Three-dimensional porous self-supporting electrode constructed by in-situ growth of copper nanoparticles on surface of foamed nickel for hydrogen evolution by water electrolysis and preparation method of three-dimensional porous self-supporting electrode

By growing copper nanoparticles in situ on the surface of nickel foam and building a three-dimensional porous self-supporting electrode, the problems of active site blocking and conductivity reduction caused by the use of adhesives in traditional electrolytic hydrodynamic hydrogen analysis technology are solved, and efficient electrochemical hydrogen evolution effect is achieved.

CN120138688APending Publication Date: 2025-06-13CHINA UNIV OF PETROLEUM (BEIJING)
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202510289833.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-03-12
Publication Date
2025-06-13

AI Technical Summary

Technical Problem

In the existing electrolytic hydrogen analysis technology, traditional powder catalysts use polymer binders with poor conductivity such as Nafion, resulting in blocking of active sites, reducing conductivity or suppressing gas transmission, and weakening catalytic activity.

Method used

The copper nanoparticles were grown in situ on the surface of the foam nickel foam by chronometer electrodeposition, and a three-dimensional porous self-supporting electrode was constructed. The preparation of self-supporting electrodes without adhesive was achieved through hydrogen bubbles as dynamic templates.

Benefits of technology

It effectively solves the problems of active site blocking, conductivity reduction and gas transmission inhibition caused by the use of adhesives in traditional technology, improves the efficiency and stability of electrochemical hydrogen evolution, and shows excellent hydrogen evolution overpotential and Tafel slope.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005308283620000061
    Figure BDA0005308283620000061
  • Figure BDA0005308283620000062
    Figure BDA0005308283620000062
  • Figure BDA0005308283620000071
    Figure BDA0005308283620000071
Patent Text Reader

Abstract

The invention discloses a three-dimensional porous self-supporting electrode constructed by in-situ growth of copper nanoparticles on the surface of foamed nickel for hydrogen evolution by water electrolysis and a preparation method of the three-dimensional porous self-supporting electrode. The preparation method of the three-dimensional porous self-supporting electrode constructed by in-situ growth of the copper nanoparticles on the surface of the foamed nickel comprises the following steps: taking the foamed nickel as a working electrode, taking a mixed solution composed of a copper salt, a chlorine salt, an inorganic acid and deionized water as an electrolyte, and carrying out electrodeposition by adopting a timing coulometric method to obtain the three-dimensional porous self-supporting electrode constructed by in-situ growth of the copper nanoparticles on the surface of the foamed nickel; the three-dimensional porous self-supporting electrode constructed by in-situ growth of the copper nanoparticles on the surface of the foamed nickel is obtained. According to the preparation method, the self-supporting electrode without the adhesive is prepared through the one-step electrodeposition method with the hydrogen bubbles as the dynamic template, no precious metal participates in the self-supporting electrode, and the problems that active sites are blocked, the conductivity is reduced or gas transmission is inhibited due to the fact that a Nafion solution and other polymer adhesives with poor conductivity are used in a traditional powdery catalyst can be effectively solved. The electrode prepared by the invention has excellent HER performance and good stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of electrolytic water hydrogen evolution catalysts, and particularly relates to a three-dimensional porous self-supporting electrode with copper nanoparticles in-situ grown on the surface of nickel foam for electrolytic water hydrogen evolution and a preparation method thereof. Background Art

[0002] As a clean and renewable energy, hydrogen energy has the characteristics of high energy density and harmless emissions during combustion, which is of crucial significance for promoting the sustainable development of future energy. Among the existing diverse hydrogen production technologies, electrolytic water hydrogen production (HER) is considered an efficient hydrogen production route with little environmental impact. In the HER reaction, the performance of the catalyst is closely related to the carrier. The design and selection of the carrier not only affect the dispersion and stability of the catalyst, but also enhance the utilization rate of the active components per unit area, thereby improving the overall catalytic efficiency. The conductivity of zero-dimensional and one-dimensional materials is relatively low, which directly limits the electron transport efficiency in the carrier and further affects the rate of the entire electrocatalytic reaction. For two-dimensional materials, due to the interlayer stacking phenomenon, the effective surface area is reduced and the ion transport channels are blocked, which increases the difficulty of ion transport and thus reduces the reaction efficiency. Therefore, developing a three-dimensional carrier that is conducive to the mass transfer of solid-liquid-gas phases to provide a larger specific surface area, increase active sites, and improve the transport efficiency has become the key to enhancing the electrochemical hydrogen evolution activity. Since the construction of three-dimensional catalytic materials usually requires loading hydrogen evolution active components onto a porous carrier and coating it on a conductive substrate. However, in most cases, this process relies on Nafion adhesives, which may block active sites, reduce conductivity, or inhibit gas transport, weakening the catalytic activity. Therefore, how to construct a three-dimensional self-supporting electrode for electrolytic water hydrogen evolution without adhesives by electrodeposition method is still a technical problem that needs to be solved urgently at present. Summary of the Invention

[0003] The purpose of the present invention is to provide a three-dimensional porous self-supporting electrode with copper nanoparticles in-situ grown on the surface of nickel foam for electrolytic water hydrogen evolution and a preparation method thereof. This method uses chronocoulometry electrodeposition to prepare the Cu NPs@NF self-supporting electrode, and prepares a self-supporting electrode without adhesives by a one-step electrodeposition method using hydrogen bubbles as a dynamic template, and no precious metals are involved, which can effectively solve the problems of blocking active sites, reducing conductivity, or inhibiting gas transport caused by using polymer adhesives with poor conductivity such as Nafion solution for traditional powdery catalysts.

[0004] To achieve the above purpose, the present invention adopts the following technical solutions:

[0005] In the first aspect, the present invention provides a preparation method for constructing a three-dimensional porous self-supporting electrode by in-situ growth of copper nanoparticles on the surface of nickel foam, comprising the following steps: using nickel foam (NF) as the working electrode, and using a mixed solution composed of a copper salt, a chloride salt, an inorganic acid, and deionized water as the electrolyte, and performing electrodeposition by chronocoulometry to obtain the three-dimensional porous self-supporting electrode with copper nanoparticles in-situ grown on the surface of the nickel foam.

[0006] Based on the above technical solution, the obtained Cu NPs@NF self-supporting electrode by electrodeposition has a three-dimensional porous structure mainly composed of mesoporous networks and slit pores coexisting, which promotes the solid-liquid-gas three-phase mass transfer during the hydrogen evolution process and helps to accelerate the catalytic reaction kinetics. Among them, the addition of NaCl additive in the electrolyte inhibits the formation of intermediate by-product CuCl and at the same time accelerates the deposition kinetics.

[0007] In the above preparation method for constructing a three-dimensional porous self-supporting electrode by in-situ growth of copper nanoparticles on the surface of nickel foam, further, the method further includes pretreating the nickel foam before electrodeposition, and the pretreatment includes: successively performing ultrasonic cleaning on the nickel foam with dilute hydrochloric acid (such as 1.0 mol / L), absolute ethanol, and deionized water, and drying it after washing. Among them, the purpose of pickling is to remove surface metal oxides, the absolute ethanol washing is to remove the oil stains on the surface of the nickel foam using an organic solvent, and the deionized water is to wash away the residual dilute hydrochloric acid and absolute ethanol. Preferably, the ultrasonic cleaning time for each solvent is 10 - 30 min, such as 20 min. As an example, the size of the nickel foam is 5 mm × 5 mm.

[0008] In the above preparation method for constructing a three-dimensional porous self-supporting electrode by in-situ growth of copper nanoparticles on the surface of nickel foam, further, the copper salt is a water-soluble copper salt, including CuSO 4 、Cu(NO 3 ) 2 、CuCl 2 ;

[0009] The chloride salt is a water-soluble chloride salt, including NaCl, KCl, MgCl 2 、CaCl 2 ;

[0010] The inorganic acid is a water-soluble strong acid, including H 2 SO 4 、HCl、HNO 3 ;

[0011] In the mixed solution, the concentration of Cu 2+ is 0.03 - 0.10 mol / L; the concentration of Cl - is 1.0 - 2.0 mol / L; the concentration of H +The concentration is 1.0 - 4.0 mol / L.

[0012] As an example, in the mixed solution, 5.43 mL of sulfuric acid solution with a mass fraction of 98% and 0.48 g of CuSO 4 and 5.85 g of NaCl are added to every 100 mL of deionized water.

[0013] In the method for preparing a three-dimensional porous self-supporting electrode by in-situ growth of copper nanoparticles on the surface of nickel foam as described above, in the chronocoulometry, the electrodeposition uses a three-electrode system, and the three-electrode system includes the working electrode, the reference electrode, and the counter electrode. The reference electrode is an Ag / AgCl electrode, and the counter electrode is a platinum wire electrode.

[0014] In the method for preparing a three-dimensional porous self-supporting electrode by in-situ growth of copper nanoparticles on the surface of nickel foam as described above, in the chronocoulometry, the deposition voltage is -0.4 to -1.2 V, and the deposition time is 500 to 3000 s. As the deposition voltage increases, finer and finer wrinkles appear on the nickel foam, and the formation of pores is accompanied. However, when the voltage is -1.0 V, the wrinkles start to aggregate. Preferably, in the chronocoulometry, the deposition voltage is -0.8 V. As the deposition time increases, the particles grown on the surface of the nickel foam aggregate and take shape, and different degrees of gaps appear on the surface layer, accompanied by the generation of disordered wrinkles. When the deposition time reaches 1000 s, the surface is completely wrinkled and a large number of irregular pores appear, which is beneficial to form a larger specific surface area and promote mass transfer in the alkaline HER process. If the deposition time continues to increase, the pores that appear on the surface will agglomerate or collapse, which is not conducive to the progress of surface mass transfer. Therefore, preferably, in the chronocoulometry, the deposition time is 1000 s.

[0015] In the method for preparing a three-dimensional porous self-supporting electrode by in-situ growth of copper nanoparticles on the surface of nickel foam as described above, after the electrodeposition, the method includes: washing the deposited electrode with deionized water, and drying it after washing; preferably, the drying temperature is 25 - 40 °C, and the drying time is 1 - 3 h, such as drying at 25 °C for 1 h.

[0016] In a second aspect, the present invention provides a three-dimensional porous self-supporting electrode with copper nanoparticles in-situ grown on the surface of nickel foam prepared by the method described in any one of the above.

[0017] In a third aspect, the present invention provides the application of the three-dimensional porous self-supporting electrode with copper nanoparticles in-situ grown on the surface of nickel foam in electrolytic water hydrogen evolution.

[0018] In a fourth aspect, the present invention provides a method for electrolytic water hydrogen evolution, including the following steps: using the three-dimensional porous self-supporting electrode with copper nanoparticles in-situ grown on the surface of nickel foam as the cathode, and performing electrolysis in an alkaline aqueous solution.

[0019] The present invention has the following beneficial effects:

[0020] (1) The self-supporting electrode prepared by the one-step electrodeposition method using hydrogen bubbles as a dynamic template provided by the present invention can effectively solve the problems of blocking active sites, reducing conductivity, or inhibiting gas transport caused by using polymer binders with poor conductivity such as Nafion solution for traditional powdered catalysts.

[0021] (2) The present invention synthesized a series of self-supporting electrodes by setting different deposition voltages and deposition times, and studied the effects of different deposition voltages and deposition times on the morphology and HER performance of the self-supporting electrodes. The HER performance was tested under alkaline conditions. The results showed that when the deposition voltage was -0.8 V and the deposition time was 1000 s, the Cu NPs@NF self-supporting electrode obtained had the optimal performance.

[0022] (3) The self-supporting Cu NPs@NF electrode synthesized by the present invention does not involve noble metals, and the synthesis method is simple and feasible, providing certain insights for the development of non-noble metal catalysts for electrolytic water hydrogen evolution. Cu nanoparticles grow in-situ on the surface of the nickel foam substrate and act as active sites, accelerating the electron transfer rate of the HER process. At the same time, Cu NPs@NF has a three-dimensional porous structure mainly composed of mesoporous networks and slit pores coexisting, which promotes the solid-liquid-gas three-phase mass transfer during the hydrogen evolution process and helps to accelerate the catalytic reaction kinetics. When the deposition voltage is -0.8 V and the deposition time is 1000 s, the prepared self-supporting electrode exhibits excellent HER performance. At 10 mA cm -2 conditions, it has a hydrogen evolution overpotential of 95 mV, a Tafel slope of 179 mV dec -1 , and has good stability. Description of the Drawings

[0023] Figure 1 is the E-pH diagram of Cu-Cl-S-H 2 O.

[0024] Figure 2 is the scanning electron microscope (SEM) image of Example 1 (Cu NPs@NF-0.8V).

[0025] Figure 3 is the transmission electron microscope (TEM) image of Example 1.

[0026] Figure 4 is the X-ray diffraction (XRD) pattern of Example 1.

[0027] Figure 5 is the full X-ray photoelectron spectroscopy (XPS) spectrum of Example 1.

[0028] Figure 6 This is the stability test curve of Embodiment 1 of the present invention. Detailed implementation manners

[0029] The present invention will be further described in detail below in conjunction with the specific implementation manners. The provided embodiments are only for clarifying the present invention, rather than limiting the scope of the present invention. The following provided embodiments can be used as a guide for those of ordinary skill in the art to make further improvements, and do not limit the present invention in any way.

[0030] The methods used in the following embodiments are all conventional methods unless otherwise specified, and are carried out according to the techniques or conditions described in the literature in the field or according to the product specifications. The materials, reagents, etc. used in the following embodiments can be obtained from commercial sources unless otherwise specified.

[0031] The nickel foam in the following embodiments was purchased from Cyber Electrochemical Materials Technology Co., Ltd., with a thickness of 0.5 mm and a surface density of 348 g / m 2 , 110 PPI.

[0032] The electrochemical workstation in the following embodiments is a CHI 760E electrochemical workstation. When in use, the chronocoulometry method is adopted, and the deposition voltage and deposition time are set for electrodeposition. Unless otherwise specified, the other parameter settings are as follows: the initial potential is 0.2 V, the end potential is -0.4 to -1.0 V, and according to different deposition times, the step numbers are respectively set to: 100, 150, 200, the pulse width is 5 s, the sampling interval is 5 s, the standing time is 2 s, and the sensitivity is 1.e-003 C.

[0033] Embodiment 1. Preparation of self-supporting Cu NPs@NF-0.8V

[0034] Prepare a three-dimensional porous self-supporting electrode with copper nanoparticles grown in-situ on the surface of nickel foam according to the following steps:

[0035] (1) Pretreatment of the nickel foam substrate

[0036] Take nickel foam (5 mm × 5 mm) as the substrate, and ultrasonically clean it with dilute hydrochloric acid (1.0 mol / L), anhydrous ethanol, and deionized water for 20 min each, and then transfer it to an oven for drying.

[0037] (2) Preparation of the electrolyte

[0038] Measure 5.43 mL of sulfuric acid solution with a mass fraction of 98%, slowly add it dropwise to 100 mL of deionized water, weigh 0.48 g of CuSO 4 , and add 5.85 g of NaCl to the diluted sulfuric acid solution, and stir for 30 min to completely dissolve it.

[0039] (3) Set the parameters for chronocoulometry deposition

[0040] In a three - electrode system, chronocoulometry is used for electrodeposition. Nickel foam serves as the working electrode, the Ag / AgCl electrode serves as the reference electrode, and the platinum wire electrode serves as the counter electrode. The CHI 760E electrochemical workstation is used as the external power supply. The deposition voltage is set to - 0.8V and the deposition time is set to 1000s.

[0041] (4) Collection of the product:

[0042] After the electrodeposition on the nickel foam is completed, it is thoroughly rinsed 2 - 3 times with deionized water and then transferred to an oven to be dried at 25°C for 1h, obtaining the self - supported electrode Cu NPs@NF - 0.8V.

[0043] Example 2

[0044] In this example, the self - supported electrode Cu NPs@NF is prepared by a method similar to that of Example 1. The difference from Example 1 is that the deposition voltage is set to - 0.4V, obtaining the self - supported electrode Cu NPs@NF - 0.4V.

[0045] Example 3

[0046] In this example, the self - supported electrode Cu NPs@NF is prepared by a method similar to that of Example 1. The difference from Example 1 is that the deposition voltage is set to - 0.6V, obtaining the self - supported electrode Cu NPs@NF - 0.6V.

[0047] Example 4

[0048] In this example, the self - supported electrode Cu NPs@NF is prepared by a method similar to that of Example 1. The difference from Example 1 is that the deposition voltage is set to - 1.0V, obtaining the self - supported electrode Cu NPs@NF - 1.0V.

[0049] Example 5

[0050] In this example, the self - supported electrode Cu NPs@NF is prepared by a method similar to that of Example 1. The difference from Example 1 is that the deposition time is set to 500s, obtaining the self - supported electrode Cu NPs@NF - 0.8V - 500s.

[0051] Example 6

[0052] In this example, the self - supported electrode Cu NPs@NF is prepared by a method similar to that of Example 1. The difference from Example 1 is that the deposition time is set to 750s, obtaining the self - supported electrode Cu NPs@NF - 0.8V - 750s.

[0053] Comparative Example 1

[0054] Commercial 20 wt.% Pt / C. Different from the examples, in this comparative example, the commercial 20 wt.% Pt / C catalyst was drop-coated on a nickel foam substrate without performing steps (1), (2), (3), and (4).

[0055] Comparative Example 2

[0056] Pure nickel foam substrate.

[0057] Comparative Example 3

[0058] In this comparative example, a self-supporting electrode Cu NPs@NF was prepared by a method similar to that of Example 1. Different from Example 1, NaCl was not added to the electrolyte.

[0059] Characterization and performance testing

[0060] 1. Characterization

[0061] Figure 1 It is the E-pH diagram of Cu-Cl-S-H 2 O. Figure 2 It is the scanning electron microscope (SEM) image of Example 1 (Cu NPs@NF-0.8V). As can be seen from the left figure, the surface of the sample has a complex three-dimensional structure, mainly showing a branched and granular microscopic morphology. These branched structures show an irregular network distribution, and the particles are densely distributed and have a certain agglomeration characteristic. As can be seen from the right figure, the entire sample substrate is wrinkled and there are irregular cracks and holes. Figure 3 It is the transmission electron microscope (TEM) image of Example 1. It can be observed that the particles grow uniformly on the nickel foam after electrodeposition. Figure 4 It is the XRD pattern of Example 1. Its relative peak positions match well with the Cu and Ni diffraction patterns on the standard PDF cards. The peak at 74.1° indicates the presence of Cu (JCPDS#85-1326), and the peak at 51.8° indicates the presence of Ni (JCPDS#04-0850), indicating that Cu nanoparticles were successfully deposited on the nickel foam. Figure 5 It is the full X-ray photoelectron spectroscopy (XPS) spectrum of Example 1. It can be seen that the surface of the catalyst mainly contains three elements: Cu, Ni, and O, specifically manifested as the Cu 2p orbital, Ni 2p orbital, and O 1s orbital. The presence of oxygen element is attributed to the natural oxidation of Cu NPs@NF.

[0062] 2. HER performance testing

[0063] The HER electrochemistry performance test was carried out in 1M KOH solution. This test was carried out at room temperature using a standard three - electrode system, with a Pt wire as the counter electrode and a Hg / HgO electrode as the reference electrode. The self - supported electrodes prepared in Examples 1 - 6 and Comparative Example 3 were used as the working electrodes; the working electrode in Comparative Example 1 was a nickel foam substrate coated with 20 wt.% Pt / C catalyst; the working electrode in Comparative Example 2 was a pure nickel foam substrate. In addition, the following formula was used to convert the measured potential to the over - potential relative to the reversible hydrogen electrode:

[0064]

[0065] The electrochemistry hydrogen evolution performance of the electrodes was tested by cathodic linear sweep voltammetry (LSV). The set parameters were: starting potential: - 0.9V, ending potential: - 1.6V, scanning rate: 5mV s -1 , and 95% automatic solution resistance compensation (iR compensation) was set before the test. Before the LSV test, all samples were scanned by cyclic voltammetry curves (CV), that is, scanned 20 times at a scanning rate of 100mV s -1 in the range of - 0.9V to - 1.6V to activate the electro - catalyst to the steady state. The stability test of the catalyst was carried out at the potential with a current density of 10mA cm -2 .

[0066] Table 1: Electrochemistry performance test results of each example and comparative example under 1.0M KOH conditions

[0067]

[0068]

[0069] Table 1 shows the alkaline HER test results of Example 1, Example 2, Example 3, Example 4 of the present invention and Comparative Example 1 (commercial 20 wt.% Pt / C), Comparative Example 2 (pure nickel foam substrate) and Comparative Example 3, indicating that the Cu nanoparticles grown on the surface of nickel foam as active sites improve the catalytic efficiency. In addition, to explore the influence of deposition voltage and deposition time on the alkaline HER performance, by comparing the test results of Example 1, Example 2, Example 3, Example 4, Example 5 and Example 6, it can be found that when the deposition voltage is - 0.8V and the deposition time is 1000s, that is, the alkaline HER performance of Example 1 is the best, mainly manifested as having the lowest over - potential and the lowest Tafel slope. Figure 6This is the stability test result of Example 1 of the present invention. Example 1 can operate stably for about 22 h, and the current density shows basically no attenuation, indicating that Example 1 has good stability. Among them, compared with Comparative Example 3, Example 1 added NaCl to the electrolyte. From the comparison results of Example 1 and Comparative Example 3 in Table 1, it can be seen that the Cu NPs@NF self-supporting electrode synthesized with NaCl added to the electrolyte has a lower overpotential. This is because the addition of NaCl additive in the electrolyte inhibits the formation of intermediate by-product CuCl, and at the same time accelerates the deposition kinetics, making the generated Cu NPs@NF self-supporting electrode have better alkaline hydrogen evolution catalytic performance.

[0070] In summary, through Table 1 and Figure 6 it can be seen that the Cu NPs@NF self-supporting electrode synthesized by the present invention accelerates the kinetics of the alkaline hydrogen evolution process, improves the charge transfer rate and catalytic efficiency, shows good hydrogen evolution performance, and at the same time has good stability.

[0071] The present invention has been described in detail above. For those skilled in the art, without departing from the purpose and scope of the present invention, the present invention can be implemented within a relatively wide range under equivalent parameters, concentrations and conditions. Although specific examples of the present invention are given, it should be understood that the present invention can be further improved. In short, according to the principle of the present invention, this application intends to cover any modification, use or improvement of the present invention, including changes made using conventional techniques known in the art that depart from the scope disclosed in this application.

Claims

1. A method for preparing a three-dimensional porous self-supporting electrode by in-situ growth of copper nanoparticles on the surface of nickel foam, comprising the following steps: With nickel foam as the working electrode and a mixed solution of copper salt, chloride salt, inorganic acid and deionized water as the electrolyte, the chronocoulometry method is used for electrodeposition to obtain a three-dimensional porous self-supporting electrode constructed by in-situ growth of copper nanoparticles on the surface of the nickel foam.

2. The method for preparing a three-dimensional porous self-supporting electrode by in-situ growth of copper nanoparticles on the surface of nickel foam according to claim 1, characterized in that: The method further comprises pre-treating the nickel foam before electrodeposition, wherein the pre-treatment comprises: ultrasonically cleaning the nickel foam with dilute hydrochloric acid, anhydrous ethanol and deionized water in sequence, and drying after cleaning; preferably, the ultrasonic cleaning time of each solvent is 10 to 30 minutes.

3. The method for preparing a three-dimensional porous self-supporting electrode by in-situ growth of copper nanoparticles on the surface of nickel foam according to any one of claims 1 to 2, characterized in that: The copper salt is a water-soluble copper salt, including one of CuSO4, Cu(NO3)2, and CuCl2; The chloride salt is a water-soluble chloride salt, including one of NaCl, KCl, MgCl2, CaCl2, and NH4Cl; The inorganic acid is a water-soluble strong acid, including one of H2SO4, HCl, and HNO3; In the mixed solution, Cu 2+ The concentration is 0.03~0.10mol / L; Cl - The concentration is 1.0~2.0mol / L; H + The concentration is 1.0~4.0mol / L.

4. The method for preparing a three-dimensional porous self-supporting electrode by in-situ growth of copper nanoparticles on the surface of nickel foam according to any one of claims 1 to 3, characterized in that: The chronocoulometry electrodeposition adopts a three-electrode system, which includes the working electrode, a reference electrode and a counter electrode. The reference electrode is an Ag / AgCl electrode, and the counter electrode is a platinum wire electrode.

5. The method for preparing a three-dimensional porous self-supporting electrode by in-situ growth of copper nanoparticles on the surface of nickel foam according to any one of claims 1 to 4, characterized in that: In the chronocoulometry, the deposition voltage is -0.4 to -1.2 V, and the deposition time is 500 s to 3000 s.

6. The method for preparing a three-dimensional porous self-supporting electrode by in-situ growth of copper nanoparticles on the surface of nickel foam according to claim 5, characterized in that: In the chronocoulometry, the deposition voltage was -0.8 V and the deposition time was 1000 s.

7. The method for preparing a three-dimensional porous self-supporting electrode by in-situ growth of copper nanoparticles on the surface of nickel foam according to any one of claims 1 to 6, characterized in that: The method comprises, after the electrodeposition, washing the deposited electrode with deionized water, and drying after washing; preferably, the drying temperature is 25 to 40° C., and the drying time is 1 to 3 hours.

8. A three-dimensional porous self-supporting electrode constructed by in-situ growing copper nanoparticles on the surface of nickel foam as claimed in any one of claims 1 to 7.

9. Use of the three-dimensional porous self-supporting electrode constructed by in-situ growth of copper nanoparticles on the surface of nickel foam as claimed in claim 8 in hydrogen evolution by electrolysis of water.

10. A method for electrolyzing water to produce hydrogen, comprising the following steps: using the three-dimensional porous self-supporting electrode constructed by in-situ growing copper nanoparticles on the surface of nickel foam as claimed in claim 8 as a cathode, and electrolyzing hydrogen in an alkaline aqueous solution.

Citation Information

Cited By

  • Hydrogen evolution electrode preparation method based on femtosecond laser liquid phase processing