Preparation method of organic expanded vermiculite / full-biodegradable composite material

The micro-wave expansion and organic modification of vermiculite with silane coupling agents addresses the challenges of mechanical loss and poor dispersion in biodegradable materials, resulting in improved mechanical strength and compatibility with polymers, suitable for various applications.

CN120310220APending Publication Date: 2025-07-15安徽金普瑞新材料有限公司

Patent Information

Application Number
CN202510571684.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-06
Publication Date
2025-07-15

AI Technical Summary

Technical Problem

In the prior art, when peeling off and organically treating vermiculite, there are problems such as serious mechanical strength loss, severe powdering and poor compatibility with polymer materials, which leads to limited application in all biodegradable materials.

Method used

Vermiculite is treated by microwave method, hydrogen peroxide reacts with vermiculite to generate gas to expand, and hydrolyze and diffuse it in microwave through maleic anhydride or silane coupling agent to the sheet layer, and organically expanded vermiculite/full biodegradable composite material is prepared in combination with the twin-screw extrusion mechanism.

Benefits of technology

It improves the mechanical strength and flexibility of the vermiculite sheet layer, enhances compatibility with polylactic acid, and the prepared composite material has excellent rigid and tough balance performance, and is suitable for a variety of disposable products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120310220A_ABST
    Figure CN120310220A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of an organic expanded vermiculite / full-biodegradable composite material, and belongs to the field of environment-friendly biodegradable materials. The composite material comprises the following raw materials in parts by weight: 5-30 parts of organic expanded vermiculite, 5-60 parts of polylactic acid, a degradable toughening agent and an auxiliary agent, and the vermiculite raw material in the organic expanded vermiculite is soaked in maleic anhydride or a silane coupling agent and is subjected to microwave expansion treatment. Compared with the prior art, degradation residues of the prepared composite material are mainly expanded vermiculite powder, and the composite material is environmentally friendly and free of pollution, has the effect of improving soil and can be applied to the fields of disposable knives, forks, spoons, straws, film bags and the like through formula adjustment of polylactic acid and the full-biodegradable flexibilizer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of environmentally friendly biodegradable materials, and particularly to a preparation method of an organic expanded vermiculite / fully biodegradable composite material. Background Art

[0002] Due to the serious "white pollution" caused by traditional plastic products to the environment, with the rising call for environmental protection and the enhancement of environmental awareness, fully biodegradable materials have become the future trend in replacing traditional plastics, especially in the field of disposable products that are difficult to recycle. Fully biodegradable materials have good degradability, can be naturally decomposed by organisms, and are ultimately converted into water, carbon dioxide, methane and gas, which can effectively alleviate environmental pollution problems. Polylactic acid is one of the most commonly used fully biodegradable materials. It is derived from the fermentation of biomass raw materials and has advantages such as biocompatibility, environmental friendliness, high rigidity and high strength. However, its impact strength is low and its toughness is poor. It often needs to be blended with other fully biodegradable elastomers such as polybutylene succinate, polybutylene succinate - adipate, copolymers of terephthalic acid (or its dimethyl ester) with 1,4 - butanediol and adipic acid, and polycaprolactone, etc. to improve the toughness of the polylactic acid material and expand its application range.

[0003] Vermiculite is an environmentally friendly layered aluminosilicate mineral material. Vermiculite has excellent ion exchangeability, adsorption and thermal expansion properties, and has application value in the fields of soil conditioner, pollutant adsorption, sound absorption, heat insulation and heat preservation, etc. However, natural vermiculite has a closely stacked layered structure, with less surface charge between layers, a small interlayer spacing, and a low specific surface area, which limits its application effect. Peeling natural vermiculite to obtain vermiculite flakes with nano - thickness can expose a large number of interlayer reaction sites and increase the internal specific surface area, and its reaction activity, adsorption, heat insulation, air permeability and moisture retention properties are also greatly improved. Currently, the commonly used methods for peeling vermiculite include thermal expansion method, physical method, chemical method and physical - chemical combined method. Among them, the thermal expansion method is the most mature in industrialization. However, the vermiculite flakes obtained by the thermal expansion method after high - temperature ablation have large mechanical strength loss, serious pulverization, and poor compatibility with polymers, and secondary surface treatment is still required to be applied to the modification of polymer materials.

[0004] In view of the above - mentioned technical problems, the current main improvement methods mainly include expanded vermiculite after thermal expansion or microwave expansion, introducing silane coupling agents, polycarboxylic acids, polyols or ion exchangers for surface treatment to introduce organophilic groups, so as to improve the compatibility with polymer materials. However, these technical solutions still have problems such as agglomeration, loss of aspect ratio and performance after multiple treatments.

[0005] For example, in Chinese Patent CN102350301A, by dispersing thermally expanded vermiculite into an aqueous solution, adding an amphoteric ionic surfactant, and filtering, organically modified expanded vermiculite is obtained, but the mechanical strength of the thermally expanded vermiculite is lost and pulverization is severe; in Chinese Patent CN107098355A, vermiculite and a dispersion liquid are fed into a stirring motor, and the vermiculite is exfoliated by a stirring paddle, without organically treating the expanded vermiculite; in Chinese Patent CN102167530A, vermiculite is thermally expanded under the condition of 150-1000°C, the preliminarily cooled expanded vermiculite is fed into a continuous mixer, and an organic modifier is sprayed thereon, and the surface of the expanded vermiculite is modified by the waste heat of the thermally expanded vermiculite; in Chinese Patent CN101172802A, the sieved vermiculite is put into a microwave oven and processed at 10-1000W for 30-120s for puffing treatment. Relying on the natural crystal water between the vermiculite flakes to be vaporized by heat and expand, there are defects such as low expansion ratio and incomplete exfoliation of the flakes; in Chinese Patent CN102167531A, vermiculite is soaked in 5-30% hydrogen peroxide solution for 1-14h, and then ultrasonically pretreated for 10-60min to promote the entry of hydrogen peroxide molecules between the vermiculite flakes. Finally, the pretreated vermiculite is taken out and put into a microwave device for processing to obtain expanded vermiculite, without organically treating the expanded vermiculite. Summary of the Invention

[0006] Aiming at the deficiencies of the prior art, the present invention provides a preparation method of an organically modified expanded vermiculite / fully biodegradable composite material.

[0007] The object of the present invention can be achieved by the following technical solutions:

[0008] In a first aspect of the present invention, it relates to an organically modified expanded vermiculite / biodegradable composite material, comprising the following raw materials in parts by weight:

[0009] 5-30 parts of organically modified expanded vermiculite, 5-60 parts of polylactic acid, a degradable toughening agent and an additive. The vermiculite raw material in the organically modified expanded vermiculite is soaked in maleic anhydride or a silane coupling agent and is subjected to microwave expansion treatment.

[0010] Optionally, the preparation method of the organically modified expanded vermiculite comprises the following steps:

[0011] Dissolve a silane coupling agent or maleic anhydride in a hydrogen peroxide solution. The container is a ceramic or glass crucible, and vermiculite is added for soaking;

[0012] Put the hydrogen peroxide solution and vermiculite into a microwave oven to expand and organically modify the vermiculite;

[0013] After drying, crushing and sieving in sequence, organically modified expanded vermiculite powder is obtained.

[0014] Optionally, the microwave oven has a frequency of 2.45 GHz, a power of 800 W, and the microwave treatment lasts for 5 to 10 minutes.

[0015] Optionally, the polylactic acid is at least one of left-handed or right-handed polylactic acid, and the weight-average molecular weight is 10 - 18 wg / mol.

[0016] Optionally, the biodegradable toughening agent is at least one of polybutylene succinate (PBS), poly(butylene succinate-co-adipate) (PBSA), and copolymers of terephthalic acid (or its dimethyl ester) with 1,4-butanediol and adipic acid (PBAT).

[0017] Optionally, it further includes one or more of anti-aging agents, cross-linking agents, and lubricants.

[0018] Optionally, the dosage of the maleic anhydride and the silane coupling agent is 1% - 5% of the weight of the vermiculite.

[0019] In the second aspect of the present invention, a method for preparing an organically expanded vermiculite / fully biodegradable composite material is provided, which includes the following steps: mixing 5 - 60 parts by weight of polylactic acid, 10 - 90 parts by weight of biodegradable toughening agent, and 5 - 30 parts by weight of organically expanded vermiculite powder to obtain a mixture, and putting the mixture into a twin-screw extruder to obtain a fully biodegradable composite material through melting, extrusion, strand drawing, water cooling, pelletizing, and drying; wherein, the vermiculite raw material in the organically expanded vermiculite is soaked in maleic anhydride or silane coupling agent and undergoes microwave expansion treatment.

[0020] Optionally, the ratio of the length to the diameter of the twin-screw extruder is 36:1 - 48:1, and the screw temperature is 175 - 200 °C.

[0021] In the third aspect of the present invention, the above-mentioned organically expanded vermiculite / fully biodegradable composite material is used in the preparation of disposable tableware or packaging.

[0022] The beneficial effects of the present invention:

[0023] 1. The present invention provides a method for preparing organically expanded vermiculite in one step by microwave method. Exchange occurs between hydrogen peroxide and water molecules in vermiculite, and gas is generated under the catalytic action of Fe 2+ / Fe 3+ ions in the microwave and vermiculite, causing the vermiculite lamellae to expand and peel rapidly. Compared with the high-temperature thermal expansion method, the mechanical strength and flexibility loss of the vermiculite lamellae are smaller; secondly, at the same time, maleic anhydride or silane coupling agent hydrolyzes in the hydrogen peroxide solution, diffuses fully between the lamellae, condenses with the hydroxyl groups on the vermiculite surface, and retains the other end with a group affinity for the resin; thirdly, introducing the coupling agent molecular chain between the vermiculite lamellae can prevent agglomeration caused by electrostatic adsorption between the lamellae and increase its dispersion performance.

[0024] 2. The organically expanded vermiculite powder prepared by the present invention can be used as a reinforcing, rigidifying and nucleating agent for fully biodegradable materials. The expanded vermiculite powder has a nanoscale lamellar structure, which can play a role in supporting and increasing the rigidity of the material. The resin can diffuse between the lamellae to form more nucleation sites and improve the crystallization rate.

[0025] 3. The organically expanded vermiculite / fully biodegradable material prepared by the present invention has excellent rigid-flexible balance performance and can be applied to a variety of disposable products. The main residue after degradation, the expanded vermiculite powder, has a fluffy and porous structure and has the function of improving soil structure, with advantages such as low carbon, environmental protection and environmental friendliness. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] The present invention will be further described below with reference to the accompanying drawings.

[0027] Figure 1 Shows the structural formula of organically expanded vermiculite;

[0028] Figure 2 Shows the synthesis route of organically expanded vermiculite. DETAILED DESCRIPTION OF THE EMBODIMENTS

[0029] The technical solutions in the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings in the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments. All other embodiments obtained by those of ordinary skill in the art based on the embodiments of the present invention without creative efforts shall fall within the protection scope of the present invention.

[0030] An organically expanded vermiculite / fully biodegradable composite material is synthesized from organically expanded vermiculite, polylactic acid, a fully biodegradable toughening agent and an auxiliary agent; wherein, the structural formula of the organically expanded vermiculite is as Figure 1 shown;

[0031] The following will be specifically described through the following embodiments. It is worth mentioning that in the preparation processes in the following embodiments, unless otherwise specified, they are all conventional means in the prior art, so they will not be described in detail; the parts in the following embodiments all refer to mass parts;

[0032] The preparation methods of the organically expanded vermiculite powder in the following embodiments are as follows:

[0033] Dissolve 50 g of KH560 in 30% hydrogen peroxide solution, put it into a ceramic crucible, add 1 kg of vermiculite cleaned and decontaminated, soak for 10 min, then put the vermiculite dispersion liquid and the crucible into a microwave oven. The microwave oven frequency is 2.45 GHz and the power is 800 W. Microwave treatment is carried out for 10 min. After filtration, drying, crushing and sieving, organically expanded vermiculite powder A is obtained.

[0034] Dissolve 10 g of maleic anhydride in 30% hydrogen peroxide solution, place it in a ceramic crucible, add 1 kg of vermiculite that has been cleaned and decontaminated, soak for 10 min, then put the vermiculite dispersion and the crucible into a microwave oven. The microwave oven frequency is 2.45 GHz and the power is 800 W. Microwave treat for 5 min, and obtain organically expanded vermiculite powder B after filtration, drying, crushing, and sieving.

[0035] Example 1

[0036] Mix 30 parts of organically expanded vermiculite powder A with a particle size of 30 μm, 60 parts of PLA, 10 parts of biodegradable toughening agent PBAT, 0.1 part of antioxidant 1010, 0.2 part of antioxidant 168, 0.3 part of carbodiimide, 0.5 part of EBS, 0.5 part of erucic acid amide, and 0.4 part of crosslinking agent ADR-4468 evenly. Put the mixture into a twin-screw extruder, and obtain a fully biodegradable composite material after melting, extrusion, strand drawing, water cooling, pelletizing, and drying. The above twin-screw extruder has a length-diameter ratio of 36:1, and the screw temperature is 175 - 200 °C.

[0037] Example 2

[0038] Mix 20 parts of organically expanded vermiculite powder A with a particle size of 5 μm, 55 parts of PLA, 15 parts of biodegradable toughening agent PBS, 10 parts of biodegradable toughening agent PBAT, 0.2 part of crosslinking agent ADR-4468, and 0.3 part of EBS evenly. Put the mixture into a twin-screw extruder, and obtain a fully biodegradable composite material after melting, extrusion, strand drawing, water cooling, pelletizing, and drying. The above twin-screw extruder has a length-diameter ratio of 40:1, and the screw temperature is 175 - 200 °C.

[0039] Example 3

[0040] Mix 30 parts of organically expanded vermiculite powder B with a particle size of 10 μm, 5 parts of PLA, 65 parts of biodegradable toughening agent PBAT, 0.2 part of crosslinking agent ADR-4468, 0.1 part of antioxidant 1010, and 0.5 part of EBS evenly. Put the mixture into a twin-screw extruder, and obtain a fully biodegradable composite material after melting, extrusion, strand drawing, water cooling, pelletizing, and drying. The above twin-screw extruder has a length-diameter ratio of 48:1, and the screw temperature is 155 - 175 °C.

[0041] Example 4

[0042] Mix 5 parts of organically modified expanded vermiculite powder B with a particle size of 5 μm, 5 parts of PLA, 90 parts of biodegradable toughening agent PBAT, 0.1 part of crosslinking agent ADR-4468, 0.2 part of antioxidant 1010, and 0.2 part of EBS evenly. Put the mixture into a twin-screw extruder, and obtain a fully biodegradable composite material through melting, extrusion, strand pulling, water cooling, pelletizing, and drying. The aspect ratio of the above twin-screw extruder is 48:1, and the screw temperature is 155 - 170 °C.

[0043] Comparative Example 1

[0044] Add 1 kg of vermiculite cleaned and decontaminated to a ceramic crucible containing 30% hydrogen peroxide solution, soak for 10 min, then put the vermiculite dispersion liquid and the crucible into a microwave oven together. The microwave oven frequency is 2.45 GHz, the power is 800 W, and microwave treatment is carried out for 10 min. After filtration, drying, crushing, and sieving, microwave-expanded vermiculite powder is obtained.

[0045] Mix 30 parts of microwave-expanded vermiculite powder with a particle size of 30 μm, 60 parts of PLA, 10 parts of biodegradable toughening agent PBAT, 0.1 part of antioxidant 1010, 0.2 part of antioxidant 168, 0.3 part of carbodiimide, 0.5 part of EBS, 0.5 part of erucic acid amide, and 0.4 part of crosslinking agent ADR-4468 evenly. Put the mixture into a twin-screw extruder, and obtain a fully biodegradable composite material through melting, extrusion, strand pulling, water cooling, pelletizing, and drying. The aspect ratio of the above twin-screw extruder is 36:1, and the screw temperature is 175 - 200 °C.

[0046] Comparative Example 2

[0047] Put 1 kg of vermiculite cleaned and decontaminated into a ceramic crucible, heat-treat it in a muffle furnace at 900 °C for 10 min, and obtain thermally expanded vermiculite powder after cooling, crushing, and sieving. Add 50 g of coupling agent KH560 to 1 kg of thermally expanded vermiculite powder and mix evenly to obtain organically modified thermally expanded vermiculite powder.

[0048] Mix 20 parts of organically modified thermally expanded vermiculite powder with a particle size of 5 μm, 55 parts of PLA, 15 parts of biodegradable toughening agent PBS, 10 parts of biodegradable toughening agent PBAT, 0.2 part of crosslinking agent ADR-4468, and 0.3 part of EBS evenly. Put the mixture into a twin-screw extruder, and obtain a fully biodegradable composite material through melting, extrusion, strand pulling, water cooling, pelletizing, and drying. The aspect ratio of the above twin-screw extruder is 40:1, and the screw temperature is 175 - 200 °C.

[0049] Comparative Example 3

[0050] Add 50 g of coupling agent KH560 to 1 kg of talc powder with a particle size of 5 μm and mix evenly to obtain organically modified talc powder.

[0051] Mix 20 parts of organic talcum powder, 55 parts of PLA, 15 parts of biodegradable toughening agent PBS, 10 parts of biodegradable toughening agent PBAT, 0.2 parts of crosslinking agent ADR-4468, and 0.3 parts of EBS evenly. Put the mixture into a twin-screw extruder, and obtain a fully biodegradable composite material through melting, extrusion, strand drawing, water cooling, pelletizing, and drying. The above-mentioned twin-screw extruder has a length-diameter ratio of 40:1, and the screw temperature is 175-200°C.

[0052] Comparative Example 4

[0053] Add 1 kg of vermiculite cleaned and decontaminated to a ceramic crucible containing 30% hydrogen peroxide solution, soak for 10 minutes, then put the vermiculite dispersion liquid and the crucible together into a microwave oven. The microwave oven has a frequency of 2.45 GHz and a power of 800 W, and perform microwave treatment for 10 minutes. After filtration, drying, crushing, and sieving, obtain microwave-expanded vermiculite powder. Add 10 g of maleic anhydride to 1 kg of microwave-expanded vermiculite powder and mix evenly to obtain organic microwave-expanded vermiculite powder.

[0054] Mix 30 parts of organic microwave-expanded vermiculite powder with a particle size of 10 μm, 5 parts of PLA, 65 parts of biodegradable toughening agent PBAT, 0.2 parts of crosslinking agent ADR-4468, 0.1 part of antioxidant 1010, and 0.5 parts of EBS evenly. Put the mixture into a twin-screw extruder, and obtain a fully biodegradable composite material through melting, extrusion, strand drawing, water cooling, pelletizing, and drying. The above-mentioned twin-screw extruder has a length-diameter ratio of 48:1, and the screw temperature is 155-175°C.

[0055] Experimental verification;

[0056] Inject the composite materials obtained in Examples 1-4 and Comparative Examples 1-3 into standard test specimens, and test their tensile strength, elongation at break, flexural strength, flexural modulus, Izod notched impact strength, and heat distortion temperature. Among them, the heat distortion temperature test specimens of Examples 1-2 and Comparative Examples 1-2 are annealed at 90°C for 10 minutes before testing. The test methods for tensile strength and elongation at break are in accordance with GB / T 1040, the test methods for flexural strength and flexural modulus are in accordance with GB / T 9341, the test method for Izod notched impact strength is in accordance with CB / T 1843, and the test method for heat distortion temperature is in accordance with GB / T 1634.

[0057] The comparative test results of Examples 1-4 and Comparative Examples 1-3 are shown in Table 1 below:

[0058] Table 1 Comparative test results of Examples 1-4 and Comparative Examples 1-3

[0059]

[0060] As can be seen from Table 1, by comparing Examples 1-4 with Comparative Examples 1-4, the comprehensive performance of Examples 1-4 is significantly better than that of the comparative examples, specifically manifested as higher strength and heat distortion temperature. Example 1 has higher rigidity and heat resistance than Comparative Example 1, indicating that the performance of vermiculite powder can be significantly improved by carrying out the organic treatment synchronously during the microwave expansion of vermiculite, which is suitable for application in injection molding products, such as crystalline heat-resistant knife, fork, and spoon materials; Example 2 has higher toughness and heat distortion temperature than Comparative Examples 2-3, indicating that the performance retention of the organically modified microwave-expanded vermiculite powder is better than that of the organically modified thermally expanded vermiculite powder and the organically modified talc powder. This is mainly because the mechanical strength of the thermally expanded vermiculite flakes decreases significantly after high-temperature ablation. Compared with the flaky talc powder, the synchronous organic treatment during microwave expansion can make the coupling agent penetrate deeper into the vermiculite flakes, with more uniform coating of the coupling agent and better compatibility with the resin, which is suitable for application in extrusion molding products, such as crystalline heat-resistant straw materials; Examples 3-4 have higher strength compared with Comparative Example 4, indicating that maleic anhydride can penetrate deeper into the vermiculite flakes during microwave expansion, assisting in the peeling of the vermiculite flakes, more complete organic digestion, and preventing the aggregation of vermiculite flakes, which is suitable for application in blown film products, such as milk tea bags, shopping bags, etc.

[0061] In the description of this specification, the descriptions referring to the terms "one embodiment", "example", "specific example", etc. mean that the specific features, structures, materials, or characteristics described in connection with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described can be combined in a suitable manner in any one or more embodiments or examples.

[0062] The above shows and describes the basic principles, main features, and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited by the above embodiments. The above embodiments and the descriptions in the specification only illustrate the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention will have various changes and improvements, and these changes and improvements all fall within the scope of the present invention claimed.

Claims

1. An organic expanded vermiculite / bio - degradable composite material, characterized in that, It includes the following raw materials in parts by weight: 5-30 parts of organically expanded vermiculite, 5-60 parts of polylactic acid, a biodegradable toughening agent and an auxiliary agent, wherein the vermiculite raw material in the organically expanded vermiculite is soaked in maleic anhydride or a silane coupling agent and is subjected to microwave expansion treatment.

2. The organic expanded vermiculite / bio-degradable composite material according to claim 1, characterized in that, The preparation method of the organically expanded vermiculite includes the following steps: Dissolve the silane coupling agent or maleic anhydride in a hydrogen peroxide solution. The container is a ceramic or glass crucible, and add vermiculite for soaking. Put the hydrogen peroxide solution and vermiculite into a microwave oven to expand and organicize the vermiculite. After drying, crushing and sieving in sequence, organically expanded vermiculite powder is obtained.

3. The organic expanded vermiculite / bio-degradable composite material according to claim 2, wherein The microwave oven frequency is 2.45 GHZ, the power is 800 W, and the microwave treatment is carried out for 5-10 min.

4. The organically expanded vermiculite / bio - degradable composite material according to claim 1, wherein The polylactic acid is at least one of left-handed or right-handed polylactic acid, and the weight-average molecular weight is 10-18 wg / mol.

5. The organically expanded vermiculite / bio-degradable composite material according to claim 1, wherein The biodegradable toughening agent is at least one of polybutylene succinate (PBS), polybutylene succinate adipate (PBSA), and a copolymer of terephthalic acid (or its dimethyl ester), 1,4-butanediol and adipic acid (PBAT).

6. The organically expanded vermiculite / bio-degradable composite material according to claim 1, wherein It also includes one or more of an anti-aging agent, a cross-linking agent, and a lubricant.

7. The organically expanded vermiculite / bio - degradable composite material according to claim 1, characterized in that, The dosage of the maleic anhydride and the silane coupling agent is 1%-5% of the weight of the vermiculite.

8. A preparation method of an organic expanded vermiculite / fully biodegradable composite material, characterized in that, It includes the following steps: Mix 5-60 parts by weight of polylactic acid, 10-90 parts by weight of a biodegradable toughening agent, and 5-30 parts by weight of organically expanded vermiculite powder evenly to obtain a mixture, and put the mixture into a twin-screw extruder to obtain a fully biodegradable composite material through melting, extrusion, strand drawing, water cooling, pelletizing and drying; wherein, the vermiculite raw material in the organically expanded vermiculite is soaked in maleic anhydride or a silane coupling agent and is subjected to microwave expansion treatment.

9. The preparation method of an organic expanded vermiculite / fully biodegradable composite material according to claim 8, characterized in that The length-diameter ratio of the twin-screw extruder is 36:1-48:1, and the screw temperature is 175-200 °C.

10. The use of an organically expanded vermiculite / fully biodegradable composite material according to any one of claims 1-7 in the preparation of disposable tableware or packaging.

Citation Information

Patent Citations

  • Method for producing expanded vermiculite with microwave method

    CN101172802A

  • Vermiculite expansion and organic modification integrated preparation process

    CN102167530A

  • Method for preparing expanded vermiculite by utilizing ultrasonic pretreatment way

    CN102167531A

  • Organically modified expanded vermiculite

    CN102350301A

  • Method for rapidly stripping expanded vermiculite

    CN107098355A