Method for machining straight micro through hole in glass through ultrafast laser and machining system

By using Bessel beam to perform ultrafast laser modification on the sandwich workpiece of the glass, the problem of the 'flare mouth' phenomenon is solved, and high-quality processing of glass micropores is achieved, ensuring the straightness and geometric accuracy of the micropores.

CN120155681APending Publication Date: 2025-06-17JIANGSU UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202510410210.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-04-02
Publication Date
2025-06-17

AI Technical Summary

Technical Problem

The existing ultrafast laser-induced material modification and assisted chemical etching methods have the phenomenon of 'flare mouth' in glass micropore processing, resulting in a decrease in straightness of the micropores, affecting the geometric accuracy and functionality of the micropores.

Method used

Sandwich workpiece and Bessel beam technology are used to perform ultra-fast laser modification on the sandwich workpiece of glass to ensure that the surface modification intensity and range of the target workpiece in the middle are equal to that of the inside, thereby avoiding the appearance of the 'flaret' morphology during subsequent chemical etching.

Benefits of technology

Effectively suppress or eliminate the defects of the 'flare mouth', ensure the uniform micropore morphology of the target workpiece, improve the processing quality of glass micro-through holes, and meet the needs of high-precision micro-nano manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120155681A_ABST
    Figure CN120155681A_ABST
Patent Text Reader

Abstract

The invention provides a method for machining a straight micro through hole in glass through ultrafast laser and a machining system. The method comprises the following steps that three glass workpieces are bonded into a sandwich type workpiece through an optical cement technology; the Bessel beam is focused on the sandwich type workpiece by adjusting the length of the Bessel beam; ultrafast laser irradiates the sandwich type workpiece, so that the material structure of the inner area of the glass is converted into a silicon-oxygen three-membered ring or a silicon-oxygen four-membered ring from a silicon-oxygen six-membered ring, and the sandwich type workpiece with a vertically-through modified microarray area inside is obtained after processing; the sandwich type workpiece after laser processing is separated through the optical cement removing technology, and only the target workpiece in the middle is reserved; putting a target workpiece into an etching solution, introducing ultrasonic oscillation for etching, and corroding a silicon-oxygen three-membered ring or a silicon-oxygen four-membered ring in an internal modified microarray region by an etching agent to form a micro through hole; and cleaning the etched target workpiece. The appearance of a horn mouth can be avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of laser processing of glass, and particularly to a method and a processing system for processing straight micro-vias on glass with ultrafast laser. Background Art

[0002] With the rapid development of modern industrial technologies, ultrafast laser processing technology has been widely applied in the field of micro-nano processing due to its unique advantages. Ultrafast laser has ultra-high peak power, ultra-short pulse duration (usually in the femtosecond to picosecond range), and non-linear absorption characteristics, enabling it to achieve high-precision three-dimensional micro-processing inside transparent materials. These characteristics make ultrafast laser an ideal tool for processing transparent hard and brittle materials such as glass and sapphire, and it has important application value especially in the processing of glass micro-vias in fields such as microfluidic chips, optical devices, and microelectronic packaging.

[0003] Currently, the common method for processing straight micro-holes on glass with ultrafast laser is Laser-Induced Modification Assisted Chemical Etching (LIMACE). The basic principle of this method is: First, use ultrafast laser to selectively modify the inside of the glass, changing its chemical properties, so that it shows different etching rate differences from the unmodified area during the subsequent chemical etching process, thus achieving the precise forming of micro-structures.

[0004] Although the LIMACE method shows high processing efficiency and good hole wall quality in the processing of glass micro-holes, it still has a significant technical defect in practical applications, that is, the "flare" phenomenon (as shown in the attachment). Figure 1 The so-called "flare" phenomenon refers to the conical structure with an enlarged aperture at the entrance of the upper and lower surfaces of the glass after processing the micro-hole, resulting in a decrease in the straightness of the micro-hole and affecting its geometric accuracy and functionality.

[0005] The generation of the "flare" phenomenon mainly stems from the following two factors:

[0006] 1. Processing threshold differences between the glass surface and the interior: The absorption rate of laser energy by the glass surface is usually higher than that of the interior, resulting in a situation where, under the same laser fluence conditions, the area near the glass surface is more likely to reach or exceed the material modification threshold. For ultrafast (taking femtosecond as an example) lasers, ionizing air only requires a single photon, while ionizing glass requires at least 6 photons. Therefore, the processing threshold of the air inside the glass surface is much lower than that of the glass. Under the action of a relatively low laser fluence, the valence electrons inside the air are excited to the conduction band to form free electrons. These free electrons in the air, as seed electrons, strike the valence electrons near the glass surface. After being struck, the valence electrons of the glass will also be excited to the conduction band to form free electrons. When the free electron density is greater than the modification threshold of the glass, modification occurs. However, a relatively low laser fluence is not sufficient to excite the free electrons inside the glass. Therefore, under the same laser fluence conditions, the degree and range of modification on the glass surface are always greater than those in the interior, and the "flare" phenomenon inevitably occurs after etching.

[0007] 2. Non-uniformity of chemical etching rate: Since the degree of modification on the glass surface is deeper, its etching rate in the chemical etching solution is faster, while the etching rate of the modified area inside is relatively slow. As the etching time extends, the material in the surface area is rapidly removed, while the etching of the interior area lags behind, ultimately forming a "flare" structure with a large entrance and a small middle.

[0008] The "flare" in the glass microvia reduces the depth-to-width ratio of the microvia, resulting in a decrease in the effective through-diameter of the microvia and limiting its high-density layout in microfluidics or optical integration. In addition, the "flare" in the glass microvia affects the optical quality of the pore wall. The pore wall in the flare area is usually relatively rough, which may cause light scattering or fluid turbulence, and is not conducive to optical or fluid transmission applications.

[0009] Currently, the solutions to the "flare" phenomenon mainly include:

[0010] Optimizing laser parameters: By adjusting the laser energy, pulse width, or scanning strategy, the modification difference between the surface and the interior is reduced. However, this method often cannot completely eliminate the flare and may sacrifice the processing efficiency.

[0011] Multi-step etching process: Using staged etching or a combination of etching solutions with different concentrations to balance the etching rates of the surface and the interior. However, this method has a complex process and is difficult to control.

[0012] Mechanical polishing and thinning post-treatment: Removing the flare area through polishing and thinning, but this will increase the processing cost and time. Moreover, it is easy for the debris powder during polishing and thinning to enter the interior of the microvia and cause blockage, which is very difficult to completely remove.

[0013] Although the ultrafast laser-induced modification-assisted chemical etching technology has significant advantages in glass micro-hole processing, the "flare" phenomenon remains a key issue restricting its further development and application. Therefore, there is an urgent need to develop a new processing method that can effectively suppress or eliminate the "flare" to improve the processing quality of glass micro-vias and meet the requirements of high-precision micro-nano manufacturing. The present invention aims to solve this technical problem and provide a more reliable solution for ultrafast laser micro-processing. Summary of the Invention

[0014] Aiming at the deficiencies in the prior art, the present invention provides a method and a processing system for processing straight micro-vias on glass with an ultrafast laser, which can solve the "flare" problem that occurs when processing micro-vias by the ultrafast laser-induced glass modification-assisted chemical etching method. The axially uniform light field of the Bessel beam is used to modify the intermediate target workpiece, so as to ensure that the surface modification intensity and range of the intermediate target workpiece are equal to those inside. In the subsequent chemical etching process, the "flare" morphology can be avoided. This method has high processing morphology accuracy, strong flexibility, and high processing efficiency, and can be applied to the packaging field in the semiconductor field.

[0015] The present invention achieves the above technical objectives through the following technical means.

[0016] A method for processing straight micro-vias on glass with an ultrafast laser, comprising the following steps:

[0017] Bond three glass workpieces into a sandwich workpiece by an optical glue process, wherein the middle glass workpiece is the target workpiece;

[0018] Determine the beam reduction ratio of the Bessel beam according to the overall thickness of the sandwich workpiece, and adjust the length of the Bessel beam so that the Bessel beam is focused on the sandwich workpiece;

[0019] Irradiate the sandwich workpiece with an ultrafast laser to transform the material structure in the internal region of the glass from a silicon-oxygen six-membered ring to a silicon-oxygen three-membered ring or a silicon-oxygen four-membered ring, and obtain a sandwich workpiece with a modified microarray region that penetrates up and down inside after processing;

[0020] Separate the laser-processed sandwich workpiece through a de-glue process, and only retain the middle target workpiece;

[0021] Put the target workpiece into an etching solution and introduce ultrasonic oscillation for etching. The silicon-oxygen three-membered ring or silicon-oxygen four-membered ring in the internal modified microarray region is corroded by the etchant to form a micro-via;

[0022] Clean the etched target workpiece.

[0023] Further, the focused Bessel beam is vertically penetrated through the sandwich workpiece to ensure that the target workpiece in the middle is completely within the non-diffracting region of the Bessel beam. The diameter of the incident beam is adjusted according to the target size of the microvia to control the diameter and length of the Bessel beam, thereby adjusting the size of the modified hole. The sandwich workpiece is moved to perform the machining of the modified hole array.

[0024] Further, the bonding surfaces of the target workpiece and the glass workpieces on both sides thereof are adsorbed to each other by intermolecular van der Waals forces, and there are no other media including air in the bonding surfaces.

[0025] Further, the ultrafast laser is a femtosecond laser or a picosecond laser.

[0026] Further, the etching solution is a hydrofluoric acid solution or a potassium hydroxide solution.

[0027] A machining system for a method of sandwich machining straight microvias on glass with an ultrafast laser, comprising an ultrafast laser system, an attenuator, a mechanical switch, a cone lens, a beam shrinking system, an observation optical path, a charge-coupled device, a six-degree-of-freedom precision displacement platform, and a computer control system;

[0028] The sandwich workpiece is placed on the six-degree-of-freedom precision displacement platform; the ultrafast laser system is used to generate Gaussian pulsed laser; the Gaussian pulsed laser sequentially passes through the attenuator, the mechanical switch, and the cone lens to form a Bessel beam; the beam shrinking system is used to shrink the Bessel beam so that the Bessel beam is focused on the sandwich workpiece; the observation optical path is used to reflect the image of the sandwich workpiece into the charge-coupled device;

[0029] The computer control system adjusts the length of the Bessel beam through the beam shrinking system so that the Bessel beam is focused on the sandwich workpiece.

[0030] Further, the computer control system is used to control the mechanical switch to adjust the number of pulses irradiated on the surface of the sandwich workpiece.

[0031] The beneficial effects of the present invention are as follows:

[0032] 1. For the method of machining straight microvias on glass with the ultrafast laser described in the present invention, by bonding sacrificial workpieces on both sides of the target workpiece, the "flare" defect is located in the sacrificial workpiece, so as to ensure that there is no "flare" in the target workpiece. The method of machining straight microvias on the sandwich workpiece with a Bessel-type ultrafast laser of the present invention can prepare straight microvias on various quartz-based transparent hard and brittle materials such as quartz glass, borosilicate glass, glass-ceramics, and Corning glass, and has a wide application range.

[0033] 2. The method for machining straight micro-vias on glass using the ultrafast laser according to the present invention. The extremely high power density formed after the ultrafast laser is focused enables the transparent material to undergo non-linear absorption of energy only at the focal point. The rapid coupling of the energy of the electron-lattice system greatly reduces the heat-affected zone during machining, effectively suppressing the effects and thermal damage caused by various effects such as the molten zone and shock waves on the surrounding materials, and ensuring good machining accuracy.

[0034] 3. The method for machining straight micro-vias on glass using the ultrafast laser according to the present invention. The "flared mouth" defect is taken over by the sacrificial workpiece, ensuring a uniform micro-hole morphology of the intermediate target workpiece and high morphology accuracy.

[0035] 4. The method for machining straight micro-vias on glass using the ultrafast laser according to the present invention. The ultrafast laser forms a uniform modified zone on the intermediate target workpiece, and ultrasonic oscillation is assisted during subsequent chemical etching, making the pore walls of the straight micro-vias smooth and achieving high-quality machining of the straight micro-vias.

[0036] 5. The method for machining straight micro-vias on glass using the ultrafast laser according to the present invention. Since it can machine micro-nano vias in an N×N array at one time, the machining efficiency is high.

[0037] 6. The method for machining straight micro-vias on glass using the ultrafast laser according to the present invention. By adjusting the Bessel beam, the size of the straight micro-vias can be quantitatively adjusted, and the machining method is flexible. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] In order to more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the following will briefly introduce the drawings required for use in the description of the embodiments or the prior art. The following drawings are some embodiments of the present invention. For those of ordinary skill in the art, without creative efforts, it is obvious that other drawings can also be obtained according to these drawings.

[0039] Figure 1 It is a schematic diagram of a straight micro-via on glass machined by the prior art.

[0040] Figure 2 It is a schematic diagram of the result of inducing modification directly on a single-piece glass, and a schematic diagram of the result of inducing modification on a sandwich-type glass workpiece according to the present invention.

[0041] Figure 3 It is a flow chart of the method for sandwich-type machining of straight micro-vias on glass using the ultrafast laser according to the present invention.

[0042] Figure 4 It is a schematic diagram of the machining system according to the present invention.

[0043] In the figure:

[0044] 1 - femtosecond laser system; 2 - attenuation sheet; 3 - mechanical switch; 4 - cone lens; 5 - plano-convex lens; 6 - beam splitter; 7 - white light source; 8 - charge-coupled device; 9 - dichroic mirror; 10 - microscope objective; 11 - sandwich workpiece; 12 - six-degree-of-freedom precision displacement platform; 13 - computer control system. Detailed implementation manners

[0045] The embodiments of the present invention will be described in detail below. The examples of the embodiments are shown in the accompanying drawings, where the same or similar reference numerals denote the same or similar elements or elements having the same or similar functions throughout. The embodiments described below by referring to the accompanying drawings are exemplary and are intended to explain the present invention and should not be construed as a limitation to the present invention.

[0046] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "transverse", "length", "width", "thickness", "upper", "lower", "axial", "radial", "vertical", "horizontal", "inner", "outer", etc. indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and thus should not be construed as a limitation to the present invention. In addition, the terms "first" and "second" are only used for descriptive purposes and cannot be construed as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, the features defined with "first" and "second" may explicitly or implicitly include one or more of such features. In the description of the present invention, "a plurality of" means two or more unless otherwise specifically defined.

[0047] In the present invention, unless otherwise clearly specified and defined, the terms "mounted", "connected", "connected", "fixed", etc. should be understood in a broad sense. For example, it may be a fixed connection, a detachable connection, or an integral connection; it may be a mechanical connection or an electrical connection; it may be directly connected or indirectly connected through an intermediate medium, and it may be the communication inside two elements. For those of ordinary skill in the art, the specific meanings of the above terms in the present invention can be understood according to specific situations.

[0048] As Figure 3 shown, the method for processing straight micro-vias on glass by the ultrafast laser according to the present invention includes the following steps:

[0049] S01: Bond three glass workpieces into a sandwich workpiece 11 through an optical adhesive process. Among them, the middle glass workpiece is the target workpiece, and the workpieces on both sides are regarded as sacrificial workpieces; the bonding surfaces between the target workpiece and the glass workpieces on both sides are adsorbed to each other through intermolecular van der Waals forces, and there is no air in the bonding surfaces.

[0050] S02: Determine the beam reduction ratio of the Bessel beam according to the overall thickness of the sandwich workpiece 11, and adjust the length of the Bessel beam, so that the Bessel beam is focused on the sandwich workpiece 11; generally, adjust the beam reduction system to adjust the beam length and increase the energy density.

[0051] S03: Ultrafast laser irradiates on the sandwich workpiece 11, and uses the mechanical switch 3 and the attenuation sheet 2 to control the number of pulses and the pulse energy irradiated on the glass workpiece respectively. The ultrafast laser irradiation changes the material structure in the internal area of the glass from the silicon-oxygen six-membered ring to the silicon-oxygen three-membered ring or the silicon-oxygen four-membered ring. After processing, a sandwich workpiece 11 with a modified microarray area (no holes are formed yet) that penetrates up and down inside is obtained; during the processing, in order to ensure that the target workpiece in the middle is completely in the non-diffraction area of the Bessel beam, adjust the incident beam diameter according to the target size of the micro-through hole to control the diameter and length of the Bessel beam, and then adjust the size of the modified hole, and move the sandwich workpiece to perform the modified hole array processing. The ultrafast laser is a femtosecond laser or a picosecond laser.

[0052] S04: Separate the sandwich workpiece 11 after laser processing through the photoresist removal process, only retain the target workpiece in the middle, and discard the upper and lower sacrificial workpieces.

[0053] S05: Place the target workpiece in the etching solution and introduce ultrasonic oscillation for etching. The silicon-oxygen three-membered ring or the silicon-oxygen four-membered ring in the internal modified microarray area is corroded by the etchant to form micro-through holes; since the silicon-oxygen three-membered ring or the silicon-oxygen four-membered ring structure is more easily corroded by the etchant than the silicon-oxygen six-membered ring structure, the area modified by the ultrafast laser will be preferentially corroded to form micro-through holes, while the unmodified area will hardly change. The etching solution is a hydrofluoric acid solution or a potassium hydroxide solution.

[0054] S06: Clean the etched target workpiece, and thus complete the processing of the straight micro-through hole array.

[0055] Example 1

[0056] The method for processing straight micro-through holes in glass by ultrafast laser in Example 1 includes the following steps:

[0057] S01: Bond three pieces of Corning glass with a thickness of 0.5 mm into a sandwich workpiece 11 through the photoresist bonding process; use the photoresist bonding process to exhaust the air between the two pieces of glass, so that during the subsequent laser modification process, the target glass in the middle will not have the situation that the processing threshold on the surface is lower than the internal processing threshold.

[0058] S02: As attached Figure 4As shown in the figure, the femtosecond laser system generates Gaussian laser with a wavelength of 800 nm, a pulse width of 150 fs, and a repetition rate of 1 kHz. The laser energy is changed by the attenuation sheet 2, and the on-off of the mechanical switch 3 is controlled by the computer system 13. The Gaussian laser beam forms a Bessel beam through the axicon lens 4, is incident on the plano-convex lens 5 with a focal length of 100 mm, and the beam direction is changed by the dichroic mirror 9 so that the beam is perpendicularly incident on the microscope objective 10 (20×, NA = 0.45). The combination of the plano-convex lens 5 and the microscope objective 10 constitutes a beam reduction system, which improves the energy density of the beam; the Bessel beam after beam reduction and focusing is irradiated on the sandwich workpiece 11. During this process, the white light emitted by the white light source 7 passes through the beam splitter 6, the dichroic mirror 9, and the microscope objective 10 and is irradiated on the processing area of the workpiece 11, and returns to the beam splitter 6 along the original path. The beam splitter 6 changes the propagation direction of the returned white light to the CCD 8 to observe the processing situation of the workpiece in real time.

[0059] S03: The diameter of the incident spot can be flexibly adjusted. The length of the non-diffracting region is proportional to the diameter of the incident beam. In this embodiment, the diameter of the incident beam is set to 6 mm, and the cone bottom angle of the axicon lens 4 is 2°. After calculation, the length Z of the non-diffracting region after passing through the 4f beam reduction system is 1.55 mm. The sandwich workpiece 11 with a thickness of 1.5 mm is fixed on the six-degree-of-freedom precision displacement platform 12, and the translation stage 12 is moved to set the middle target workpiece of the sandwich workpiece 11 at the midpoint position of the non-diffracting region. The laser energy is adjusted to 10 μJ by the attenuation sheet 2, and 100×100 modified holes are programmed for processing. The mechanical switch 3 is used to ensure that the number of deposited pulses for each modified hole is 100. The processing time for a single modified hole is only 0.1 second, and the time for processing 100×100 modified holes is less than 20 minutes.

[0060] S04: Separate the sandwich workpiece 11 after laser processing and retain the middle target workpiece.

[0061] S05: The target workpiece is cleaned and then placed in a 35.8% potassium hydroxide KOH solution for etching for 6 minutes. The etching rate of the KOH solution in the modified region is about 800 μm / s. Since the aspect ratio of the modified holes is relatively high, the solution is not easily introduced into the interior of the modified holes in the static state. Therefore, ultrasonic oscillation is introduced to enable the solution to better enter the modified region. The silicon-oxygen ternary ring or quaternary ring in the modified region is more sensitive to the KOH solution than the silicon-oxygen hexacyclic ring in the unmodified region. The etching rate ratio of the former to the latter in the 35.8% KOH solution is 200:1. Therefore, compared with the modified region, the volume of the material removed from the unmodified region can be ignored in a short time.

[0062] S06: Clean the etched target workpiece, and thus complete the processing of the straight micro-through hole array.

[0063] Since the modified region generated by femtosecond laser is very uniform and the ultrasonic oscillation computer system 13 is introduced, the sidewall morphology of the microholes after etching is also very uniform, and the taper is almost zero. The glass workpiece after the modified region is completely etched is taken out, and after thorough cleaning, a Corning glass straight microvia array with uniform morphology is obtained, and there is no "flare" defect on the glass surface. The method for sandwich-type machining of straight microvias on glass by the ultrafast laser of the present invention prepares a straight microvia array on glass with low cost, high morphology accuracy and high efficiency.

[0064] As Figure 4 shown, the processing system for machining straight microvias on glass by the ultrafast laser of the present invention includes an ultrafast laser system, an attenuation sheet 2, a mechanical switch 3, a cone lens 4, a beam shrinking system, an observation optical path, a charge-coupled device 8, a six-degree-of-freedom precision displacement platform 11 and a computer control system 13;

[0065] The sandwich-type workpiece 11 is placed on the six-degree-of-freedom precision displacement platform 11; the ultrafast laser system is used to generate Gaussian pulse laser; the Gaussian pulse laser sequentially passes through the attenuation sheet 2, the mechanical switch 3 and the cone lens 4 to form a Bessel beam; the beam shrinking system includes a plano-convex lens 5 and a microscope objective 10, and is used for shrinking the Bessel beam so that the Bessel beam is focused on the sandwich-type workpiece 11; the observation optical path is used to reflect the image of the sandwich-type workpiece 11 into the charge-coupled device 8;

[0066] The computer control system 13 adjusts the length of the Bessel beam through the beam shrinking system, so that the Bessel beam is focused on the sandwich-type workpiece 11. The computer control system 13 is used to control the mechanical switch 3 to adjust the number of pulses irradiated on the surface of the sandwich-type workpiece 11.

[0067] The observation optical path includes a beam splitter 6, a white light source 7 and a dichroic mirror 9; the dichroic mirror 9 changes the beam direction so that it is vertically incident on the microscope objective 10; during this process, the white light generated by the white light source passes through the beam splitter 6, the dichroic mirror 9 and the microscope objective 10 and then irradiates the processing area of the sandwich-type workpiece 11, and then returns to the beam splitter 6 along the original path. The beam splitter 6 changes the propagation direction of the reflected light and is incident on the charge-coupled device 8, so as to realize the real-time monitoring of the processing process.

[0068] It should be understood that although this specification is described according to each embodiment, not every embodiment only contains an independent technical solution. This narrative way of the specification is only for clarity. Those skilled in the art should regard the specification as a whole, and the technical solutions in each embodiment can also be appropriately combined to form other embodiments that can be understood by those skilled in the art.

[0069] The series of detailed descriptions listed above are only specific descriptions of the feasible embodiments of the present invention, and they are not intended to limit the protection scope of the present invention. Any equivalent embodiments or changes made without departing from the technical spirit of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for processing straight micro-through holes on glass using ultrafast laser, characterized in that: The steps include: Bonding three glass workpieces into a sandwich workpiece (11) by means of a photobonding process, wherein the middle glass workpiece is the target workpiece; Determining the beam reduction ratio of the Bessel beam according to the overall thickness of the sandwich workpiece (11), and adjusting the length of the Bessel beam so that the Bessel beam is focused on the sandwich workpiece (11); An ultrafast laser is irradiated on the sandwich workpiece (11) to change the material structure of the inner region of the glass from a six-membered silicon-oxygen ring to a three-membered silicon-oxygen ring or a four-membered silicon-oxygen ring, and after processing, a sandwich workpiece (11) having a modified microarray region penetrating from top to bottom is obtained; The sandwich workpieces (11) processed by laser are separated by a de-glazing process, and only the target workpiece in the middle is retained; The target workpiece is placed in an etching solution and ultrasonic oscillation is introduced for etching, and the silicon-oxygen ternary ring or silicon-oxygen quaternary ring in the internal modified microarray region is corroded by the etchant to form micro-through holes; Clean the target workpiece after etching.

2. The method for processing straight micro-through holes on glass using ultrafast laser according to claim 1, characterized in that: The Bessel beam after the beam reduction is focused vertically through the sandwich workpiece (11) to ensure that the target workpiece in the middle is completely in the non-diffraction area of ​​the Bessel beam. The incident beam diameter is adjusted according to the target size of the micro-through hole to control the diameter and length of the Bessel beam, thereby adjusting the size of the modified hole and moving the sandwich workpiece to perform modified hole array processing.

3. The method for processing straight micro-through holes on glass using ultrafast laser according to claim 1, characterized in that: The bonding surfaces of the target workpiece and the glass workpieces on both sides thereof are adsorbed to each other by intermolecular van der Waals forces, and no air exists in the bonding surfaces.

4. The method for processing straight micro-through holes on glass using ultrafast laser according to claim 1, characterized in that: The ultrafast laser is a femtosecond laser or a picosecond laser.

5. The method for processing straight micro-through holes on glass using ultrafast laser according to claim 1, characterized in that: The etching solution is a hydrofluoric acid solution or a potassium hydroxide solution.

6. A processing system for the method for processing straight micro-through holes on glass using ultrafast laser according to any one of claims 1 to 5, characterized in that: It includes an ultrafast laser system, an attenuation plate (2), a mechanical switch (3), a conical lens (4), a beam reduction system, an observation optical path, a charge coupled device (8), a six-degree-of-freedom precision displacement platform (11) and a computer control system (13); The sandwich workpiece (11) is placed on a six-degree-of-freedom precision displacement platform (11); the ultrafast laser system is used to generate Gaussian pulse laser; the Gaussian pulse laser passes through an attenuation plate (2), a mechanical switch (3) and a conical lens (4) in sequence to form a Bessel beam; the beam reduction system is used to reduce the Bessel beam so that the Bessel beam is focused on the sandwich workpiece (11); the observation optical path is used to reflect an image of the sandwich workpiece (11) into a charge coupled device (8); The computer control system (13) adjusts the length of the Bessel light beam through the beam reduction system, thereby focusing the Bessel light beam on the sandwich workpiece (11).

7. The processing system of the method for processing straight micro-through holes on glass using ultrafast laser according to claim 6, characterized in that: A computer control system (13) is used to control the mechanical switch (3) to adjust the number of pulses irradiated to the surface of the sandwich workpiece (11).

Citation Information

Cited By

  • Processing method of TGV glass straight through hole

    CN122127075A