Self-cleaning photovoltaic super-hydrophobic coating based on nano-porous structure and preparation method of self-cleaning photovoltaic super-hydrophobic coating
By applying a self-cleaning superhydrophobic coating with nanoporous structures on photovoltaic panels, combined with the photocatalytic effect of micro-nano composite structure and TiO2, the problem of pollutant removal of photovoltaic panels is solved, and efficient dynamic hydrophobic, photocatalytic decomposition and wear resistance are achieved, which significantly improves the power generation efficiency of the photovoltaic system and the service life of the coating.
Patent Information
- Application Number
- CN202510426576.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-04-07
- Publication Date
- 2025-06-17
AI Technical Summary
Photovoltaic panels are prone to accumulate pollutants in outdoor environments, resulting in power loss and material corrosion. Traditional superhydrophobic coatings are difficult to effectively remove organic pollutants, and have low hardness and short service life.
A self-cleaning photovoltaic superhydrophobic coating based on nanoporous structure is adopted, which contains nanoporous silica, low surface energy modifier, photocatalytic nanotitanium dioxide and silicone resin. Through the micro-nano composite structure and the photocatalytic effect of TiO2, dynamic hydrophobic, photocatalytic decomposition and wear resistance are achieved.
This coating can effectively remove more than 90% of dust and bird droppings and other pollutants, increase light transmittance by 2%-5%, gain power generation by 5%-15%, and the coating life is up to 5-8 years. It is suitable for diverse climate environments, and has high hardness and wear resistance.
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of photovoltaic panel coatings, and particularly relates to a self-cleaning photovoltaic superhydrophobic coating based on a nanoporous structure and a preparation method thereof. Background Art
[0002] Photovoltaic panels are long-term exposed to outdoor environments, and their surfaces are prone to accumulating various pollutants such as dust, sand, bird droppings, and industrial pollutants. According to research, when a photovoltaic power station has not been cleaned for a long time, the average power loss can reach 15.27%. Moreover, acidic substances in the pollutants can corrode the surface materials of the components, resulting in a decrease in the photoelectric conversion efficiency, hot spot effect, and even a shortening of the component lifespan. Organic substances such as bird droppings form sticky dirt on the surface of the components, and their adhesiveness far exceeds that of ordinary dust, making it difficult for traditional superhydrophobic coatings combined with rainwater to effectively remove them. In addition, most coatings only focus on hydrophobic performance and lack the ability to decompose organic pollutants such as bird droppings, resulting in the long-term residue of pollutants. For traditional superhydrophobic coatings, after being washed by rainwater, water stains are easily formed on the coating surface or pollutants are re-adsorbed, the self-cleaning efficiency is unstable, and the coating has low hardness and is prone to wear and fall off under environments such as sand and dust and ultraviolet rays, and its service life is usually only 2 - 3 years. Additionally, some coatings require high-temperature curing (>100°C) or special equipment to achieve coating performance, making it difficult to adapt to complex scenarios such as distributed rooftop photovoltaics.
[0003] In view of the above problems, there is an urgent need to develop a superhydrophobic coating with both photocatalytic decomposition, dynamic hydrophobicity, and long-term wear resistance performance, which is of great significance for improving the power generation efficiency of photovoltaic systems and reducing the full life cycle cost. Summary of the Invention
[0004] In order to overcome the above-mentioned disadvantages of the prior art, the purpose of the present invention is to provide a self-cleaning photovoltaic superhydrophobic coating based on a nanoporous structure and a preparation method thereof. This coating has superhydrophobicity, photocatalytic decomposition of organic substances, and wear resistance performance, and can solve problems such as dust accumulation, bird droppings, and organic pollution on photovoltaic panels, and improve the power generation efficiency of photovoltaic systems.
[0005] To achieve the above purpose, the present invention adopts the following technical solutions:
[0006] The present invention provides a self-cleaning photovoltaic superhydrophobic coating based on a nanoporous structure, which, by mass percentage, includes 15 - 25% of nanoporous silica particles, 5 - 10% of low surface energy modifiers, 3 - 8% of photocatalytic nano-titanium dioxide, 30 - 40% of silicone resin, and the balance is deionized water.
[0007] In one embodiment, the particle size of the nanoporous silica particles is 10 - 50 nm.
[0008] In one embodiment, the low surface energy modifier is perfluorodecyltrimethoxysilane, perfluorooctyltriethoxysilane, or octadecyltrimethoxysilane.
[0009] In one embodiment, the pore size of the photocatalytic nano-titanium dioxide is 5 - 15 nm.
[0010] The present invention also provides a method for preparing a self-cleaning photovoltaic superhydrophobic coating based on a nanoporous structure, comprising the following steps:
[0011] Ultrasonically disperse nanoporous silica particles and photocatalytic nano-titanium dioxide in deionized water, add a low surface energy modifier and stir to obtain a dispersion; add an organosilicon resin as a film-forming agent to the dispersion, heat and stir to obtain a coating;
[0012] Spray or scrape the coating onto the surface of the photovoltaic panel and then dry it to form a coating;
[0013] Perform a curing treatment on the coating, and then crosslink it by ultraviolet irradiation to obtain a self-cleaning photovoltaic superhydrophobic coating based on a nanoporous structure.
[0014] In one embodiment, the temperature of the heat stirring is 70 - 80 °C, and the time is 1 - 2 h.
[0015] In one embodiment, the temperature of the drying is 70 - 80 °C, and the time is 1 - 2 h.
[0016] In one embodiment, the curing treatment is carried out at room temperature, and the time of the curing treatment is 24 - 30 h; the wavelength of the ultraviolet irradiation is 365 - 400 nm, and the intensity is 500 - 800 mW / cm 2 .
[0017] In one embodiment, the thickness of the coating is 0.3 - 0.5 μm.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] The present invention provides a superhydrophobic coating for self-cleaning photovoltaic panels based on a nano-porous structure. Among them, nano-silica can form a Wenzel rough structure to enhance hydrophobicity; a low surface energy modifier can reduce the surface energy. Photocatalytic nano-titanium dioxide can decompose organic substances and enhance wear resistance. Organosilicon resin can be used as a film-forming agent to improve adhesion and weather resistance. The contact angle of the coating is increased through a micro-nano composite structure, and TiO2 photocatalytically decomposes the organic substances in bird droppings, reducing the adhesion. After being washed by rain, more than 90% of pollutants such as dust and bird droppings can be taken away. The light reflection loss is reduced, the light transmittance is increased by 2%-5%, and combined with the photocatalytic decomposition of organic substances, the comprehensive power generation gain reaches 5%-15%. The entire coating system adopts an aqueous system, without volatile organic compounds, uses deionized water as a solvent, and there are no residual pollutants after construction. The operation and maintenance cost is greatly reduced, and the coating life is up to 5-8 years. It is high temperature resistant (>80°C), resistant to salt spray corrosion, and suitable for diverse climate scenarios such as deserts and coasts. The hardness of the coating enhanced by TiO2 reaches 6H, and the performance is stable after 30 times of tape peeling, far exceeding the wear resistance life of traditional coatings. Detailed implementation manners
[0020] To enable those skilled in the art to understand the features and effects of the present invention, the following provides a general description and definition of the terms and phrases mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used herein shall have the ordinary meaning understood by those skilled in the art regarding the present invention. In case of conflict, the definition in this specification shall prevail.
[0021] The theories or mechanisms described and disclosed herein, whether correct or incorrect, shall in no way limit the scope of the present invention, that is, the content of the present invention can be implemented without being limited by any specific theory or mechanism.
[0022] In this article, all features defined in the form of numerical ranges or percentage ranges, such as numerical values, quantities, contents, and concentrations, are only for the sake of brevity and convenience. Accordingly, the description of numerical ranges or percentage ranges should be regarded as having covered and specifically disclosed all possible sub-ranges and individual numerical values within the range (including integers and fractions).
[0023] In this article, unless otherwise specified, terms such as "comprising", "including", "containing", "having", or similar terms cover the meanings of "consisting of" and "mainly consisting of". For example, "A comprises a" covers the meanings of "A comprises a and others" and "A only comprises a".
[0024] In this article, for the sake of concise description, all possible combinations of all technical features in each embodiment or example are not described. Therefore, as long as there is no contradiction in the combination of these technical features, the technical features in each embodiment or example can be combined arbitrarily, and all possible combinations should be considered as the scope described in this specification.
[0025] The present invention provides a superhydrophobic coating for self-cleaning photovoltaic panels based on a nanoporous structure. By mass percentage, the raw materials of the superhydrophobic coating for self-cleaning photovoltaic panels based on a nanoporous structure include 15-25% nanoporous silica (SiO2), 5-10% low surface energy modifier, 3-8% photocatalytic nano-titanium dioxide (TiO2), 30-40% silicone resin, and the balance is deionized water.
[0026] Among them, the nano-silica can form a Wenzel rough structure to enhance hydrophobicity; the low surface energy modifier, which is any one of perfluorodecyltrimethoxysilane, perfluorooctyltriethoxysilane, and octadecyltrimethoxysilane, preferably perfluorodecyltrimethoxysilane, can reduce the surface energy to below 20 mN / m. The photocatalytic nano-titanium dioxide can decompose organic substances and enhance wear resistance. The silicone resin can be used as a film-forming agent to improve adhesion and weather resistance.
[0027] Among them, the particle size of the nanoporous silica particles is 10-50 nm; the pore size of the photocatalytic nano-titanium dioxide is 5-15 nm.
[0028] The present invention also provides a preparation method for a superhydrophobic coating for self-cleaning photovoltaic panels based on a nanoporous structure, including nanoparticle dispersion, coating preparation, coating application, curing, and post-treatment carried out in sequence; the above processes are as follows:
[0029] Step 1: Nanoparticle dispersion:
[0030] Disperse the nanoporous silica particles SiO2 (particle size 10-50 nm) and photocatalytic nano-titanium dioxide TiO2 (anatase type) ultrasonically in deionized water, add the low surface energy modifier, and stir for 30 minutes to obtain a dispersion.
[0031] Step 2: Coating preparation:
[0032] Add the silicone resin as a film-forming agent to the dispersion, heat and stir to obtain a coating.
[0033] Step 3: Coating application:
[0034] Spray or scrape the coating on the surface of the photovoltaic panel, and dry it with hot air at 70-80 °C for 1-2 hours to form a coating with a thickness of 0.3-0.5 μm.
[0035] Step 4: Curing and post-treatment:
[0036] The coating is cured at room temperature for 24-30 hours, and crosslinked by ultraviolet irradiation (wavelength 365-400 nm, intensity 500-800 mW / cm 2 ) to improve the wear resistance to more than 10,000 times.
[0037] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and not to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the appended claims of this application.
[0038] Conventional instrumentation and equipment in the art are used in the following embodiments. For the experimental methods without specific conditions noted in the following embodiments, they are generally carried out under conventional conditions or according to the conditions recommended by the manufacturer. Various raw materials are used in the following embodiments. Unless otherwise stated, commercially available products are used, and their specifications are the conventional specifications in the art. In the specification of the present invention and the following embodiments, unless otherwise specified, "%" represents weight percentage, "parts" represents weight parts, and the ratio represents weight ratio.
[0039] Example 1
[0040] On the one hand, this embodiment provides a self-cleaning photovoltaic superhydrophobic coating based on a nanoporous structure. By mass percentage, it includes 25% of nanoporous silica particles, 10% of a low surface energy modifier, 8% of photocatalytic nano-titanium dioxide, 40% of silicone resin, and the balance is deionized water. Among them, the low surface energy modifier is perfluorodecyltrimethoxysilane.
[0041] On the other hand, this embodiment provides a method for preparing a self-cleaning photovoltaic superhydrophobic coating based on a nanoporous structure, including the following steps:
[0042] Step 1: Nanoparticle dispersion:
[0043] Disperse nanoporous silica particles SiO2 (particle size 10 - 50 nm) and photocatalytic nano-titanium dioxide TiO2 (anatase type) in deionized water by ultrasonic dispersion, add a low surface energy modifier, and stir for 30 minutes to obtain a dispersion.
[0044] Step 2: Coating preparation:
[0045] Add silicone resin as a film-forming agent to the dispersion, heat to 80 °C and stir for 2 hours to obtain a coating.
[0046] Step 3: Coating application:
[0047] Spray or scrape the coating on the surface of the photovoltaic panel, and dry it with hot air at 80 °C for 1 hour to form a coating with a thickness of 0.3 - 0.5 μm.
[0048] Step 4: Curing and post-treatment:
[0049] The coating is cured at room temperature for 24 hours and crosslinked by ultraviolet irradiation (wavelength 365 nm, intensity 500 mW / cm 2 ), improving the wear resistance to more than 10,000 times.
[0050] Example 2
[0051] On the one hand, this example provides a self-cleaning photovoltaic superhydrophobic coating based on a nanoporous structure. By mass percentage, it includes 15% of nanoporous silica particles, 5% of a low surface energy modifier, 3% of photocatalytic nano-titanium dioxide, 30% of silicone resin, and the balance is deionized water. Among them, the low surface energy modifier is perfluorodecyltrimethoxysilane.
[0052] On the other hand, this example provides a preparation method for a self-cleaning photovoltaic superhydrophobic coating based on a nanoporous structure, including the following steps:
[0053] Step 1: Nanoparticle dispersion:
[0054] The nanoporous silica particles SiO2 (particle size 10 - 50 nm) and photocatalytic nano-titanium dioxide TiO2 (anatase type) are ultrasonically dispersed in deionized water, and the low surface energy modifier is added, followed by stirring for 30 minutes to obtain a dispersion.
[0055] Step 2: Coating preparation:
[0056] The silicone resin is added as a film-forming agent to the dispersion, and the mixture is heated to 70 °C and stirred for 2 hours to obtain a coating.
[0057] Step 3: Coating application:
[0058] The coating is sprayed or scrape-coated on the surface of the photovoltaic panel and dried with hot air at 70 °C for 1 hour to form a coating with a thickness of 0.3 - 0.5 μm.
[0059] Step 4: Curing and post-treatment:
[0060] The coating is cured at room temperature for 24 hours and crosslinked by ultraviolet irradiation (wavelength 380 nm, intensity 500 mW / cm 2 ), improving the wear resistance to more than 10,000 times.
[0061] Example 3
[0062] On the one hand, this example provides a self-cleaning photovoltaic superhydrophobic coating based on a nanoporous structure. By mass percentage, it includes 20% of nanoporous silica particles, 5% of a low surface energy modifier, 5% of photocatalytic nano-titanium dioxide, 30% of silicone resin, and the balance is deionized water. Among them, the low surface energy modifier is perfluorodecyltrimethoxysilane.
[0063] On the other hand, this embodiment provides a method for preparing a self-cleaning photovoltaic superhydrophobic coating based on a nanoporous structure, including the following steps:
[0064] Step 1: Nanoparticle dispersion:
[0065] Disperse nanoporous silica particles SiO2 (particle size 10 - 50 nm) and photocatalytic nano-titanium dioxide TiO2 (anatase type) in deionized water by ultrasonic dispersion, add a low surface energy modifier, and stir for 30 minutes to obtain a dispersion.
[0066] Step 2: Coating preparation:
[0067] Add silicone resin as a film-forming agent to the dispersion, heat to 80 °C and stir for 1 hour to obtain a coating.
[0068] Step 3: Coating application:
[0069] Spray or scrape the coating on the surface of the photovoltaic panel, and dry it with hot air at 80 °C for 1 hour to form a coating with a thickness of 0.3 - 0.5 μm.
[0070] Step 4: Curing and post-treatment:
[0071] The coating is cured at room temperature for 30 hours and crosslinked by ultraviolet irradiation (wavelength 365 nm, intensity 500 mW / cm 2 ) to improve the wear resistance to more than 10,000 times.
[0072] Example 4
[0073] On one hand, this embodiment provides a self-cleaning photovoltaic superhydrophobic coating based on a nanoporous structure, which, by mass percentage, includes 25% of nanoporous silica particles, 8% of a low surface energy modifier, 5% of photocatalytic nano-titanium dioxide, 35% of silicone resin, and the balance is deionized water. Among them, the low surface energy modifier is perfluorodecyltrimethoxysilane.
[0074] On the other hand, this embodiment provides a method for preparing a self-cleaning photovoltaic superhydrophobic coating based on a nanoporous structure, including the following steps:
[0075] Step 1: Nanoparticle dispersion:
[0076] Disperse nanoporous silica particles SiO2 (particle size 10 - 50 nm) and photocatalytic nano-titanium dioxide TiO2 (anatase type) in deionized water by ultrasonic dispersion, add a low surface energy modifier, and stir for 30 minutes to obtain a dispersion.
[0077] Step 2: Coating preparation:
[0078] The silicone resin is added to the dispersion as a film-forming agent, heated to 75 °C and stirred for 2 hours to obtain a coating.
[0079] Step 3: Coating application:
[0080] The coating is sprayed or knife-coated on the surface of the photovoltaic panel and dried with hot air at 75 °C for 1 hour to form a coating with a thickness of 0.3 - 0.5 μm.
[0081] Step 4: Curing and post-treatment:
[0082] The coating is cured at room temperature for 24 hours and crosslinked by ultraviolet irradiation (wavelength 400 nm, intensity 800 mW / cm 2 ) to improve the abrasion resistance to more than 10,000 times.
[0083] Example 5
[0084] On the one hand, this example provides a self-cleaning photovoltaic superhydrophobic coating based on a nanoporous structure, which, by mass percentage, includes 20% of nanoporous silica particles, 5% of a low surface energy modifier, 8% of photocatalytic nano-titania, 35% of silicone resin, and the balance is deionized water. Among them, the low surface energy modifier is perfluorodecyltrimethoxysilane.
[0085] On the other hand, this example provides a preparation method of a self-cleaning photovoltaic superhydrophobic coating based on a nanoporous structure, including the following steps:
[0086] Step 1: Nanoparticle dispersion:
[0087] The nanoporous silica particles SiO2 (particle size 10 - 50 nm) and photocatalytic nano-titania TiO2 (anatase type) are ultrasonically dispersed in deionized water, the low surface energy modifier is added, and stirred for 30 minutes to obtain a dispersion.
[0088] Step 2: Coating preparation:
[0089] The silicone resin is added to the dispersion as a film-forming agent, heated to 80 °C and stirred for 1 hour to obtain a coating.
[0090] Step 3: Coating application:
[0091] The coating is sprayed or knife-coated on the surface of the photovoltaic panel and dried with hot air at 80 °C for 1 hour to form a coating with a thickness of 0.3 - 0.5 μm.
[0092] Step 4: Curing and post-treatment:
[0093] The coating is cured at room temperature for 30 hours and crosslinked by ultraviolet irradiation (wavelength 365 nm, intensity 500 mW / cm 2 ) to improve the abrasion resistance to more than 10,000 times.
[0094] Example 6
[0095] On the one hand, this example provides a self-cleaning photovoltaic superhydrophobic coating based on a nanoporous structure. By mass percentage, it includes 18% of nanoporous silica particles, 10% of a low surface energy modifier, 8% of photocatalytic nano-titanium dioxide, 30% of silicone resin, and the balance is deionized water. Among them, the low surface energy modifier is octadecyltrimethoxysilane.
[0096] On the other hand, this example provides a preparation method for a self-cleaning photovoltaic superhydrophobic coating based on a nanoporous structure, including the following steps:
[0097] Step 1: Nanoparticle dispersion:
[0098] Disperse nanoporous silica particles SiO2 (particle size 10 - 50 nm) and photocatalytic nano-titanium dioxide TiO2 (anatase type) in deionized water by ultrasonic dispersion, add a low surface energy modifier, and stir for 30 minutes to obtain a dispersion.
[0099] Step 2: Coating preparation:
[0100] Add silicone resin as a film-forming agent to the dispersion, heat to 70°C and stir for 2 hours to obtain a coating.
[0101] Step 3: Coating application:
[0102] Spray or scrape the coating on the surface of the photovoltaic panel, and dry it with hot air at 70°C for 2 hours to form a coating with a thickness of 0.3 - 0.5 μm.
[0103] Step 4: Curing and post-treatment:
[0104] The coating is cured at room temperature for 24 hours and crosslinked by ultraviolet irradiation (wavelength 385 nm, intensity 600 mW / cm 2 ) to improve the wear resistance to more than 10,000 times.
[0105] Example 7
[0106] On the one hand, this example provides a self-cleaning photovoltaic superhydrophobic coating based on a nanoporous structure. By mass percentage, it includes 25% of nanoporous silica particles, 5% of a low surface energy modifier, 3% of photocatalytic nano-titanium dioxide, 35% of silicone resin, and the balance is deionized water. Among them, the low surface energy modifier is perfluorooctyltriethoxysilane.
[0107] On the other hand, this example provides a preparation method for a self-cleaning photovoltaic superhydrophobic coating based on a nanoporous structure, including the following steps:
[0108] Step 1: Nanoparticle Dispersion:
[0109] Disperse nanoporous silica particles SiO2 (particle size 10 - 50 nm) and photocatalytic nano-titanium dioxide TiO2 (anatase type) ultrasonically in deionized water, add a low surface energy modifier, and stir for 30 minutes to obtain a dispersion.
[0110] Step 2: Coating Preparation:
[0111] Add silicone resin as a film-forming agent to the dispersion, heat to 75 °C and stir for 2 hours to obtain a coating.
[0112] Step 3: Coating Coating:
[0113] Spray or scrape the coating onto the surface of the photovoltaic panel, and dry it with hot air at 75 °C for 2 hours to form a coating with a thickness of 0.3 - 0.5 μm.
[0114] Step 4: Curing and Post-treatment:
[0115] The coating is cured at room temperature for 30 hours and crosslinked by ultraviolet irradiation (wavelength 365 nm, intensity 500 mW / cm 2 ) to improve the wear resistance to more than 10,000 times.
[0116] Example 8
[0117] This example provides a self-cleaning photovoltaic superhydrophobic coating based on a nanoporous structure. By mass percentage, it includes 20% nanoporous silica particles, 10% low surface energy modifier, 3% photocatalytic nano-titanium dioxide, 35% silicone resin, and the balance is deionized water. Among them, the low surface energy modifier is octadecyltrimethoxysilane.
[0118] This example also provides a preparation method of a self-cleaning photovoltaic superhydrophobic coating based on a nanoporous structure, including the following steps:
[0119] Step 1: Nanoparticle Dispersion:
[0120] Disperse nanoporous silica particles SiO2 (particle size 10 - 50 nm) and photocatalytic nano-titanium dioxide TiO2 (anatase type) ultrasonically in deionized water, add a low surface energy modifier, and stir for 30 minutes to obtain a dispersion.
[0121] Step 2: Coating Preparation:
[0122] Add silicone resin as a film-forming agent to the dispersion, heat to 75 °C and stir for 2 hours to obtain a coating.
[0123] Step 3: Coating Coating:
[0124] Spray or scrape the coating on the surface of the photovoltaic panel and dry it with hot air at 75 °C for 2 hours to form a coating with a thickness of 0.3 - 0.5 μm.
[0125] Step 4: Curing and post-treatment:
[0126] The coating is cured at room temperature for 30 hours and crosslinked by ultraviolet irradiation (wavelength 400 nm, intensity 500 mW / cm 2 ) to improve the abrasion resistance to more than 10,000 times.
[0127] The coating increases the surface contact angle through the design of the micro-nano composite structure and decomposes the organic matter in bird droppings by using the photocatalytic effect of TiO2, thereby reducing the adhesion of pollutants. After being washed by rain, more than 90% of the pollutants such as dust and bird droppings can be removed from the surface. At the same time, the coating effectively reduces the light reflection loss, increases the light transmittance by 2% - 5%, and combines with the function of photocatalytic decomposition of organic matter, and the comprehensive power generation gain reaches 5% - 15%. The entire coating system uses an aqueous formulation, uses deionized water as a solvent, does not contain volatile organic compounds, and has no residual pollutants after construction. The coating has low operation and maintenance costs, a service life of up to 5 - 8 years, has the properties of high temperature resistance (exceeding 80 °C) and salt spray corrosion resistance, and can adapt to various climate environments such as deserts and coasts. In addition, the addition of TiO2 makes the coating hardness reach 6H, and the performance remains stable after 30 tape peeling tests.
[0128] The above content is only to illustrate the technical idea of the present invention, and the protection scope of the present invention cannot be limited thereby. Any modification made on the basis of the technical solution according to the technical idea proposed by the present invention falls within the protection scope of the claims of the present invention.
Claims
1. A self-cleaning photovoltaic super-hydrophobic coating based on a nanoporous structure, characterized in that: In terms of mass percentage, the invention comprises 15-25% of nano porous silicon dioxide particles, 5-10% of low surface energy modifier, 3-8% of photocatalytic nano titanium dioxide, 30-40% of organic silicon resin, and the balance is deionized water.
2. The self-cleaning photovoltaic super-hydrophobic coating based on nanoporous structure according to claim 1, characterized in that: The particle size of the nanoporous silica particles is 10-50 nm.
3. The self-cleaning photovoltaic super-hydrophobic coating based on nanoporous structure according to claim 1, characterized in that: The low surface energy modifier is perfluorodecyltrimethoxysilane, perfluorooctyltriethoxysilane, or octadecyltrimethoxysilane.
4. The self-cleaning photovoltaic super-hydrophobic coating based on nanoporous structure according to claim 1, characterized in that: The pore size of the photocatalytic nano titanium dioxide is 5-15 nm.
5. A method for preparing a self-cleaning photovoltaic super-hydrophobic coating based on a nanoporous structure according to any one of claims 1 to 4, characterized in that: The following steps are involved: The nanoporous silica particles and the photocatalytic nano-titanium dioxide are ultrasonically dispersed in deionized water, and a low surface energy modifier is added and stirred to obtain a dispersion liquid; an organic silicone resin is added into the dispersion liquid as a film-forming agent, and the coating is obtained by heating and stirring; Spray or scrape the coating onto the surface of the photovoltaic panel and then dry it to form a coating; The coating is cured and then cross-linked by ultraviolet radiation to produce a self-cleaning photovoltaic super-hydrophobic coating based on a nanoporous structure.
6. The method for preparing a self-cleaning photovoltaic super-hydrophobic coating based on a nanoporous structure according to claim 5, characterized in that: The heating and stirring is performed at a temperature of 70-80° C. and for a time of 1-2 h.
7. The method for preparing a self-cleaning photovoltaic super-hydrophobic coating based on a nanoporous structure according to claim 5, characterized in that: The drying temperature is 70-80°C and the drying time is 1-2h.
8. The method for preparing a self-cleaning photovoltaic super-hydrophobic coating based on a nanoporous structure according to claim 5, characterized in that: The curing treatment is carried out at room temperature, and the curing treatment time is 24-30 hours.
9. The method for preparing a self-cleaning photovoltaic super-hydrophobic coating based on a nanoporous structure according to claim 5, characterized in that: The wavelength of the ultraviolet radiation is 365-400nm, and the intensity is 500-800mW / cm 2 .
10. The method for preparing a self-cleaning photovoltaic super-hydrophobic coating based on a nanoporous structure according to claim 5, characterized in that: The coating has a thickness of 0.3-0.5 μm.
Citation Information
Cited By
Photovoltaic panel self-cleaning nano coating in alpine region and preparation method of photovoltaic panel self-cleaning nano coating
CN121574581A
Self-cleaning nano-coating for photovoltaic panels in alpine regions and method for its preparation
CN121574581B
Super-hydrophobic self-cleaning coating for photovoltaic panel and preparation method of super-hydrophobic self-cleaning coating
CN121991567A