution with a mass concentration of 1.5 wt% of FeCl 3 for oxidative polymerization. When the hydrogel matrix changes from transparent to black, it indicates that the polymerization is completed. Then soak it in water to remove the excess FeCl on the surface 3 to obtain an oxidized and polymerized hydrogel matrix (denoted as P(NIPAM-co-DMAPS)-PPy).
[0088] S5. Immerse the oxidized and polymerized hydrogel matrix in a LiCl solution (LiCl concentration is 10 wt%) for 24 h, and finally dry it to remove the moisture to obtain a 4D printing hydrogel material (denoted as P(NIPAM-co-DMAPS)-PPy-LiCl).
[0089] In this invention, under the condition of 90% humidity, the moisture absorption performance of the hydrogel material of Example 2 was tested. It can be seen from Figure 4 that there is no leakage problem during the moisture absorption process of the hydrogel material of Example 2, and the hydrogel will swell after moisture absorption. This is due to the anti-polyelectrolyte effect of PDMAPS, which inhibits the salting-out effect of the hydrogel, thus showing excellent atmospheric water collection performance.
[0090] It can be seen from Figure 5It can be seen that under the irradiation of one-fold sunlight, the 4D printing hydrogel material of Example 2 exhibits excellent thermosensitive response, can undergo structural contraction rapidly (3 min) and release liquid water quickly, and release 90% of the water in 25 min to achieve the collection of fresh water, solving the problem that traditional materials usually need to overcome the evaporation enthalpy of water during the desorption process and having high energy consumption.
[0091] It is known from Figure 6 It can be seen that the moisture absorption properties of the 4D printing hydrogel materials of Example 1 and Example 2 are not very different under different humidities, indicating that the introduction of polypyrrole not only does not have an obvious impact on the moisture absorption properties of the hydrogel material, but also endows the hydrogel material with photothermal conversion properties, enabling the hydrogel material to release the adsorbed water under light irradiation.
[0092] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those of ordinary skill in the art should understand that they can still modify the technical solutions described in the foregoing embodiments, or perform equivalent replacements for some of the technical features; and these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the various embodiments of the present invention.
Claims
1. A method for preparing a 4D printing hydrogel material, characterized in that: The preparation method comprises: S1. Prepolymerizing N-isopropylacrylamide under the action of a photoinitiator to obtain a prepolymer; S2. mixing the prepolymer, [2-(methacryloyloxy)ethyl]dimethyl-(3-sulfonic acid propyl)ammonium hydroxide and a crosslinking agent to obtain a printing paste; S3. Using the printing slurry to perform 3D photocuring printing to obtain a hydrogel matrix having a porous structure; S4. Soaking the hydrogel matrix in a lithium salt solution to obtain a 4D printing hydrogel material.
2. The preparation method according to claim 1, characterized in that: Before step S4, the method further includes: The hydrogel matrix is immersed in a pyrrole monomer solution, and then oxidatively polymerized in an oxidant solution.
3. The preparation method according to claim 1 or 2, characterized in that: The mass ratio of N-isopropylacrylamide to the initiator is 1:0.005-0.01; preferably, the photoinitiator is phenyl (2,4,6-trimethylbenzoyl) lithium phosphate; The mass ratio of N-isopropylacrylamide to water is 1:0.8-0.12; The mass ratio of N-isopropylacrylamide to [2-(methacryloyloxy)ethyl]dimethyl-(3-sulfonic acid propyl)ammonium hydroxide is 1:0.2-0.3; and / or The mass ratio of N-isopropylacrylamide to the cross-linking agent is 1:0.05-0.08; preferably, the cross-linking agent is N,N'-methylenebisacrylamide.
4. The preparation method according to claim 1 or 2, characterized in that: The prepolymerization reaction is carried out by irradiating ultraviolet light at 20 to 30° C. for 1 to 3 minutes; and / or During the light-curing printing process, the thickness of a single layer is 50 to 100 μm, and the light-curing time of a single layer is 40 to 60 seconds.
5. The preparation method according to claim 1 or 2, characterized in that: The lithium salt solution contains 5 to 40 wt% lithium salt, and the lithium salt is preferably lithium chloride; and / or The soaking time is 12 to 24 hours.
6. The preparation method according to claim 2, characterized in that: The pyrrole monomer solution contains 2-3 wt% pyrrole monomer; and / or The oxidant solution is a FeCl3 solution, and preferably, the FeCl3 in the FeCl3 solution accounts for 1-2 wt%.
7. The preparation method according to claim 2, characterized in that: The soaking time is 1 to 2 hours; and / or The time of the oxidative polymerization is 1 to 2 hours.
8. The preparation method according to claim 1 or 2, characterized in that: After the lithium salt solution is soaked, a drying step is also included; the drying is at least one of freeze drying and normal pressure drying.
9. A 4D printing hydrogel material, characterized in that: The method is prepared by the method according to any one of claims 1 to 8.
10. An application of the 4D printing hydrogel material according to claim 9, characterized in that: Applied in the field of atmospheric water harvesting.
Citation Information
Cited By
Copolymerized temperature-sensitive hygroscopic gel material as well as preparation method and application thereof
CN120923675A
Porous composite gel as well as preparation method and application thereof in atmospheric catchment