All-solid-waste asphalt-imitating material as well as preparation method and application thereof
By using all solid waste raw materials to prepare imitation asphalt materials, the problems of high cost and poor performance of existing imitation asphalt materials are solved, and low-cost and high-performance imitation asphalt materials are realized, which are suitable for road construction.
Patent Information
- Application Number
- CN202510637702.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-19
- Publication Date
- 2025-06-17
- Estimated Expiration
- 2045-05-19
AI Technical Summary
The existing imitation asphalt materials have high preparation costs and their performance cannot reach the level of traditional asphalt, resulting in poor mechanical properties of imitation asphalt mixtures.
Imitation asphalt materials are prepared using all solid waste raw materials, including waste glue powder, waste plastic, kitchen waste oil, waste petroleum resin and waste fillers. The materials have excellent road performance through specific preparation methods.
It realizes low-cost and high-performance imitation asphalt materials, excellent mechanical properties, dynamic stability up to 3876 times/mm, and Marshall stability up to 11.3KN, which is suitable for road construction.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of pavement materials, and particularly relates to a fully solid waste asphalt-like material, a preparation method thereof, and an application thereof. Background Art
[0002] Asphalt materials have good adhesion, waterproofness and other characteristics, and are widely used in road engineering and the construction field. In road engineering, asphalt is one of the main materials for paving roads, which can provide a flat and comfortable driving surface for vehicles; in the construction field, it is mainly used to manufacture oil paper, asphalt felt, waterproof coatings and asphalt caulking paste, etc., for building roofing projects, underground waterproof projects, etc. However, asphalt materials have significant thermal sensitivity. They present as solids or semi-solids at normal temperature, but are extremely easy to melt as the temperature rises, and it is difficult to present good performance at high and low temperatures. In addition, asphalt materials are greatly affected by the environment and are prone to aging. Under the long-term action of factors such as heat, sunlight, oxygen and moisture, the low-molecular components in petroleum asphalt are transformed into high-molecular components, reducing the plasticity of petroleum asphalt, increasing its viscosity, gradually becoming brittle and hard until brittle cracking, losing its service function. Moreover, during the production and use process, asphalt may release harmful substances, causing certain harm to the environment and human health. Therefore, developing alternative materials with similar or better performance has become a hot topic in current research.
[0003] In the prior art, it is a common method to prepare asphalt-like materials using polymer materials. A material with asphalt-like properties in the form of a rollable sheet is processed through a certain process by using synthetic rubber, synthetic resin or a blend of the two as the base material and adding appropriate chemical additives and fillers. There are also cases where inorganic materials and polymer materials are compounded to prepare asphalt-like materials with excellent properties by utilizing the rigidity of inorganic materials and the flexibility of polymer materials. However, the preparation cost of existing asphalt-like materials is relatively high, making it difficult to replace asphalt materials for large-scale application in road construction. Moreover, the properties of existing asphalt-like materials such as penetration, softening point and ductility still cannot reach the level of traditional asphalt, resulting in poor mechanical properties of asphalt-like mixtures prepared using asphalt-like materials.
[0004] Based on this, it is of great practical significance for road construction to develop an asphalt-like material with good adhesion and low cost. Summary of the Invention
[0005] Aiming at the problems in the prior art that the preparation cost of asphalt-like materials is high, and the material properties cannot reach the level of traditional asphalt, resulting in poor mechanical properties of asphalt-like mixtures prepared from asphalt-like materials, the present invention provides a fully solid waste asphalt-like material, its preparation method and application. The raw materials of the fully solid waste asphalt-like material include waste rubber powder, waste plastic, kitchen waste oil, waste petroleum resin and waste filler. By utilizing the interaction of each raw material component and combining with a specific preparation method, the fully solid waste asphalt-like material has excellent road performance. Moreover, since each raw material component is waste, the preparation cost is low and easy to obtain, and it can effectively relieve the treatment pressure of solid waste.
[0006] In order to achieve the above invention purpose, the present invention provides the following technical solutions: The first aspect of the present invention provides a fully solid waste asphalt-like material, including the following raw material components in parts by mass: 60-80 parts of waste rubber powder, 20-50 parts of waste plastic, 5-15 parts of kitchen waste oil, 5-15 parts of waste petroleum resin and 20-30 parts of waste filler; Among them, the waste filler includes the following raw material components in mass percentage: 20%-30% of waste glass fiber, 15%-20% of straw residue, 15%-20% of waste clay and the balance of coal gangue powder.
[0007] Compared with the prior art, the present invention prepares a fully solid waste asphalt-like material using waste rubber powder, waste plastic, kitchen waste oil, waste petroleum resin and waste filler as the main raw materials. Among them, the waste rubber powder and waste plastic have certain elasticity and toughness, which can endow the asphalt-like material with excellent high-temperature deformation resistance and low-temperature flexibility, and help improve the durability of the asphalt-like material. And, some components in the waste rubber powder and waste plastic can resist the aging effect of ultraviolet rays and slow down the aging speed of the asphalt-like material. The fatty acids contained in the kitchen waste oil can increase the fluidity and penetration of the asphalt-like material to a certain extent, so that the asphalt-like material can better adapt to the deformation of the road surface in different temperature environments. Moreover, the kitchen waste oil can enhance the adhesion between the asphalt-like material and the aggregate, thereby improving the mechanical strength and stability of the road surface, helping to resist the action of vehicle loads, improving the quality and durability of the road surface, and reducing the occurrence of road surface diseases.
[0008] The addition of waste petroleum resin can form strong intermolecular forces with other components in the asphalt-like material, thus effectively enhancing the internal cohesion of the asphalt-like material and improving the overall bonding strength and softening point temperature of the asphalt-like material. Moreover, waste petroleum resin can improve the bonding performance between the asphalt-like material and the base layer, increase the adhesion and friction between the two, make the asphalt-like material not easily separate from the base layer, and improve the overall stability of the road surface. More importantly, waste petroleum resin has certain heat resistance and cold resistance, which can reduce the temperature sensitivity of the asphalt-like material. In a high-temperature environment, it can reduce the fluidity of the asphalt-like material and keep the road surface in good flatness and rutting resistance; in a low-temperature environment, it can increase the flexibility of the material and prevent cracks from occurring on the road surface due to temperature shrinkage.
[0009] The raw materials of the waste fillers used in the present invention include waste glass fiber, straw residue, waste clay, and coal gangue powder. Among them, waste glass fiber has high strength and modulus, can effectively bear and transfer stress, and reduce stress concentration; moreover, waste glass fiber can play a role in skeleton support, it can limit the deformation of the asphalt-like material and prevent the expansion of microcracks, thereby enhancing the compressive capacity of the asphalt-like material and improving its road performance. Straw residue has a certain fiber structure and strength. When subjected to vehicle loads, it can share part of the stress, reduce the deformation and damage of the asphalt-like material, and extend the service life of the road surface material. Moreover, the unique fiber structure of straw residue has certain flexibility and elasticity, which can absorb and buffer the stress generated by low-temperature shrinkage and reduce the probability of cracks occurring in the road surface material in a low-temperature environment. Waste clay has certain high-temperature resistance characteristics, can improve the thermal stability of the asphalt-like material, and reduce the thermal expansion coefficient of the asphalt-like material. The particles of waste clay can also play a role as a dispersion medium, making the various components in the asphalt-like material more evenly distributed, which helps to improve the overall stability of the material. The addition of coal gangue powder can endow the asphalt-like material with high hardness and rigidity, improve the compressive strength and fatigue resistance of the road surface material, and extend the service life of the road surface material under alternating loads.
[0010] Preferably, the waste rubber powder is any one or more of waste styrene-butadiene rubber powder, waste ethylene-propylene rubber powder, or waste nitrile rubber powder.
[0011] Preferably, the waste plastic is waste PP plastic or waste PE plastic.
[0012] Preferably, the waste petroleum resin is waste C5 / C9 copolymerized petroleum resin.
[0013] Preferably, the length of the waste glass fiber is 0.3 mm - 0.6 mm.
[0014] Preferably, the specific surface area of the straw residue is 80 m 2 / g - 120 m 2 / g。
[0015] Preferably, the particle size of the waste bleaching clay is 0.1 mm - 0.5 mm.
[0016] Preferably, the particle size of the coal gangue powder is 100 μm - 200 μm.
[0017] The second aspect of the present invention provides a preparation method of the all-solid waste asphalt-like material, comprising the following steps: Step 1: Weigh each component raw material according to the designed ratio, mix the waste rubber powder and waste plastic evenly, disperse them in an organic solvent, add a degradation agent, and carry out a hydrothermal reaction at 160°C - 185°C under an inert atmosphere to obtain an organic degradation liquid; Step 2: Crush the waste filler, calcine it at 520°C - 600°C, and grind it to obtain a filler powder; Step 3: Add kitchen waste oil and waste petroleum resin to the organic degradation liquid, mix evenly, carry out a first heating at 120°C - 140°C, add the filler powder, then raise the temperature to 150°C - 200°C for a second heating, and cool to obtain the all-solid waste asphalt-like material.
[0018] Preferably, in Step 1, the organic solvent is a mixed solution of dimethyl sulfide, 1,4-dioxane, and toluene with a volume ratio of 1:2:10 - 3:5:10.
[0019] Preferably, in Step 1, the mass-volume ratio of the total mass of the waste rubber powder and waste plastic to the organic solvent is 1 g:3 mL - 1 g:5 mL.
[0020] Preferably, in Step 1, the degradation agent is a mixed solution of sodium hydroxide solution and tetrahydrofuran; wherein, the concentration of the sodium hydroxide solution is 0.5 mol / L - 1.0 mol / L; the volume ratio of the sodium hydroxide solution to tetrahydrofuran is 1:1 - 1:2.
[0021] Preferably, in Step 1, the addition amount of the degradation agent is 70% - 80% of the total mass of the waste rubber powder and waste plastic.
[0022] Preferably, in Step 1, the time of the hydrothermal reaction is 8 h - 10 h.
[0023] Preferably, in Step 2, the time of the calcination is 3 h - 4 h.
[0024] Preferably, in Step 2, the temperature is raised to 520°C - 600°C by means of programmed temperature rise, and the heating rate is 8°C / min - 10°C / min.
[0025] Preferably, in step two, the rotation speed of the grinding is 500 rpm - 1000 rpm, and the grinding time is 20 min - 40 min.
[0026] Preferably, in step three, the heat preservation time of the primary heating is 2 h - 3 h.
[0027] Preferably, in step three, the heat preservation time of the secondary heating is 3 h - 4 h.
[0028] The third aspect of the present invention provides an application of the all-solid waste asphalt-like material or the all-solid waste asphalt-like material prepared by the preparation method of the all-solid waste asphalt-like material in the preparation of pavement materials.
[0029] In summary, the all-solid waste asphalt-like material provided by the present invention has good road performance, low preparation cost, can effectively relieve the treatment pressure of solid waste, and the mechanical properties of the asphalt-like mixture prepared by using the all-solid waste asphalt-like material are excellent, with a dynamic stability of up to 3876 times / mm and a Marshall stability of up to 11.3 KN, providing a new idea for the development of pavement materials. Detailed Embodiments
[0030] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all of the embodiments. All other embodiments obtained by those of ordinary skill in the art based on the embodiments of the present invention without creative efforts shall fall within the protection scope of the present invention.
[0031] Example 1 This example provides an all-solid waste asphalt-like material and its preparation method, which specifically include the following contents: The all-solid waste asphalt-like material includes the following raw material components in parts by mass: 70 g of waste styrene-butadiene rubber powder, 40 g of waste PP plastic, 10 g of kitchen waste oil, 10 g of waste C5 / C9 copolymer petroleum resin, and 25 g of waste filler; the waste filler includes the following raw material components in mass percentage: 25% of waste glass fiber, 20% of straw residue, 18% of waste clay, and the balance of coal gangue powder.
[0032] Among them, the length of the waste glass fiber is 0.45 mm; the specific surface area of the straw residue is 100 m 2 / g; the particle size of the waste clay is 0.36 mm; the particle size of the coal gangue powder is 150 μm.
[0033] The preparation method of the all-solid waste asphalt-like material includes the following steps: Step 1: Weigh each component raw material according to the designed ratio. Mix the waste styrene-butadiene rubber powder and waste PP plastic evenly, disperse them in 400 mL of a mixed solvent of dimethyl sulfide, 1,4-dioxane and toluene with a volume ratio of 1:3:10. Add 80 g of a degradation agent, and carry out a hydrothermal reaction at 175 °C for 9 h under an inert atmosphere to obtain an organic degradation liquid. Among them, the degradation agent is a mixed solution of a sodium hydroxide solution and tetrahydrofuran with a volume ratio of 1:1.5, and the concentration of the sodium hydroxide solution is 0.8 mol / L.
[0034] Step 2: Crush the waste filler, and use a programmed heating method to heat it to 550 °C at a heating rate of 10 °C / min for calcination for 3.5 h. After cooling, grind it at a rotation speed of 800 rpm for 30 min to obtain filler powder.
[0035] Step 3: Add kitchen waste oil and waste petroleum resin to the organic degradation liquid, mix evenly, carry out a first heating at 130 °C for 2.5 h, add the filler powder, then raise the temperature to 180 °C for a second heating for 4 h, and cool to obtain a fully solid waste asphalt-like material.
[0036] Example 2 This example provides a fully solid waste asphalt-like material and its preparation method, which specifically includes the following content: The fully solid waste asphalt-like material includes the following raw material components in parts by mass: 68 g of waste ethylene-propylene rubber powder, 45 g of waste PE plastic, 12 g of kitchen waste oil, 12 g of waste C5 / C9 copolymerized petroleum resin, and 30 g of waste filler. The waste filler includes the following raw material components in mass percentage: 22% of waste glass fiber, 20% of straw residue, 20% of waste clay, and the balance of coal gangue powder.
[0037] Among them, the length of the waste glass fiber is 0.5 mm; the specific surface area of the straw residue is 120 m 2 / g; the particle size of the waste clay is 0.4 mm; the particle size of the coal gangue powder is 170 μm.
[0038] The preparation method of the fully solid waste asphalt-like material includes the following steps: Step 1: Weigh each component raw material according to the designed ratio. Mix the waste styrene-butadiene rubber powder and waste PP plastic evenly, disperse them in 400 mL of a mixed solvent of dimethyl sulfide, 1,4-dioxane and toluene with a volume ratio of 1:2:10. Add 80 g of a degradation agent, and carry out a hydrothermal reaction at 170 °C for 9 h under an inert atmosphere to obtain an organic degradation liquid. Among them, the degradation agent is a mixed solution of a sodium hydroxide solution and tetrahydrofuran with a volume ratio of 1:1.5, and the concentration of the sodium hydroxide solution is 0.5 mol / L.
[0039] Step 2: Crush the waste filler, and adopt a programmed heating method to heat it to 580 °C at a heating rate of 10 °C / min for calcination for 3.5 h. After cooling, grind it at a rotation speed of 800 rpm for 30 min to obtain filler powder.
[0040] Step 3: Add kitchen waste oil and waste petroleum resin to the organic degradation liquid, mix them evenly, heat them at 140 °C for the first time for 2.5 h, add the filler powder, then heat it up to 175 °C for the second time for 4 h, and cool it to obtain the all-solid waste asphalt-like material.
[0041] Example 3 This example provides an all-solid waste asphalt-like material and a preparation method thereof, which specifically include the following contents: The all-solid waste asphalt-like material includes the following raw material components in parts by mass: 72 g of waste nitrile rubber powder, 38 g of waste PP plastic, 8 g of kitchen waste oil, 12 g of waste C5 / C9 copolymerized petroleum resin, and 30 g of waste filler; the waste filler includes the following raw material components in mass percentage: 25% of waste glass fiber, 20% of straw residue, 18% of waste clay, and the balance of coal gangue powder.
[0042] Among them, the length of the waste glass fiber is 0.45 mm; the specific surface area of the straw residue is 100 m 2 / g; the particle size of the waste clay is 0.36 mm; the particle size of the coal gangue powder is 150 μm.
[0043] The preparation method of the all-solid waste asphalt-like material includes the following steps: Step 1: Weigh each component of raw materials according to the designed ratio, mix the waste styrene-butadiene rubber powder and waste PP plastic evenly, disperse them in 400 mL of a mixed solvent of dimethyl sulfide, 1,4-dioxane and toluene with a volume ratio of 2:5:10, add 80 g of a degradation agent, and carry out a hydrothermal reaction at 175 °C for 9 h in an inert atmosphere to obtain an organic degradation liquid; among them, the degradation agent is a mixed solution of a sodium hydroxide solution and tetrahydrofuran with a volume ratio of 1:1.5, and the concentration of the sodium hydroxide solution is 0.8 mol / L.
[0044] Step 2: Crush the waste filler, and adopt a programmed heating method to heat it to 600 °C at a heating rate of 10 °C / min for calcination for 3 h. After cooling, grind it at a rotation speed of 600 rpm for 40 min to obtain filler powder.
[0045] Step 3: Add kitchen waste oil and waste petroleum resin to the organic degradation liquid, mix them evenly, heat them at 130 °C for the first time for 2.5 h, add the filler powder, then heat it up to 190 °C for the second time for 4 h, and cool it to obtain the all-solid waste asphalt-like material.
[0046] Comparative Example 1 This comparative example provides a fully solid waste asphalt-like material and its preparation method. The difference from Example 1 is that the waste petroleum resin is replaced with an equal amount of waste epoxy resin, and other components and raw materials remain unchanged. The specific content is as follows: The fully solid waste asphalt-like material includes the following raw material components in parts by mass: 70 g of waste styrene-butadiene rubber powder, 40 g of waste PP plastic, 10 g of kitchen waste oil, 10 g of waste epoxy resin, and 25 g of waste filler; the waste filler includes the following raw material components in mass percentage: 25% of waste glass fiber, 20% of straw residue, 18% of waste clay, and the balance of coal gangue powder.
[0047] Among them, the length of the waste glass fiber is 0.45 mm; the specific surface area of the straw residue is 100 m 2 / g; the particle size of the waste clay is 0.36 mm; the particle size of the coal gangue powder is 150 μm.
[0048] The preparation method of the fully solid waste asphalt-like material includes the following steps: Step 1: Weigh each component of the raw materials according to the designed ratio. Mix the waste styrene-butadiene rubber powder and the waste PP plastic evenly, disperse them in 400 mL of a mixed solvent of dimethyl sulfide, 1,4-dioxane, and toluene with a volume ratio of 1:3:10, add 80 g of a degradation agent, and carry out a hydrothermal reaction at 175 °C for 9 h in an inert atmosphere to obtain an organic degradation solution; among them, the degradation agent is a mixed solution of a sodium hydroxide solution and tetrahydrofuran with a volume ratio of 1:1.5, and the concentration of the sodium hydroxide solution is 0.8 mol / L.
[0049] Step 2: Crush the waste filler, and use a programmed heating method to heat it to 550 °C at a heating rate of 10 °C / min for calcination for 3.5 h. After cooling, grind it at a rotation speed of 800 rpm for 30 min to obtain filler powder.
[0050] Step 3: Add the kitchen waste oil and the waste epoxy resin to the organic degradation solution, mix evenly, carry out a first heating at 130 °C for 2.5 h, add the filler powder, then raise the temperature to 180 °C for a second heating for 4 h, and cool to obtain the fully solid waste asphalt-like material.
[0051] Comparative Example 2 This comparative example provides a fully solid waste asphalt-like material and its preparation method. The difference from Example 1 is that the waste filler is replaced with an equal amount of coal gangue powder, and other components and raw materials remain unchanged. The specific content is as follows: The fully solid waste asphalt-like material includes the following raw material components in parts by mass: 70 g of waste styrene-butadiene rubber powder, 40 g of waste PP plastic, 10 g of kitchen waste oil, 10 g of waste C5 / C9 copolymerized petroleum resin, and 25 g of coal gangue powder.
[0052] Among them, the length of the waste glass fiber is 0.45 mm; the specific surface area of the straw residue is 100 m 2 / g; the particle size of the waste bleaching earth is 0.36 mm; the particle size of the coal gangue powder is 150 μm.
[0053] The preparation method of the all-solid waste asphalt-like material comprises the following steps: Step 1: Weigh each component raw material according to the designed ratio, mix the waste styrene-butadiene rubber powder and the waste PP plastic evenly, disperse them in 400 mL of a mixed solvent of dimethyl sulfide, 1,4-dioxane and toluene with a volume ratio of 1:3:10, add 80 g of a degradation agent, and carry out a hydrothermal reaction at 175 °C for 9 h under an inert atmosphere to obtain an organic degradation liquid; among them, the degradation agent is a mixed solution of a sodium hydroxide solution and tetrahydrofuran with a volume ratio of 1:1.5, and the concentration of the sodium hydroxide solution is 0.8 mol / L.
[0054] Step 2: Crush the coal gangue, and use a programmed heating method to heat it to 550 °C at a heating rate of 10 °C / min for calcination for 3.5 h. After cooling, grind it at a rotation speed of 800 rpm for 30 min to obtain a filler powder.
[0055] Step 3: Add kitchen waste oil and waste petroleum resin to the organic degradation liquid, mix evenly, carry out a first heating at 130 °C for 2.5 h, add the filler powder, and then raise the temperature to 180 °C for a second heating for 4 h, and cool to obtain the all-solid waste asphalt-like material.
[0056] Comparative Example 3 This comparative example provides an all-solid waste asphalt-like material, which is different from Example 1 in that: kitchen waste oil is not added, and other components and preparation processes remain unchanged. The specific contents are as follows: The all-solid waste asphalt-like material comprises the following raw material components in parts by mass: 70 g of waste styrene-butadiene rubber powder, 40 g of waste PP plastic, 10 g of waste 5 / C9 copolymerized petroleum resin, and 25 g of waste filler; the waste filler comprises the following raw material components in mass percentage: 25% of waste glass fiber, 20% of straw residue, 18% of waste bleaching earth, and the balance of coal gangue powder.
[0057] Among them, the length of the waste glass fiber is 0.45 mm; the specific surface area of the straw residue is 100 m 2 / g; the particle size of the waste bleaching earth is 0.36 mm; the particle size of the coal gangue powder is 150 μm.
[0058] The preparation method of the all-solid waste asphalt-like material comprises the following steps: Step 1: Weigh each component raw material according to the designed ratio. Mix the waste styrene-butadiene rubber powder and waste PP plastic evenly, disperse them in 400 mL of a mixed solvent of dimethyl sulfide, 1,4-dioxane, and toluene with a volume ratio of 1:3:10. Add 80 g of a degradation agent, and carry out a hydrothermal reaction at 175°C for 9 h in an inert atmosphere to obtain an organic degradation liquid. Among them, the degradation agent is a mixed solution of a sodium hydroxide solution and tetrahydrofuran with a volume ratio of 1:1.5, and the concentration of the sodium hydroxide solution is 0.8 mol / L.
[0059] Step 2: Crush the waste filler, and use a programmed heating method to heat it to 550°C at a heating rate of 10°C / min for calcination for 3.5 h. After cooling, grind it at a rotation speed of 800 rpm for 30 min to obtain filler powder.
[0060] Step 3: Add waste C5 / C9 copolymerized petroleum resin to the organic degradation liquid, mix evenly, carry out a first heating at 130°C for 2.5 h, add the filler powder, then raise the temperature to 180°C for a second heating for 4 h, and cool to obtain a fully solid waste asphalt-like material.
[0061] To further demonstrate the technical effects of the present invention, the present invention conducted the following performance tests on the fully solid waste asphalt-like materials obtained in Examples 1-3 and Comparative Examples 1-3: Refer to JTT798-2011 to conduct penetration tests, softening point tests, and ductility tests on each fully solid waste asphalt-like material. The results are shown in Table 1; refer to JTGE20-2011 to prepare asphalt mixtures for each fully solid waste asphalt-like material, and conduct Marshall stability tests and dynamic stability tests on the asphalt mixtures. The results are shown in Table 2.
[0062] Table 1 Performance test results of each fully solid waste asphalt-like material
[0063] Table 2 Performance test results of each asphalt mixture
[0064] The above are only the preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent replacements, or improvements made within the spirit and principles of the present invention shall be included within the protection scope of the present invention.
Claims
1. A solid waste imitation asphalt material, characterized by: The all-solid waste asphalt-like material includes the following raw material components by weight: 60-80 parts of waste rubber powder, 20-50 parts of waste plastics, 5-15 parts of waste kitchen grease, 5-15 parts of waste petroleum resin and 20-30 parts of waste fillers; The waste filler includes the following raw material components in percentage by mass: 20%-30% of waste glass fiber, 15%-20% of straw residue, 15%-20% of waste clay and the remainder of coal gangue powder.
2. The all-solid waste asphalt-like material according to claim 1, characterized in that: The waste rubber powder is any one or more of waste styrene-butadiene rubber powder, waste ethylene-propylene rubber powder or waste nitrile-butadiene rubber powder; and / or The waste plastic is waste PP plastic or waste PE plastic; and / or The waste petroleum resin is waste C5 / C9 copolymerized petroleum resin.
3. The all-solid waste asphalt-like material according to claim 1, characterized in that: The length of the waste glass fiber is 0.3mm-0.6mm; and / or The specific surface area of the straw residue is 80m 2 / g-120m 2 / g; and / or The particle size of the waste clay is 0.1 mm to 0.5 mm; and / or The particle size of the coal gangue powder is 100 μm-200 μm.
4. A method for preparing the all-solid waste asphalt-like material according to any one of claims 1 to 3, characterized in that: The steps include: Step 1: weigh the raw materials of each component according to the designed ratio, mix the waste rubber powder and waste plastic evenly, disperse them in an organic solvent, add a degradation agent, and perform a hydrothermal reaction at 160° C.-185° C. under an inert atmosphere to obtain an organic degradation liquid; Step 2: crushing the waste filler, calcining at 520°C-600°C, and grinding to obtain filler powder; Step 3: Add waste cooking oil and waste petroleum resin to the organic degradation liquid, mix well, heat once at 120°C-140°C, add the filler powder, heat to 150°C-200°C for secondary heating, and cool to obtain a full solid waste asphalt imitation material.
5. The method for preparing the all-solid waste asphalt-like material according to claim 4, characterized in that: In step 1, the organic solvent is dimethyl sulfide, 1,4-dioxane and toluene in a volume ratio of 1:2:10-3:5:10; and / or In step 1, the mass volume ratio of the total mass of the waste rubber powder and waste plastic to the organic solvent is 1g:3mL-1g:5mL.
6. The method for preparing the all-solid waste asphalt-like material according to claim 4, characterized in that: In step 1, the degradation agent is a mixed solution of sodium hydroxide solution and tetrahydrofuran; wherein the concentration of the sodium hydroxide solution is 0.5 mol / L-1.0 mol / L; the volume ratio of the sodium hydroxide solution to the tetrahydrofuran solution is 1:1-1:2; and / or In step 1, the amount of the degradation agent added is 70%-80% of the total mass of the waste rubber powder and waste plastics.
7. The method for preparing the all-solid waste asphalt-like material according to claim 4, characterized in that: In step 1, the hydrothermal reaction time is 8h-10h; and / or In step 2, the calcination time is 3h-4h.
8. The method for preparing the all-solid waste asphalt-like material according to claim 4, characterized in that: In step 2, the temperature is raised to 520°C-600°C by programmed heating at a heating rate of 8°C / min-10°C / min; and / or In step 2, the grinding speed is 500rpm-1000rpm, and the grinding time is 20min-40min.
9. The method for preparing the all-solid waste asphalt-like material according to claim 4, characterized in that: In step 3, the heating time is 2h-3h; and / or In step three, the insulation time of the secondary heating is 3h-4h.
10. Use of the all-solid waste asphalt-imitation material as claimed in any one of claims 1 to 3 or the all-solid waste asphalt-imitation material prepared by the method for preparing the all-solid waste asphalt-imitation material as claimed in any one of claims 4 to 9 in preparing pavement materials.
Citation Information
Patent Citations
Bituminous mixture for high-environment-protection road and construction method of bituminous mixture
CN106277941A
Anti-rut agent prepared by utilizing waste plastics and preparation method of anti-rut agent
CN106750791A
Green asphalt concrete-modified asphalt with high durability and preparation method thereof
CN107304112A
Asphalt concrete with improved environmental protection performance and preparation method thereof
CN114262176A
High-temperature-resistant warm-mixed rubber asphalt mixture as well as preparation method and application thereof
CN118754508A
Cited By
High-strength asphalt-based pavement material as well as preparation method and application thereof
CN120504891A