Porous adsorption material for water environment purification treatment as well as preparation method and application of porous adsorption material
Through the porous adsorption materials of specific formulations and preparation processes, the problem of insufficient adsorption capacity and stability of existing materials in water purification is solved, and efficient removal of metal ions and organic pollutants is achieved, and good stability and recyclability is achieved.
Patent Information
- Application Number
- CN202510521593.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-04-24
- Publication Date
- 2025-07-01
- Estimated Expiration
- 2045-04-24
AI Technical Summary
The existing porous adsorption materials have limited adsorption capacity, low selectivity, poor stability and difficult to recycle and reuse in water purification treatment, which limits their wide application.
A specific formula of porous adsorption materials, including matrix materials, crosslinkers, pore-generating agents, stabilizers, nanosilica and carboxylic functional graphene, is used to form a multi-stage pore structure through hot water bath prepolymerization, ultrasonic dispersion and template pore making technology, and stabilizers are used to enhance the stability and adsorption properties of the material.
It significantly improves adsorption capacity and selectivity, the material has good stability in complex water environments, and is recyclable, reducing the cost of use, and has excellent metal ion and organic pollutant removal effect.
Smart Images

Figure CN120227858A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of water purification materials, and particularly relates to a porous adsorption material for water environment purification treatment, its preparation method and application. Background Art
[0002] With the acceleration of the industrialization process and the continuous growth of the population, the problem of water pollution has become increasingly severe, posing a serious threat to the ecological environment and human health. A large amount of wastewater generated during industrial production contains harmful substances such as high-concentration metal ions and organic pollutants. If directly discharged without effective treatment, it will pollute water resources such as rivers, lakes, and groundwater. Agricultural non-point source pollution cannot be ignored either. Excessive use of chemical fertilizers and pesticides enters water bodies with rainwater runoff, causing problems such as eutrophication of water bodies. In addition, the random discharge of domestic sewage also increases the load of water pollution.
[0003] Currently, there are various methods for water purification treatment, including physical methods, chemical methods, and biological methods, etc. Physical methods such as sedimentation and filtration can remove some suspended solids and large particle impurities, but have limited treatment effects on dissolved pollutants. Chemical methods convert pollutants into harmless substances or forms that are easy to separate through chemical reactions, such as chemical precipitation, oxidation-reduction, etc., but may cause secondary pollution and have relatively high treatment costs. Biological methods utilize the metabolic functions of microorganisms to decompose organic pollutants, but the treatment speed is relatively slow, and the treatment effects on high-concentration or difficult-to-degrade pollutants are not good.
[0004] As a new water treatment technology, adsorption technology has received extensive attention due to its advantages such as simple operation, high treatment efficiency, and relatively low cost. Porous adsorption materials play a key role in the adsorption process. They have a large specific surface area and a rich pore structure, which can provide more adsorption sites for pollutants, thereby effectively removing metal ions and organic pollutants in water bodies. However, existing porous adsorption materials still have some deficiencies, such as limited adsorption capacity, low selectivity, poor stability in complex water environments, and difficulty in recycling and reuse. These problems limit their wide application in actual water purification treatment. Therefore, developing a porous adsorption material for water environment purification treatment with high adsorption capacity, high selectivity, good stability, and recyclability has important practical significance for solving the current water pollution problem. Summary of the Invention
[0005] The purpose of the present invention is to provide a porous adsorption material for water environment purification treatment with high adsorption capacity, high selectivity, good stability, and recyclability in view of the problems existing in the prior art, so as to overcome the deficiencies of the prior art.
[0006] To achieve the above object, the technical solution adopted by the present invention is as follows: A porous adsorbent material for water environment purification treatment, characterized in that it comprises the following components in parts by weight: 30-50 parts of matrix material, 5-15 parts of cross-linking agent, 10-25 parts of pore-forming agent, 1-5 parts of stabilizer, 10-15 parts of nano-silica, and 5-8 parts of carboxyl-functionalized graphene;
[0007] Further, the stabilizer has the structure shown in Formula 1;
[0008]
[0009] In Formula 1, R1-R2 are the same or different and are selected from: alkyl groups having 1-5 carbon atoms, alkoxy groups having 1-5 carbon atoms, heteroaryl groups having 4- 10 carbon atoms, and aryl groups having 6- 15 carbon atoms;
[0010] Or R1 and R2 are the same or different and independently selected from: heteroaryl groups having 4- 10 carbon atoms and aryl groups having 6- 15 carbon atoms, which are substituted by alkyl groups having 1-5 carbon atoms, alkoxy groups having 1-5 carbon atoms, deuterated alkyl groups having 1-5 carbon atoms, and deuterated alkoxy groups having 1-5 carbon atoms;
[0011] Or R1 and R2 are the same or different and independently selected from: deuterated alkyl groups having 1-5 carbon atoms, deuterated alkoxy groups having 1-5 carbon atoms, deuterated heteroaryl groups having 4- 10 carbon atoms, and deuterated aryl groups having 6- 15 carbon atoms;
[0012] In Formula 1, R3 is selected from: alkyl groups having 1-5 carbon atoms, aryl groups having 6- 15 carbon atoms, deuterated alkyl groups having 1-5 carbon atoms, and deuterated aryl groups having 6- 15 carbon atoms;
[0013] Or R3 is selected from: aryl groups having 6- 15 carbon atoms and deuterated aryl groups having 6- 15 carbon atoms, which are substituted by alkyl groups having 1-5 carbon atoms, deuterated alkyl groups having 1-5 carbon atoms, and alkoxy groups having 1-5 carbon atoms.
[0014] Further, the alkyl group having 1-5 carbon atoms is selected from: methyl, ethyl, propyl, tert-butyl; the deuterated alkyl group having 1-5 carbon atoms is selected from: deuterated methyl, deuterated ethyl, deuterated propyl, deuterated tert-butyl.
[0015] Further, the alkoxy group having 1-5 carbon atoms is selected from: methoxy, ethoxy; the deuterated alkoxy group having 1-5 carbon atoms is selected from: deuterated methoxy, deuterated ethoxy.
[0016] Further, the C4- 10The heteroaryl group is selected from: furyl, thienyl; C6-C 15 The aryl group is selected from: phenyl, naphthyl, biphenyl; C4-C 10 The deuterated heteroaryl group is selected from: deuterated furyl, deuterated thienyl; C6-C 15 The deuterated aryl group is selected from: deuterated phenyl, deuterated naphthyl, deuterated biphenyl.
[0017] Furthermore, the stabilizer is selected from any one of the compounds represented by the following structures:
[0018]
[0019]
[0020]
[0021]
[0022] Where D represents deuterium.
[0023] Furthermore, the preparation method of the stabilizer is as shown in Figure 1 :
[0024]
[0025] The first step: Raw material 1 and AlCl3 are added to dichloromethane, and the dichloromethane solution of raw material 2 is slowly added dropwise. The feeding is carried out at -20 to 10 °C, and the reaction is carried out at room temperature. After the reaction is complete, intermediate 1 is obtained through post-treatment;
[0026] The second step: Intermediate 1, hydroxylamine hydrochloride, and sodium acetate are added to tetrahydrofuran, and the reaction is carried out for 6-12 h. After the reaction is complete, intermediate 2 is obtained through post-treatment;
[0027] The third step: Intermediate 2 and raw material 3 are added to dichloromethane, and triethylamine is slowly added dropwise at 0 °C. The reaction is carried out at room temperature for 4-6 h. After the reaction is complete, intermediate 3 is obtained through post-treatment;
[0028] The fourth step: Intermediate 3 and raw material 4 are dissolved in DMF (N,N-dimethylformamide), then triethylamine is added to maintain an alkaline environment, and the reaction is carried out in an oil bath at 80 °C with stirring for 10-12 h. After the reaction is complete, the stabilizer is obtained through post-treatment.
[0029] Furthermore, the matrix material is composed of polymer resin and activated carbon in a mass ratio of 3:1; the crosslinking agent is polyethyleneimine; the pore-forming agent is sodium bicarbonate or sodium bicarbonate;
[0030] The polymer resin is selected from any one of polyacrylamine and polystyrene.
[0031] A preparation method of a porous adsorbent material for water environment purification treatment, comprising the following steps:
[0032] S1. Mix the matrix material and the crosslinking agent in proportion, stir and react in a water bath for 1-2 hours to form a prepolymer; add a pore-forming agent and a stabilizer to the prepolymer, and disperse at a speed of 100-200 rpm to form a uniform slurry;
[0033] S2. Sequentially add nano-silica and carboxyl-functionalized graphene to the slurry prepared in S1, perform ultrasonic treatment for 30-60 minutes, then inject into a mold, and cure and form at 60-80 °C to form a cured product;
[0034] S3. Soak the cured product in deionized water for 12-24 hours to dissolve out the pore-forming agent to form a porous material, and vacuum-dry the obtained porous material at 50-70 °C to constant weight to obtain a porous adsorbent material for water environment purification treatment.
[0035] Further, the temperature of the water bath is hot water at 70-80 °C.
[0036] An application of a porous adsorbent material for water environment purification treatment, which is applied to the adsorption of metal ions or organic pollutants in water, and the metal ions include at least one of lead, cadmium, chromium, and calcium.
[0037] Further, the organic pollutant is PFAS (perfluoro- and polyfluoroalkyl substances).
[0038] Further, the stabilizer shown in Formula 1 can offset the damage of oxidizing substances in water to the matrix. The steric configuration of the R1-R3 groups in its structure produces a significant steric hindrance effect. During the curing process, large-volume aryl groups (such as naphthyl and biphenyl) inhibit the excessive aggregation of polymer chains through physical blocking. The C-D bond energy of the deuterated alkyl group is 5-10% higher than that of the C-H bond, which can reduce the radical chain breakage during high-temperature curing. The conjugated π-electron system of the heteroaryl group can capture free radicals, improving the oxidation resistance of the material. The D atom of the deuterated aryl group reduces the C-D bond vibration frequency through the isotope effect, increasing the thermal decomposition temperature of the material in an 80 °C water bath. The lone pair electrons of the alkoxy group can form a coordination bond with the surface hydroxyl group of nano-silica, increasing the filler dispersion, and the hydrophobic effect of the deuterated methoxy group can reduce the water absorption rate of the material.
[0039] The amide group of polyacrylamide forms a hydrogen bond network with the aromatic ring of the stabilizer, reducing the anti-swelling coefficient of the material. The hydrophobic interaction of the deuterated phenyl group and the micropores of activated carbon produce synergistic adsorption. The -COOH of the carboxyl-functionalized graphene forms an ester bond with the alkoxy group of the stabilizer, improving the compressive strength of the material. The D...O hydrogen bond between the silanol group on the surface of nano-SiO2 and the deuterated alkoxy group enhances the thermal stability. The carboxyl-functionalized graphene can adsorb biological macromolecules such as proteins in water. The aromatic ring of the stabilizer and the CO2 bubbles generated by the decomposition of sodium bicarbonate produce π-cation interaction. The low surface energy of the deuterated group makes the pore wall form a superhydrophobic surface. The chelation of heavy metals, the aromatic or heteroaromatic ring structure in the stabilizer and Ca 2+ 、Pb 2+ 、Cr 6+ and other metal ions form ligands. Through four mechanisms including steric hindrance, chemical bonding, interface regulation, and sacrificial protection of the matrix, this stabilizer makes the material superior to traditional stable systems.
[0040] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0041] The porous adsorption material for water environment purification treatment of the present invention significantly improves the adsorption capacity and selectivity through unique formulation design. The aromatic or heteroaromatic ring structure in the stabilizer can form ligands with metal ions (such as lead, chromium, calcium, etc.), thereby enhancing the adsorption ability of metal ions. At the same time, it shows excellent removal effects on organic pollutants, especially perfluoro and polyfluoroalkyl substances (PFAS).
[0042] The designed stabilizer structure endows the material with good stability. The bond energy of the C-D bond in the deuterated alkyl group in the stabilizer is 5-10% higher than that of the C-H bond, which can reduce the radical chain breakage during high-temperature curing; the conjugated π-electron system of the heteroaryl group can capture free radicals, further improving the oxidation resistance of the material; and the large-volume aryl group inhibits the excessive aggregation of polymer chains through physical blocking during the curing process. These characteristics make the material not easily degraded in a complex water environment, ensuring long-term purification effects.
[0043] The preparation process provided by the present invention is simple to operate and highly controllable, and is easy to realize large-scale production. At the same time, the material has the characteristics of recyclability, which not only reduces the use cost but also reduces resource waste, and has important economic and environmental significance for water purification treatment in practical applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 It is the synthesis route of the stabilizer in a porous adsorption material for water environment purification treatment of the present invention.
[0045] Figure 2 It is the removal rate of calcium ions in the examples and comparative examples of the present invention. Detailed implementation mode
[0046] The technical solution of the present invention will be clearly and completely described below in conjunction with the accompanying drawings in the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without creative work conditions belong to the scope of protection of the present invention.
[0047] Synthesis Example 1
[0048]
[0049] First step: 20 g of raw material 1 and 19.20 g of AlCl3 are added to 200 g of dichloromethane. After the temperature is lowered to -20 °C, a solution of 6.78 g of raw material 2 dissolved in 100 mL of dichloromethane is slowly added dropwise. During the dropping process, the temperature does not exceed 10 °C. After the dropping is completed, the reaction is carried out at room temperature for 12 h. The reaction solution is slowly poured into 500 mL of 0.1 mol / L HCl at 0 °C, stirred for 30 min and then left to stand for liquid separation, and the organic phase is retained. The aqueous phase is washed with 50 mL of dichloromethane 2 - 3 times, the organic phases are combined, 100 mL of 0.1 mol / L sodium bicarbonate solution is added, stirred and shaken until the pH is adjusted to neutral, and the organic phase is retained. It is dried with 20 g of anhydrous magnesium sulfate, filtered, rotary evaporated, and dried to obtain 17.82 g of intermediate 1;
[0050] Second step: 17.82 g of intermediate 1, 5.81 g of hydroxylamine hydrochloride, and 6.86 g of sodium acetate are added to 200 g of tetrahydrofuran. After reacting for 12 hours and the reaction is complete, the reaction solution is added to 1000 mL of water and left overnight at 0 °C, and then filtered by suction to obtain a powdery solid. The powdery solid is dissolved in 100 mL of ethyl acetate, 20 g of anhydrous magnesium sulfate is added for drying, filtered and then rotary evaporated, and then dried to finally obtain 15.61 g of intermediate 2;
[0051] Third step: Under a light-shielded reaction system, 15.61 g of intermediate 2 and 4.39 g of raw material 3 are added to 160 g of dichloromethane. 9.44 g of triethylamine is slowly added dropwise at 0 °C, and the reaction is carried out at room temperature for 6 h. After the reaction is complete, 500 mL of water at 0 °C is slowly added dropwise, stirred for 1 h, left to stand for layer separation, and the organic phase is retained. Then, the pH of the organic phase is adjusted to neutral with 0.1 mol / L dilute hydrochloric acid, washed with water once, and the organic phase is retained again. 30 g of anhydrous magnesium sulfate is added to the organic phase for drying, filtered, and the solvent is rotary evaporated to obtain a viscous liquid with a purity greater than 93%. The viscous liquid is dissolved in 100 mL of ethanol, and then under high-speed stirring, the ethanol solution is added dropwise to a large amount of water, and a white solid product can be precipitated. After filtration and drying, 13.09 g of intermediate 3 is obtained;
[0052] Step 4: Under a light-shielding reaction system, dissolve 13.09 g of intermediate 3 and 10.64 g of raw material 4 in 150 g of DMF, and then slowly add dropwise 8.79 g of triethylamine to maintain an alkaline environment. Under stirring conditions, react in an 80 °C oil bath for 12 h. After the reaction is complete, add 100 mL of deionized water, extract with DMF repeatedly for 3 times, combine the organic phases, and dry the organic phases with anhydrous magnesium sulfate. Then rotary evaporate to remove DMF, and then load the sample by dry method, use petroleum ether / ethyl acetate as the eluent, and carry out silica gel column chromatography purification. Finally, rotary dry to obtain 13.84 g of stabilizer 1. The MS [MS+H + : 615. 1 H NMR (deuterochloroform) δ 8.90 - 8.84 (m, 1H), 8.61 (p, 1H), 8.32 - 8.27 (m, 2H), 8.03 (dd, 1H), 7.82 - 7.76 (m, 1H), 7.74 - 7.68 (m, 1H), 7.63 (dd, 1H), 7.46 - 7.31 (m, 9H), 7.28 - 7.19 (m, 1H), 6.65 (p, 1H), 6.58 (s, 2H), 2.45 (s, 3H), 2.20 (s, 3H), 2.11 (t, 3H).
[0053] Synthesis Examples 2 - 12
[0054] For the stabilizers synthesized in Synthesis Examples 2 - 12, refer to the synthesis steps of Synthesis Example 1, only replace raw materials 1, 2, and 3 therein, and keep the remaining steps such as post-treatment and feed equivalent ratio unchanged. The structures of raw material 1, raw material 2, raw material 3, the stabilizer structure, and the MS [MS+H + data are shown in the following table.
[0055]
[0056]
[0057]
[0058] Example 1
[0059] A preparation method of a porous adsorbent material for water environment purification treatment, comprising the following steps:
[0060] S1. Mix 50 parts of the matrix material (a mixture of polyacrylamide and activated carbon in a mass ratio of 3:1) with 8 parts of the cross-linking agent (polyethyleneimine), and stir and react in a water bath at 80 °C for 2 hours to form a prepolymer; add 12 parts of the pore-forming agent (sodium bicarbonate) and 5 parts of the stabilizer (Synthesis Example 1) to the prepolymer, and disperse at a speed of 150 rpm to form a uniform slurry;
[0061] S2. Sequentially add 10 parts of nano-silica and 5 parts of carboxyl-functionalized graphene (purchased from Scientific Materials Station http: / / www.scimaterials.cn / Default.aspx, AMG008 CarboxylGraphene) to the slurry prepared in S1, ultrasonically treat for 30 minutes, and cure and mold at 80 °C to form a cured product;
[0062] S3. Immerse the cured product in deionized water for 24 hours, dissolve out the pore-forming agent to form a porous material, and vacuum dry the obtained porous material at 70 °C to constant weight to obtain a porous adsorbent material for water environment purification treatment.
[0063] Examples 2 - 12
[0064] In Examples 2 - 12, a porous adsorbent material for water environment purification treatment was prepared, and the stabilizer therein was sequentially replaced with the stabilizers prepared in Synthesis Examples 2 - 12, and the rest remained unchanged.
[0065] Comparative Example 1
[0066] A water environment purification material was prepared with reference to the preparation method of Example 1 without adding the stabilizer therein, and the rest remained unchanged.
[0067] Comparative Example 2
[0068] A water environment purification material was prepared with reference to the preparation method of Example 1, and the matrix material therein was replaced with polyacrylamide, and the rest remained unchanged.
[0069] Comparative Example 3
[0070] A water environment purification material was prepared with reference to the preparation method of Example 1, and the stabilizer therein was replaced with Comparative Stabilizer 1, and the rest remained unchanged.
[0071] The structure of Comparative Stabilizer 1 is:
[0072] Performance test:
[0073] 1. Determination of calcium ion removal rate (%):
[0074] Test method: The materials prepared in Examples 1 - 12 and Comparative Examples 1 - 3 (cut into a diameter of 150 mm and a thickness of 1 mm) were closely attached inside a Buchner funnel (inner diameter of 150 mm and height of 210 mm). A 100 mL sludge mixture (sewage from a municipal sewage treatment plant and calcium peroxide mixed evenly at a mass ratio of 1:0.001) was taken to detect the copper ion concentration P0 by ICP - MS. Filtration was carried out under a pressure of 0.04 Mpa, allowing the liquid to drain from the bottom of the funnel through the filter material for sewage treatment, and then the copper ion concentration P1 was measured again. The data of the calcium ion removal rate (%) of the materials prepared in Examples 1 - 12 and Comparative Examples 1 - 3 are shown in Table 1 and Figure 2 。
[0075] The calculation formula for the removal rate is:
[0076] Table 1 Calcium ion removal rate (%) of the materials prepared in Examples 1 - 12 and Comparative Examples 1 - 3.
[0077]
[0078]
[0079] The data in Table 1 show that the water environment purification materials of the present invention have relatively high calcium ion removal rates under different formulations. The removal rates of Examples 1 - 12 are all above 97.45%, and among them, the removal rate of Example 5 is the highest, reaching 99.68%. The removal rates of Comparative Examples 1 - 3 are significantly lower than those of the examples, indicating that the stabilizer added in the present invention and the matrix material composed of the combination of polystyrene and activated carbon play an important role in improving the calcium ion removal rate, and the stabilizer structure designed in the present invention is superior to the comparative stabilizer. Overall, the materials of the present invention have good calcium ion adsorption and / or interception performance and application potential.
[0080] Although the embodiments of the present invention have been shown and described, for those of ordinary skill in the art, it can be understood that various changes, modifications, substitutions, and variations can be made to these embodiments without departing from the principles and spirit of the present invention. The scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A porous adsorbent material for water environment purification, characterized in that: The invention comprises the following components in parts by weight: 30-50 parts of base material, 5-15 parts of cross-linking agent, 10-25 parts of porogen, 1-5 parts of stabilizer, 10-15 parts of nano-silicon dioxide, and 5-8 parts of carboxyl functionalized graphene; Further, the stabilizer has a structure shown in Formula 1; In Formula 1, R1-R2 are the same or different and are selected from: C1-C5 alkyl, C1-C5 alkoxy, C4-C 10 Heteroaryl, C6-C 15 The aromatic group; or R1 and R2 are the same or different and are independently selected from: C4-C5 alkyl, C1-C5 alkoxy, C1-C5 deuterated alkyl, C1-C5 deuterated alkoxy substituted 10 Heteroaryl, C6-C 15 The aromatic group; or R1 and R2 are the same or different and are independently selected from: C1-C5 deuterated alkyl, C1-C5 deuterated alkoxy, C4-C 10 Deuterated heteroaryl, C6-C 15 deuterated aryl; In formula 1, R3 is selected from: C1-C5 alkyl, C6-C 15 Aryl, C1-C5 deuterated alkyl, C6-C 15 deuterated aryl; or R3 is selected from: C6-C5 alkyl, C1-C5 deuterated alkyl, C1-C5 alkoxy substituted C6-C5 15 The aromatic and C6-C 15 Deuterated aryl.
2. The porous adsorbent material for water environment purification according to claim 1, characterized in that: The C1-C5 alkyl group is selected from the group consisting of methyl, ethyl, propyl and tert-butyl; the C1-C5 deuterated alkyl group is selected from the group consisting of deuterated methyl, deuterated ethyl, deuterated propyl and deuterated tert-butyl.
3. The porous adsorbent material for water environment purification according to claim 1, characterized in that: The C1-C5 alkoxy group is selected from: methoxy group and ethoxy group; the C1-C5 deuterated alkoxy group is selected from: deuterated methoxy group and deuterated ethoxy group.
4. The porous adsorbent material for water environment purification according to claim 1, characterized in that: The C4-C 10 The heteroaryl group is selected from the group consisting of furanyl, thienyl; C6-C 15 The aryl group is selected from: phenyl, naphthyl, biphenyl; C4-C 10 The deuterated heteroaryl is selected from: deuterated furanyl, deuterated thienyl; C6-C 15 The deuterated aryl group is selected from the group consisting of deuterated phenyl, deuterated naphthyl and deuterated biphenyl.
5. The porous adsorbent material for water environment purification according to claim 1, characterized in that: The stabilizer is selected from any one of the compounds shown in the following structures: Wherein D represents deuterium.
6. The porous adsorbent material for water environment purification according to claim 1, characterized in that: The matrix material is: a polymer resin and activated carbon in a mass ratio of 3:1; the cross-linking agent is polyethyleneimine; the porogen is sodium bicarbonate or sodium bicarbonate; The polymer resin is selected from any one of polyacrylamine and polystyrene.
7. A method for preparing a porous adsorbent material for water environment purification according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1. The base material and the crosslinking agent are mixed in proportion, stirred in a water bath for 1-2 hours to form a prepolymer; a porogen and a stabilizer are added to the prepolymer, and dispersed at a speed of 100-200 rpm to form a uniform slurry; S2. Add nano-silica and carboxyl-functionalized graphene to the slurry prepared in S1, perform ultrasonic treatment for 30-60 minutes, inject into a mold, and cure at 60-80° C. to form a cured product; S3. Soak the solidified product in deionized water for 12-24 hours to dissolve the porogen to form a porous material, and vacuum dry the obtained porous material at 50-70° C. to constant weight to obtain a porous adsorption material for water environment purification.
8. The preparation method according to claim 7, characterized in that: The temperature of the water bath is 70-80°C.
9. The use of the porous adsorbent material for water environment purification according to any one of claims 1 to 6, characterized in that: It is used for adsorption of metal ions or organic pollutants in water, wherein the metal ions include at least one of lead, cadmium, chromium and calcium.
10. The use according to claim 9, characterized in that The organic pollutants are fluorine and polyfluoroalkyl substances.
Citation Information
Patent Citations
Porous spherical crosslinking resin-graphene oxide compound adsorbing material and preparation and application thereof
CN106799215A
Nano-composite material for adsorbing calcium and magnesium ions in water
CN108043366A
Hydroxyl graphene-nano silicon dioxide modified chitosan composite material and application thereof
CN111659354A
Porous graphene adsorption material as well as preparation method and application thereof
CN116688945A
Preparation method of porous polymer and application of porous polymer in treatment of high-salt high-ammonia-nitrogen wastewater and metal wastewater
CN118440300A
Cited By
Stain-resistant and corrosion-resistant coating for stainless steel surface and preparation method of stain-resistant and corrosion-resistant coating
CN121673872A
A stain-resistant and corrosion-resistant coating for stainless steel surfaces and a method for preparing the same
CN121673872B