High-adhesion transparent self-healing super-smooth coating and preparation method thereof

By grafting 2-urea-4-pyrimidine (UPy) units in polydimethylsiloxane (PDMS) and building a three-arm topological network, combined with silicone oil, the defects of traditional self-healing materials in transparency, interface adhesion and underwater adaptability are solved, and a high adhesion, transparent, self-healing and super-slip coating is achieved, which is suitable for a variety of marine application scenarios.

CN120137507APending Publication Date: 2025-06-13INST OF OCEANOLOGY - CHINESE ACAD OF SCI
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202510213774.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-02-26
Publication Date
2025-06-13

AI Technical Summary

Technical Problem

Traditional self-healing materials have significant shortcomings in transparency, interface adhesion and underwater adaptability, and it is difficult to achieve collaborative optimization in multifunctional integration.

Method used

Polydimethylsiloxane (PDMS) is used as the matrix, and grafting 2-urea-4-pyrimidine (UPy) units onto the PDMS main chain or side chain, and connecting the siloxane backbone with the UPy unit as the crosslinking node, a three-arm topological network is constructed, and silicone oil is combined to improve antifouling performance.

Benefits of technology

It achieves a high adhesion, transparency, self-healing and super-slip coating, with excellent visible light transmittance, extremely strong interface combination strength and good underwater pollution resistance, and is suitable for scenes such as ship optical sensor protection and self-cleaning portholes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120137507A_ABST
    Figure CN120137507A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a high-adhesion transparent self-healing super-smooth coating. Polydimethylsiloxane is taken as a matrix, a three-arm type dynamic hydrogen bond network structure is constructed, and 2-ureido-4-pyrimidone (UPy unit) is taken as a crosslinking node to be connected with a siloxane main chain, so that the crosslinking density and the interface binding energy are remarkably improved. According to the invention, a UPy unit is innovatively introduced into a main chain or a side chain to construct two topological structures of (SUP) 2TD or (MUP) 2TD. Compared with (MUP) 2TD, the (SUP) 2TD shows excellent tensile property and self-healing property in both air and underwater environments. The enhancement of this performance is attributed to the improvement of chain displacement capability in (SUP) 2TD. Through interface dynamics, a UPy unit is guided to an interface and interacts with an interface group, and a very strong adhesion effect is obtained. In addition, the coating shows excellent self-healing performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of functional material preparation, and particularly relates to a highly adhesive transparent self-healing super-slippery coating and a preparation method thereof. Background Art

[0002] Traditional self-healing material systems face three technical bottlenecks in achieving multifunctional integration: First, the selectivity limitation of dynamic bonding groups results in a negative correlation between material transparency and interfacial adhesion. Although a high-density hydrogen bond network can enhance mechanical strength, it causes a light scattering effect due to the formation of a crystalline phase. Second, most existing dynamic crosslinking network designs adopt a single topological structure, and the synergistic effect between physical crosslinking and chemical crosslinking is insufficient. It is difficult to construct a stable energy dissipation mechanism while maintaining chain segment mobility, resulting in significant performance differences in dry / wet environments. Third, the interfacial bonding of conventional super-slippery coatings mostly relies on weak interactions such as van der Waals forces, lacking a controllable chemical bond anchoring strategy, and is prone to interfacial slip failure under dynamic water flow shear or temperature alternating conditions.

[0003] A deeper contradiction lies in the inherent conflict between dynamic bond recombination kinetics and environmental adaptability: Systems based on reversible covalent bonds exhibit efficient self-healing ability in dry environments, but the interference of water on the dissociation activation energy of dynamic bonds significantly delays the bond recombination rate; while physical crosslinking networks mainly composed of non-covalent bonds maintain responsiveness in humid environments, but have poor mechanical properties due to too low bond energy. In terms of optical transparency, traditional anti-fouling coatings mostly achieve surface hydrophobicity through plasticizer migration, but phase separation caused by small molecule diffusion forms a light scattering interface at the micron scale, resulting in irreversible loss of light transmittance.

[0004] In harsh marine application scenarios, the protective coating needs to meet multiple requirements simultaneously: It must withstand long-term chemical erosion such as biofouling, and maintain stable super-slippery characteristics and interfacial integrity under dynamic mechanical loads, which poses higher requirements for the multi-scale structure design of materials. Current technical routes often adopt a performance compromise strategy - either enhancing interfacial bonding through gradient modulus design but sacrificing the self-healing rate, or constructing a sacrificial lubricating layer to improve wear resistance but exacerbating optical loss, and have not achieved the synergistic optimization of interfacial bond strength, dynamic network reconstruction efficiency, and light transmission characteristics at the molecular dynamics level. Summary of the Invention

[0005] The purpose of the present invention is to provide a highly adhesive transparent self-healing super-slippery coating and a preparation method thereof for the problems that existing traditional self-healing materials have significant defects in transparency, interfacial adhesion, and underwater adaptability.

[0006] To achieve the above object, the technical solution provided by the present invention is: a highly adhesive transparent self-healing super-slippery coating, with PDMS as the matrix, grafting UPy units onto the main chain or side chain of PDMS, and using UPy units as crosslinking nodes to connect the silicone main chain.

[0007] The present invention also provides a preparation method of the highly adhesive transparent self-healing super-slippery coating, including: (1) Prepare UPy units for grafting onto the side chain or main chain of PDMS; (2) Prepare a three-arm structure polymer with PDMS as the main chain; Charge poly(dimethylsiloxane) bis(3-aminopropyl) terminated and chloroform into a flask equipped with a reflux condenser, slowly dropwise add a trifunctional homopolymer of hexamethylene diisocyanate, and react under nitrogen protection; the molar ratio of poly(dimethylsiloxane) bis(3-aminopropyl) terminated to the trifunctional homopolymer of hexamethylene diisocyanate is 3:1; then rotary distill to remove the solvent chloroform, and wash the solid product PDMS 3 -T; collect by filtration, vacuum dry overnight for standby; (3) Prepare a polymer elastomer with UPy units grafted onto the main / side chain of the three-arm structure polymer Equip a flask with a reflux condenser, charge isophorone diisocyanate and tetrahydrofuran, and magnetically stir at room temperature for 10 min; dissolve the PDMS 3 -T prepared in step (3) in tetrahydrofuran, slowly drop it into the flask, and stir under a nitrogen atmosphere to obtain an (IP) 3 T prepolymer solution; the molar ratio of isophorone diisocyanate to PDMS 3 -T is 3:1; dissolve the UPy units and 4,4'-dihydroxybiphenyl prepared in step (1) in anhydrous dimethyl sulfoxide under nitrogen protection, and drop them into the prepolymer solution; the molar ratio of UPy units, 4,4'-dihydroxybiphenyl and (IP) 3 T is 2:1:1; stir at 70 °C under a nitrogen atmosphere for 3 h, stop the chain extension reaction, expose to air to obtain a polymer solution; then pour the polymer solution into a glass petri dish and dry overnight in the surrounding air to form an elastomer; finally, cut the elastomer into particles, wash, and dry overnight; (4) Prepare a highly adhesive transparent self-healing super-slippery coating Dissolve the elastomer in step (3) in tetrahydrofuran, spin-coat it on the required substrate to obtain a coating; soak the sample in silicone oil to obtain a super-slippery coating.

[0008] Preferably, the preparation method of the UPy unit grafted on the side chain of PDMS is as follows: 2-amino-4-hydroxy-6-methylpyrimidine and hexamethylene diisocyanate are stirred and mixed at a molar ratio of 1:8 under nitrogen protection to synthesize the crude product 2-(6-isocyanato-hexylamine)-6-methyl-4[1H]pyrimidinone; the crude product is washed with hexane and dried overnight to obtain the pure product; the product and 2-amino-2-methyl-1,3-propanediol are dissolved in anhydrous chloroform at a molar ratio of 1:0.74; subsequently, the mixture is stirred under a nitrogen atmosphere and purified and dried.

[0009] Preferably, the preparation method of the UPy unit grafted on the main chain of PDMS is as follows: a mixture of α-acetyl-γ-butyrolactone and guanidine carbonate with a molar ratio of 1:1 is refluxed with absolute ethanol in the presence of triethylamine; then, the product is filtered, washed, and dried.

[0010] Preferably, during the spin coating of the elastomer, the rotation speed is 1000 rpm, the rotation time is 60 s, and the original sample is soaked in silicone oil for 24 h.

[0011] This coating uses polydimethylsiloxane (PDMS) as the backbone and exhibits ultrafast dynamic reversibility by integrating multiple dynamic hydrogen bonds, especially 2-ureido-4-pyrimidine (UPy) units and amide (-CO-NH 2 ) units. Secondly, inspired by the cobweb structure, UPy acts as a connection point in the three-arm structure to connect the silicone main chains, thus significantly increasing the density of the crosslinked network and endowing the material with excellent self-healing performance and mechanical strength. Finally, by introducing silicone oil with a certain fluidity, the anti-fouling performance of the coating is further significantly improved.

[0012] The beneficial effects of the present invention are as follows: The present invention relates to a high-performance transparent self-healing super-slippery coating based on polydimethylsiloxane (PDMS), and its core lies in achieving multifunctional integration through the synergistic effect of molecular structure design and dynamic bonds. Specifically: (1) A three-arm topological network is constructed with PDMS as the backbone, and 2-ureido-4-pyrimidinone (UPy) dynamic hydrogen bond units are used as crosslinking nodes to connect the silicone main chains, forming a network structure with both high crosslinking density and dynamic reversibility; (2) By grafting UPy units differently on the main chain and side chain, two topological configurations of (SUP)2TD and (MUP) 2 TD are formed, where (SUP) 2TD exhibits better tensile strength and air / underwater self-healing efficiency due to enhanced segment displacement ability; (3) The interface dynamics control mechanism is introduced to make the UPy unit directional enriched at the interface and form multiple interactions with the substrate, combined with the light scattering inhibition effect of silicone oil, to achieve >92% visible light transmittance and extremely strong interface bonding strength; (4) The prepared coating has good effect in underwater antifouling. This system breaks through the technical bottlenecks of self-healing failure, optical loss and weak interface bonding of traditional materials in a humid environment, and is particularly suitable for scenes such as ship optical sensor protection and self-cleaning portholes that require transparency, strong adhesion and corrosion resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 This is an AFM image of the highly adhesive, transparent, self-healing, super-slip coating provided in Example 1 of the present invention; Figure 2 A statistical graph of adhesion strength test data of the high-adhesion transparent self-healing super-slip coating provided in Example 1 of the present invention; Figure 3 A statistical graph of light transmittance data of an original optical glass sheet and an optical glass coated with a highly-adhesive transparent self-healing super-slip coating provided in Example 1 of the present invention; Figure 4 This is a graph showing underwater scratch self-healing changes of the highly adhesive transparent self-healing super-slip coating provided in Example 1 of the present invention; Figure 5 This is a statistical graph of visible light transmittance data of the tempered glass original sheet immersed in unrealistic seawater for 3 months and the tempered glass coated with the prepared high-adhesion transparent self-healing super-slip coating sample provided in Example 1 of the present invention. DETAILED DESCRIPTION

[0014] The specific implementation modes of the present invention are further described below in conjunction with examples. It should be noted that the specific implementation modes described here are only for illustrating and explaining the present invention, and are not limited to the present invention.

[0015] The high-adhesion transparent self-healing super-slip coating prepared by the present invention has good underwater self-healing performance. The high-adhesion transparent self-healing super-slip coating prepared by the present invention has excellent high adhesion performance, high transmittance performance and long-term anti-fouling performance, and has broad application prospects in marine optical instruments and underwater glass window anti-fouling.

[0016] Example 1 Preparation of highly adhesive transparent self-healing super-slip coating: (1) Preparation of UPy units for grafting onto PDMS side chains (S-UPy) First, add 2-amino-4-hydroxy-6-methylpyrimidine (1 g, 8 mmol) and hexamethylene diisocyanate (8.09 g, 48 mmol) into a round-bottom flask. Stir at 100 °C under nitrogen protection for 24 h to synthesize 2-(6-isocyanato-hexylamine)-6-methyl-4[1H]pyrimidinone. Wash the crude product-1 with hexane to remove unreacted HDI, and dry it overnight under vacuum at 50 °C to obtain pure product-1 (white powder). Dissolve product-1 (3 g, 10.24 mmol) and 2-amino-2-methyl-1,3-propanediol (1.464 g, 13.94 mmol) in anhydrous chloroform in a round-bottom flask. Subsequently, stir the mixture under a nitrogen atmosphere at 60 °C for 5 h to synthesize S-UPy. Then wash the crude S-UPy product with chloroform, dissolve it in N,N-dimethylformamide and centrifuge. Finally, precipitate the supernatant in diethyl ether, filter and wash it several times with acetone to obtain pure S-UPy. Dry the product overnight in a vacuum oven at 60 °C to obtain yellowish-white S-UPy.

[0017] (2)Preparation of UPy units (M-UPy) grafted onto the PDMS backbone A mixture of α-acetyl-γ-butyrolactone (2.2 mL, 20 mmol) and guanidine carbonate (1.5 g, 20 mmol) is refluxed in anhydrous ethanol (20 mL) at 80 °C for 1 h in the presence of triethylamine (2.5 mL, 40 mmol). Then, filter the product and wash it with ethanol. Obtain the M-UPy monomer by vacuum drying.

[0018] (3)Preparation of a three-armed structure polymer with PDMS as the backbone (PDMS 3 -T) Generally, charge poly(dimethylsiloxane) bis(3-aminopropyl) terminated (2 g, 2 mmol) and chloroform (50 mL) into a 250 mL round-bottom flask equipped with a reflux condenser, slowly dropwise add a trifunctional homopolymer of hexamethylene diisocyanate (0.336 g, 0.67 mmol), and react at 60 °C under nitrogen protection for 6 h. Then rotary evaporate to remove the solvent chloroform, and wash the solid product three times with 125 mL of acetone. PDMS 3 -T is collected by filtration and dried overnight under vacuum at 60 °C.

[0019] (4)Preparation of a polymer elastomer with UPy units grafted on the main / side chains of a three-armed structure polymer ((SUP) 2 TD / (MUP) 2 TD) Typically, a 250 mL round-bottom flask equipped with a reflux condenser was charged with isophorone diisocyanate (0.44456 g, 2 mmol) and tetrahydrofuran (100 mL), and magnetically stirred at room temperature for 10 min. PDMS 3 -T (1.6 g, 0.13 mmol) was dissolved in 20 mL of tetrahydrofuran, slowly added dropwise into the flask, and stirred under a nitrogen atmosphere at 60 °C for 6 h. The S-UPy (0.079 g, 0.4 mmol) or M-UPy (0.067 g, 0.4 mmol) monomer and 4,4'-dihydroxybiphenyl (0.037 g, 0.2 mmol) were dissolved in anhydrous dimethyl sulfoxide (3 mL) under nitrogen protection and added dropwise to the prepolymer solution. Stirring was carried out under a nitrogen atmosphere at 70 °C for 3 h, and the chain extension reaction was stopped and exposed to air to obtain (SUP) 2 TD or (MUP) 2 TD polymer solution. Then the polymer solution was poured into a glass petri dish and dried overnight in the surrounding air to form an elastomer. Finally, the elastomer was cut into particles, thoroughly washed with water to remove dimethyl sulfoxide, and dried overnight under vacuum at 50 °C.

[0020] (5) Preparation of a highly adhesive transparent self-healing super-slippery coating The prepared elastomer was dissolved in tetrahydrofuran and spin-coated on the desired substrate to obtain a coating. The coating sample was soaked in silicone oil to obtain (SUP) 2 TD@OIL and (MUP) 2 TD@OIL super-slippery coatings.

[0021] The morphology of the prepared highly adhesive transparent self-healing super-slippery coating was characterized by atomic force microscopy (AFM) and compared with the original glass substrate. As Figure 1 shown, the surfaces of the prepared highly adhesive transparent self-healing super-slippery coatings were all very smooth surfaces, and the roughnesses of the (SUP) 2 TD and (MUP) 2 TD coatings were 8.720 and 8.616 nm, respectively. After injecting silicone oil, the roughness further decreased, and the roughnesses of the (SUP) 2 TD@OIL and (MUP) 2 TD@OIL super-slippery coatings were 2.277 and 2.176 nm, respectively.

[0022] Example 2 High adhesion test of the highly adhesive transparent self-healing super-slippery coating: For the shear strength test of adhesion, the highly adhesive transparent self-healing super-slippery coating was dissolved and deposited on the substrate. The deposition area was fixed at 6.25 cm 2After deposition, the deposited highly adhesive transparent self-healing super-slippery coating was bonded with another substrate. The thickness of the supramolecular polymer between the two substrates was 0.2 mm. The shear strength test was carried out using a universal testing machine. The two substrates were adhered in a vertical direction between two clamps. The applied strain rate was 10 mm min -1 , and the data was recorded in real time.

[0023] As Figure 2 shown (SUP) 2 TD elastomer and (SUP) 2 The shear strength of TD@OIL both exceeded 10 MPa, while (MUP) 2 TD and (MUP) 2 The bonding strength of TD@OIL exceeded 5 MPa, showing excellent performance and exceeding the performance of other reported adhesive coatings.

[0024] Example 3 High transmittance test of highly adhesive transparent self-healing super-slippery coating: First, the transmittance of visible light, infrared light, and ultraviolet light of the untreated optical glass was detected by an optical transmittance tester. Then, the prepared highly adhesive transparent self-healing super-slippery coating was dissolved and spin-coated on the surface of the glass after testing. After the sample was dried, the transmittance was detected again. Finally, the spin-coated glass was immersed in silicone oil for 24 h and the transmittance was measured again.

[0025] As Figure 3 can be seen, the optical glass itself has strong optical transmittance to all lights, ultraviolet light (90.03%), infrared light (86.23%), and visible light (91.46%). After spin-coating (MUP) 2 TD and (SUP) 2 TD coatings, the light transmittance was instead enhanced. Especially the visible light transmittance reached 92.23% and 92.3% respectively, and the transmittance of all three lights increased by about 101%. This increase in transmittance indicates that the coating effectively reduces the reflection loss of light at the air-glass interface. After oiling the coating (MUP) 2 TD@OIL and (SUP) 2 TD@OIL further improved the light transmittance of the material, making the light transmittance reach about 103% of the original. The silicone oil filled the tiny unevenness and roughness on the surface of the coating, reducing the surface light scattering and making the light more easily pass through the material, thereby improving the light transmittance. This gives the coating significant advantages in the application on the surface of optical glass.

[0026] Example 4 Underwater self-healing property test of highly adhesive transparent self-healing super-slippery coating: In the underwater healing test, the prepared highly adhesive transparent self-healing super-slippery coating was dissolved and spin-coated on the glass surface to prepare (MUP)2 TD and (SUP) 2 TD coating, and (MUP) 2 TD and (SUP) 2 The TD coating was immersed in silicone oil for 24 h to prepare (MUP) 2 TD@OIL and (SUP) 2 TD@OIL coating. Next, a scratch recovery test was carried out by scraping the film with a scalpel. The change in the scratch width trajectory was also observed using a confocal laser scanning microscope (CLSM).

[0027] As Figure 4 shown, after scratching the coating surface with a scalpel, the CLSM images showed that after 24 hours, the scratches on the (SUP) 2 TD@OIL surface protected by silicone oil were almost completely healed, leaving only a deeper mark, while the (SUP) 2 TD and (MUP) 2 scratches on the TD surface were difficult to heal due to the continuous action of water molecules. (MUP) 2 The unhealed state of TD@OIL was mainly due to the too high crosslinking density, making it difficult for molecular chains to migrate. This indicates that the prepared highly adhesive transparent self-healing super-slippery coating has good underwater self-healing properties.

[0028] Example 5 Long-term antifouling performance test of highly adhesive transparent self-healing super-slippery coating: The marine field test was carried out in Tangdao Bay (35.93 N, 120.21 E). During the biologically active season of marine pollutants, the prepared highly adhesive transparent self-healing super-slippery coating was added to tempered glass at a water depth of 0.5 m and soaked for 3 months (from August to November). The test panel was placed on a floating valve parallel to the sea surface at 0.5 m. In the offshore field test, the dry film thickness of the antifouling coating was controlled between 100 and 150 μm. The panel was taken out of the sea regularly, and the visible light transmittance was measured using an optical transmittance tester, and the biological fouling deposition on the coating was observed.

[0029] As Figure 5 shown, after spin-coating (SUP) 2 TD and (MUP) 2 TD, the transmittance increased. After adding silicone oil, the transmittance further increased. The transmittance of the bare glass decreased sharply on the 10th day of soaking, from 91.3% to 56.5%, and decreased to 32.2% on the 90th day. In contrast, the transmittance of the tempered glass with the (SUP) 2 TD and (MUP) 2 TD coating gradually decreased from 91.6% to 69.0%. While the (MUP) 2 TD@OIL and (SUP) 2The transmittance of the TD@OIL coating remained stable in the first 20 days and even increased due to the seepage of oil. After the 30th day, the transmittance decreased slightly, but still remained at 83.0% on the 90th day. To sum up, (SUP) 2 The TD@OIL coating has the ability of self-healing in seawater, can effectively resist marine microorganisms and fouling, and maintain the transmittance of the optical glass surface for a long time.

Claims

1. A highly adhesive transparent self-healing super-slip coating, characterized in that: Taking PDMS as the matrix, the UPy unit is grafted onto the main chain or side chain of PDMS, and the UPy unit is used as a cross-linking node to connect the siloxane main chain.

2. A method for preparing the highly adhesive transparent self-healing super-slip coating according to claim 1, characterized in that: include: (1) Preparation of UPy units for grafting on the side chains or main chains of PDMS; (2) Preparation of a three-arm structure polymer with PDMS as the main chain; In a flask equipped with a reflux cooler, poly(dimethylsiloxane) bis(3-aminopropyl) end-capping agent and chloroform are charged, and a trifunctional homopolymer of hexamethylene diisocyanate is slowly added dropwise, and the reaction is carried out under nitrogen protection; the molar ratio of poly(dimethylsiloxane) bis(3-aminopropyl) end-capping agent to the trifunctional homopolymer of hexamethylene diisocyanate is 3:1; then the solvent chloroform is removed by rotary distillation, and the solid product PDMS3-T is washed; it is collected by filtration, vacuum dried overnight, and used for later use; (3) Preparation of polymer elastomers with three-arm polymer main / side chains grafted with UPy units The flask is equipped with a reflux cooler, filled with isophorone diisocyanate and tetrahydrofuran, and magnetically stirred at room temperature for 10 minutes; the PDMS3-T prepared in step (3) is added to tetrahydrofuran to dissolve, slowly dripped into the flask, and stirred under a nitrogen atmosphere to obtain an (IP)3T prepolymer solution; the molar ratio of isophorone diisocyanate to PDMS3-T is 3:1; the UPy unit and 4,4'-dihydroxybiphenyl prepared in step (1) are dissolved in anhydrous dimethyl sulfoxide under nitrogen protection, and dripped into the prepolymer solution; the molar ratio of UPy unit to 4,4'-dihydroxybiphenyl and (IP)3T is 2:1:1; the mixture is stirred under a nitrogen atmosphere at 70°C for 3 hours, the chain extension reaction is stopped, and the mixture is exposed to air to obtain a polymer solution; the polymer solution is then poured into a glass culture dish and dried in ambient air overnight to form an elastomer; finally, the elastomer is cut into particles, washed, and dried overnight; (4) Preparation of highly adhesive, transparent, self-healing, super-slip coatings The elastomer in step (3) is dissolved in tetrahydrofuran and spin-coated on a desired substrate to obtain a coating; the sample is immersed in silicone oil to obtain an ultra-slippery coating.

3. The method for preparing a highly adhesive transparent self-healing super-slip coating according to claim 2, characterized in that: The preparation method of the UPy unit grafted on the side chain of PDMS is as follows: 2-amino-4-hydroxy-6-methylpyrimidine and hexamethylene diisocyanate are stirred and mixed at a molar ratio of 1:8 under nitrogen protection to synthesize a crude product 2-(6-isocyanate-hexylamine)-6-methyl-4[1H]pyrimidinone; the crude product is washed with hexane and dried overnight to obtain a pure product; the product and 2-amino-2-methyl-1,3-propanediol are dissolved in anhydrous chloroform at a molar ratio of 1:0.74; the mixture is then stirred under a nitrogen atmosphere to obtain an S-UPy monomer; and the S-UPy monomer is purified and vacuum dried.

4. The method for preparing a highly adhesive transparent self-healing super-slip coating according to claim 2, characterized in that: The preparation method of the UPy unit grafted on the PDMS main chain is as follows: a mixture of α-acetyl-γ-butyrolactone and guanidine carbonate in a molar ratio of 1:1 is refluxed with anhydrous ethanol in the presence of triethylamine; the reaction temperature is 80°C and the stirring time is 1 h; then, the product is filtered, washed, and vacuum dried to obtain the M-UPy monomer.

5. The method for preparing a highly adhesive transparent self-healing super-slip coating according to claim 2, characterized in that: During the elastomer spin coating process, the spinning speed was 1000 rpm, the spinning time was 60 s, and the samples were immersed in silicone oil for 24 h.

Citation Information

Cited By

  • Laser preparation method of oleophobic anti-adhesion surface

    CN120945355A

  • Anti-fouling and anti-corrosion integrated coating with long-acting, high-adhesion and super-lubricity functions as well as preparation method and application of anti-fouling and anti-corrosion integrated coating

    CN121086633A

  • An antifouling and anticorrosion integrated coating with long-acting high adhesion and super-slippery function, and a preparation method and application thereof

    CN121086633B