Bursting bead bubble cap, preparation method thereof and application of blasting bead bubble cap in self-heating patch

By using antibacterial mesoporous silica blisters in self-heating patches, the temperature controlled release and antibacterial properties of essential oils are achieved, and the problems of single function and high production cost of self-heating patches are solved, which improves the diversified application and safety of the product.

CN120382688APending Publication Date: 2025-07-29GUANGZHOU SANSEN HEALTH IND TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510873887.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-06-27
Publication Date
2025-07-29

AI Technical Summary

Technical Problem

The existing self-heating patch has a single function, which cannot accurately control the release of active ingredients, insufficient antibacterial performance, and high production costs. The structural design needs to be optimized to improve fit and use safety.

Method used

Antibacterial mesoporous silica is used as the shell material of the beads to build a mesoporous structure through a one-step hydrothermal reaction, and the core-shell structure mesoporous silica is used to quickly release essential oil at high temperatures, and combine ethylene glycol dimethacrylate to form a three-dimensional network structure to achieve temperature-controlled release function and antibacterial performance.

Benefits of technology

Quickly release essential oil at the working temperature of the self-heating patch and retain it at room temperature. It has antibacterial properties, simplifies the process and reduces production costs, and improves product performance and service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120382688A_ABST
    Figure CN120382688A_ABST
Patent Text Reader

Abstract

The invention discloses a blasting bead bubble cap, a preparation method thereof and application of the blasting bead bubble cap in a self-heating patch, and relates to the technical field of blasting bead bubble caps, and the blasting bead bubble cap structurally comprises an upper layer fabric, a middle layer core material and a bottom layer fabric; the upper-layer fabric comprises any one of printed leather, printed spunlace, white spunlace, white leather and non-woven fabric; the middle-layer core material is composed of hole digging sponge and blasting beads embedded in holes of the hole digging sponge; the bottom layer fabric is composed of a spraying film and an adhesive layer prepared on the surface of the spraying film through an adhesive dispensing technology. The self-heating patch can be applied to any one of a steam hot-compress eye patch, a hot-compress warm protection patch, a hot-compress neck warming patch, a hot-compress knee warming patch, a hot-compress waist and abdomen patch, a hot-compress ankle patch and a hot-compress wrist patch.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of bursting bead blister, and specifically to a bursting bead blister, its preparation method and application in a self-heating patch. Background Art

[0002] In the field of hot compress physiotherapy, self-heating patches have been widely used due to their convenience and comfort, but there is still room for improvement in their function expansion and use experience. Traditional self-heating patches mainly provide a warm effect through heating materials, with relatively single functions and unable to meet people's needs for diversified physiotherapy, such as precisely controlling the release of active ingredients and enhancing antibacterial properties.

[0003] In the prior art, although the bursting bead technology has been applied in some fields, when combined with self-heating patches, it faces many challenges: on the one hand, how to achieve the rapid release of active ingredients (such as essential oils) at the working temperature of the self-heating patch while maintaining stable retention at room temperature to avoid premature loss of ingredients; on the other hand, the addition of antibacterial agents in traditional processes may affect the loading performance of the carrier material, and the process flow is complex with high production costs.

[0004] In addition, the structural design of self-heating patches needs to be further optimized to improve the fitting degree, comfort and use safety. Therefore, developing a bursting bead blister with temperature-responsive release function, antibacterial property and structural stability is of great significance for expanding the application scenarios of self-heating patches and improving product performance. Summary of the Invention

[0005] The purpose of the present invention is to provide a bursting bead blister, its preparation method and application in a self-heating patch to solve the problems raised in the prior art.

[0006] To achieve the above purpose, the present invention provides the following technical solutions: A bursting bead blister, the structure of the bursting bead blister includes: an upper fabric layer, a middle core layer, and a bottom fabric layer; the middle core layer is composed of a perforated sponge and bursting beads embedded in the holes of the perforated sponge; the bottom fabric layer is composed of a lamination and an adhesive layer prepared by a dotting process on the surface of the lamination.

[0007] Further, the upper fabric layer includes any one of printed leather, printed spunlace fabric, white spunlace fabric, white leather, and non-woven fabric.

[0008] Further, the preparation method of the bursting beads includes the following steps: S1: Add benzalkonium chloride, ammonia water, and deionized water into a reaction vessel, stir evenly, add tetraethyl orthosilicate, stir evenly, heat to 80 - 85 °C and react for 72 h, filter, wash the solid product with deionized water, and vacuum dry at 50 - 55 °C to obtain antibacterial mesoporous silica; S2: Add antibacterial mesoporous silica and 3-aminopropyltriethoxysilane into toluene, stir evenly, under the argon atmosphere, heat to 125 - 130 °C and react for 24 h, centrifuge, wash the product with ethanol, and dry it under vacuum at 50 - 55 °C to obtain amino-functionalized mesoporous silica; S3: Add amino-functionalized mesoporous silica, RAFT reagent, and 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride into dry dichloromethane, stir at room temperature for 24 h under the argon atmosphere, centrifuge, wash the product with ethanol, and dry it under vacuum at 50 - 55 °C to obtain RAFT reagent-modified mesoporous silica; S4: Add RAFT reagent-modified mesoporous silica, 2-(2-methoxyethoxy)ethyl methacrylate, methoxypolyethylene glycol methacrylate, and ethylene glycol dimethacrylate into ethanol, disperse them by ultrasonic, add azobisisobutyronitrile, stir at room temperature for 45 - 60 min under the argon atmosphere, heat to 70 - 75 °C and react for 24 h, centrifuge, wash the product with ethanol to obtain core-shell structured mesoporous silica; S5: Add the core-shell structured mesoporous silica into the essential oil nanoemulsion, stir at room temperature for 12 - 24 h, then heat to 45 - 50 °C and stir for 3 - 4 h to obtain the core material solution; S6: Using ethylene-vinyl acetate copolymer as the wall material of the bursting bead and the core material solution as the core material, solidify the capsules dropped by the dropper head in the coolant, filter and wash to obtain the bursting beads.

[0009] Further, in the preparation process of the antibacterial mesoporous silica, the molar ratio of tetraethyl orthosilicate: benzalkonium chloride: ammonia water is (1 - 1.25):(4 - 6):(0.25 - 0.3).

[0010] Further, in the preparation process of the amino-functionalized mesoporous silica, the mass ratio of antibacterial mesoporous silica: 3-aminopropyltriethoxysilane is (0.1 - 0.2):(0.5 - 1).

[0011] Further, in the preparation process of the RAFT reagent-modified mesoporous silica, add 0.324 - 0.346 mmol of RAFT reagent for every 46 mg of amino-functionalized mesoporous silica; the RAFT reagent is 3-benzylthio thiocarbonylthiopropionic acid.

[0012] Further, in the preparation process of the core-shell structured mesoporous silica, the molar ratio of 2-(2-methoxyethoxy)ethyl methacrylate: methoxypolyethylene glycol methacrylate is (90 - 92):(8 - 10); the addition amount of ethylene glycol dimethacrylate is 4 - 5% of the total molar amount of the monomers.

[0013] Furthermore, the Mn of the 2-(2-methoxyethoxy)ethyl methacrylate is 188.22 g / mol.

[0014] Furthermore, the Mn of the polyethylene glycol methyl ether methacrylate is 475 g / mol.

[0015] Furthermore, during the preparation of the core material solution, 1 mL of essential oil nanoemulsion is added to every 0.5-1 mg of core-shell structured mesoporous silica; the essential oil nanoemulsion is prepared from essential oil, Tween 80, and deionized water by ultrasonic treatment.

[0016] Furthermore, the essential oils include any one or more of thyme essential oil, clove essential oil, oregano essential oil, litsea cubeba essential oil, wintergreen oil, safflower oil, wormwood oil, ginger oil, Chuanxiong oil, fangfeng oil, Panax notoginseng oil, peony root oil, cinnamon oil, lycopodiella cava oil, peppermint oil, menthol, angelica oil, lavender essential oil, rose essential oil, ginseng essential oil, angelica pubescens essential oil, lemon essential oil, citronella essential oil, peppermint oil, eucalyptus oil, arnica oil, frankincense essential oil, tangerine peel oil, smilax glabra oil, atractylodes oil, atractylodes macrocephala oil, Atlantic cedar oil, and Roman chamomile oil.

[0017] Furthermore, during the preparation of the popping beads, the melt viscosity of the ethylene-vinyl acetate copolymer is 150-250 MPa·s, the coolant temperature is 20-25°C, the core material temperature is 60-65°C, and the capsule drop height is 0.9-1.1 cm. The coolant is composed of an ethanol-water solution with a volume ratio of 100:6.

[0018] A method for preparing a popping bead blister comprises the following steps: preparing a glue layer on the surface of a coating by a glue dispensing process, placing a hole-punched sponge on the glue layer, placing popping beads in the holes of the hole-punched sponge, laminating an upper fabric to the coating to form a structure comprising an upper fabric, a middle core material, and a bottom fabric from top to bottom, ultrasonically pressing and cutting to prepare the popping bead blister.

[0019] The invention discloses an application of a bursting bead blister in a self-heating patch, wherein the application includes any one of a steam hot compress eye mask, a hot compress warming patch, a hot compress neck warming patch, a hot compress knee warming patch, a hot compress waist and abdomen patch, a hot compress ankle patch, and a hot compress wrist patch.

[0020] Compared with the prior art, the present invention has the following beneficial effects: 1. The present invention plans to prepare a temperature-controlled essential oil-releasing bursting bead blister to meet its applications in steam hot compress eye masks, hot compress warming patches, hot compress neck patches, hot compress knee patches, hot compress waist and abdomen patches, hot compress ankle patches, and hot compress wrist patches. The purpose is to meet the requirements of rapid release at the working temperature of 40 - 50 °C of self-heating patches and retention at room temperature. In the present invention, 2-(2-methoxyethoxy)ethyl methacrylate and methoxypolyethylene glycol methacrylate are polymerized through free radical polymerization to form a random copolymer. Utilizing the change in the hydration ability of the methoxypolyethylene glycol methacrylate chain segment. At low temperatures, the polymer chains are tightly bound to water molecules through hydrogen bonds, presenting a hydrophilic extended state; at high temperatures, the hydrogen bonds are broken, and the characteristic of the chain segment hydrophobic collapse. By adjusting the molar ratio of the two, a core-shell structured mesoporous silica is prepared on the surface of mesoporous silica. At low temperatures, the polymer shell layer expands, hindering the diffusion of essential oils; at high temperatures, the shell layer collapses, accelerating the release of essential oils through the "sponge extrusion" effect.

[0021] 2. The present invention further uses ethylene glycol dimethacrylate as a cross-linking agent to introduce a three-dimensional network structure during the copolymerization process to form a gel-like shell layer. Cross-linking restricts the mobility of the polymer chains but retains the temperature responsiveness. The cross-linked shell layer can still absorb and retain drug molecules at low temperatures, while showing a stronger "extrusion" effect during high-temperature collapse, and the release rate is significantly higher than that of the linear polymer shell layer, further improving the essential oil release rate of the bursting bead at high temperatures.

[0022] 3. The present invention innovatively uses benzalkonium chloride as a template agent to prepare mesoporous silica with antibacterial properties, realizing the construction of the mesoporous structure and the loading of the template agent in a one-step hydrothermal reaction manner, avoiding the influence of the addition of additional antibacterial agents on the loading performance of mesoporous silica, simplifying the process flow, greatly improving the production efficiency, and reducing the production cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a top view structural schematic diagram of a bursting bead blister of the present invention; Figure 2 It is a side view structural schematic diagram of a bursting bead blister of the present invention; Among them, 1: Laminated film; 2: Perforated sponge; 3: Bursting bead; 4: Upper fabric. DETAILED DESCRIPTION OF THE EMBODIMENTS

[0024] Next, the technical solutions in the embodiments of the present invention will be clearly and completely described in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative efforts shall fall within the protection scope of the present invention.

[0025] In the following examples, the preparation method of the essential oil nanoemulsion comprises the following steps: Add 20 mL of thyme essential oil and 5 mL of Tween 80 into a reaction vessel, stir evenly, add 75 mL of deionized water, stir evenly, and perform ultrasonic treatment at 350 W to obtain the essential oil nanoemulsion.

[0026] Example 1: A preparation method of a bursting bead blister comprises the following steps: S1: Add 4 mmol of benzalkonium chloride, 0.25 mmol of ammonia water, and 125 mL of deionized water into a reaction vessel, stir evenly, add 1 mmol of tetraethyl orthosilicate, stir evenly, heat to 80 °C and react for 72 h, filter, wash the solid product with deionized water, and vacuum dry at 50 - 55 °C to obtain antibacterial mesoporous silica; S2: Add 0.2 g of antibacterial mesoporous silica and 0.5 g of 3-aminopropyltriethoxysilane into toluene, stir evenly, heat to 125 °C and react for 24 h under an argon atmosphere, centrifuge, wash the product with ethanol, and vacuum dry at 50 °C to obtain amino-functionalized mesoporous silica; S3: Add 46 mg of amino-functionalized mesoporous silica, 0.324 mmol of RAFT reagent, and 1 equivalent of 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride into dry dichloromethane, stir at room temperature for 24 h under an argon atmosphere, centrifuge, wash the product with ethanol, and vacuum dry at 50 °C to obtain RAFT reagent-modified mesoporous silica; S4: Add 40 mg of RAFT reagent-modified mesoporous silica, 92 mmol of 2-(2-methoxyethoxy)ethyl methacrylate, 8 mmol of methoxypolyethylene glycol methacrylate, and 4 mmol% of ethylene glycol dimethacrylate into ethanol, ultrasonically disperse, add azobisisobutyronitrile, stir at room temperature for 45 min under an argon atmosphere, heat to 70 °C and react for 24 h, centrifuge, and wash the product with ethanol to obtain core-shell structured mesoporous silica; S5: Add 1 mg of core-shell structured mesoporous silica into 1 mg of the essential oil nanoemulsion, stir at room temperature for 12 h, and stir at 45 °C for 3 h to obtain the core material solution; S6: Using ethylene-vinyl acetate copolymer as the bursting bead wall material and the core material solution as the core material, solidify the capsules dropped by the dropper head in the coolant, filter, and wash to obtain bursting bead 3; wherein, the melt viscosity of the ethylene-vinyl acetate copolymer is 200 MPa·s, the temperature of the coolant is 25 °C, the temperature of the core material is 65 °C, and the dropping height of the capsule is 1 cm; S7: Prepare an adhesive layer on the surface of the film laminating layer 1 through a dispensing process, place the perforated sponge 2 on the adhesive layer, place the bursting bead 3 in the holes of the perforated sponge 2, bond the upper fabric 4 with the film laminating layer 1 to form a structure consisting of the upper fabric 4, the middle core material, and the bottom fabric from top to bottom, perform ultrasonic pressing and cutting to prepare a bursting bead blister.

[0027] Example 2: A method for preparing a bursting bead blister, comprising the following steps: S1: Add 6 mmol of benzalkonium chloride, 0.25 mmol of ammonia water, and 125 mL of deionized water into a reaction vessel, stir evenly, add 1.25 mmol of tetraethyl orthosilicate, stir evenly, heat to 80 °C and react for 72 h, filter, wash the solid product with deionized water, and perform vacuum drying at 50 - 55 °C to obtain antibacterial mesoporous silica; S2: Add 0.2 g of antibacterial mesoporous silica and 0.5 g of 3-aminopropyltriethoxysilane into toluene, stir evenly, under an argon atmosphere, heat to 125 °C and react for 24 h, centrifuge, wash the product with ethanol, and perform vacuum drying at 50 °C to obtain amino-functionalized mesoporous silica; S3: Add 46 mg of amino-functionalized mesoporous silica, 0.324 mmol of RAFT reagent, and 1 equivalent of 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride into dry dichloromethane, under an argon atmosphere, stir at room temperature for 24 h, centrifuge, wash the product with ethanol, and perform vacuum drying at 50 °C to obtain RAFT reagent-modified mesoporous silica; S4: Add 40 mg of RAFT reagent-modified mesoporous silica, 92 mmol of 2-(2-methoxyethoxy)ethyl methacrylate, 8 mmol of methoxypolyethylene glycol methacrylate, and 4 mmol% of ethylene glycol dimethacrylate into ethanol, perform ultrasonic dispersion, add azobisisobutyronitrile, under an argon atmosphere, stir at room temperature for 45 min, heat to 70 °C and react for 24 h, centrifuge, wash the product with ethanol to obtain core-shell structured mesoporous silica; S5: Add 1 mg of core-shell structured mesoporous silica into 1 mg of essential oil nanoemulsion, stir at room temperature for 12 h, heat to 45 °C and stir for 3 h to obtain a core material solution; S6: Use ethylene-vinyl acetate copolymer as the bursting bead wall material and the core material solution as the core material, solidify the capsules dropped by the dropper head in the coolant, filter and wash to obtain the bursting bead 3; wherein, the melt viscosity of the ethylene-vinyl acetate copolymer is 200 MPa·s, the coolant temperature is 25 °C, the core material temperature is 65 °C, and the capsule dropping height is 1 cm; S7: Prepare a glue layer on the surface of the laminating film 1 by a dispensing process, place the hole-punched sponge 2 on the glue layer, place the bursting beads 3 in the holes of the hole-punched sponge 2, and fit the upper fabric 4 to the laminating film 1 to form a structure of upper fabric 4, middle core material, and bottom fabric from top to bottom, perform ultrasonic pressing, and cut to prepare the bursting bead blister.

[0028] Example 3: A method for preparing a popping bubble capsule, comprising the following steps: S1: adding 6 mmol of benzalkonium chloride, 0.25 mmol of ammonia water, and 125 mL of deionized water to a reaction vessel, stirring evenly, adding 1.25 mmol of ethyl orthosilicate, stirring evenly, heating to 80° C. to react for 72 h, filtering, washing the solid product with deionized water, and vacuum drying at 50-55° C. to obtain antibacterial mesoporous silica; S2: Add 0.2 g of antibacterial mesoporous silica and 0.5 g of 3-aminopropyltriethoxysilane to toluene, stir evenly, heat to 125°C under argon atmosphere, react for 24 h, centrifuge, wash the product with ethanol, and dry it in vacuum at 50°C to obtain amino-modified mesoporous silica; S3: 46 mg of amino-modified mesoporous silica, 0.324 mmol of RAFT reagent, and 1 equivalent of 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride were added to dry dichloromethane. The mixture was stirred at room temperature for 24 h under an argon atmosphere. The mixture was centrifuged, washed with ethanol, and dried under vacuum at 50°C to obtain RAFT reagent-modified mesoporous silica. S4: 40 mg of RAFT agent-modified mesoporous silica, 90 mmol of 2-(2-methoxyethoxy)ethyl methacrylate, 10 mmol of polyethylene glycol methyl ether methacrylate, and 4 mmol% of ethylene glycol dimethacrylate were added to ethanol and ultrasonically dispersed. Azobisisobutyronitrile was added and stirred at room temperature for 45 min under argon atmosphere. The mixture was heated to 70°C for 24 h, centrifuged, and the product was washed with ethanol to obtain core-shell structured mesoporous silica. S5: Add 1 mg of core-shell mesoporous silica to 1 mg of essential oil nanoemulsion, stir at room temperature for 12 h, heat to 45 °C and stir for 3 h to obtain a core material solution; S6: Using ethylene-vinyl acetate copolymer as the wall material of the popping beads and the core material solution as the core material, the capsules dripped from the dripper were solidified in the coolant, filtered, and washed to obtain popping beads 3; wherein the melt viscosity of the ethylene-vinyl acetate copolymer was 200 MPa·s, the coolant temperature was 25°C, the core material temperature was 65°C, and the capsule dripping height was 1 cm; S7: A glue layer is prepared on the surface of the film laminating 1 through a dispensing process. The perforated sponge 2 is placed on the glue layer, the bursting bead 3 is placed in the holes of the perforated sponge 2, and the upper fabric 4 is laminated with the film laminating 1 to form a structure consisting of the upper fabric 4, the middle core material, and the bottom fabric from top to bottom. Ultrasonic pressing and cutting are performed to prepare the bursting bead blister.

[0029] Comparative Example 1: A method for preparing a bursting bead blister, comprising the following steps: S1: 4 mmol of benzalkonium chloride, 0.25 mmol of ammonia water, and 125 mL of deionized water are added to a reaction vessel, stirred evenly, 1 mmol of tetraethyl orthosilicate is added, stirred evenly, heated to 80 °C and reacted for 72 h, filtered, the solid product is washed with deionized water, and vacuum dried at 50 - 55 °C to obtain antibacterial mesoporous silica; S2: 0.2 g of antibacterial mesoporous silica and 0.5 g of 3-aminopropyltriethoxysilane are added to toluene, stirred evenly, and under an argon atmosphere, heated to 125 °C and reacted for 24 h, centrifuged, the product is washed with ethanol, and vacuum dried at 50 °C to obtain amino-functionalized mesoporous silica; S3: 46 mg of amino-functionalized mesoporous silica, 0.324 mmol of RAFT reagent, and 1 equivalent of 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride are added to dry dichloromethane, and under an argon atmosphere, stirred at room temperature for 24 h, centrifuged, the product is washed with ethanol, and vacuum dried at 50 °C to obtain RAFT reagent-modified mesoporous silica; S4: 40 mg of RAFT reagent-modified mesoporous silica, 99 mmol of 2-(2-methoxyethoxy)ethyl methacrylate, 1 mmol of methoxypolyethylene glycol methacrylate, and 4 mmol% of ethylene glycol dimethacrylate are added to ethanol, ultrasonically dispersed, azobisisobutyronitrile is added, and under an argon atmosphere, stirred at room temperature for 45 min, heated to 70 °C and reacted for 24 h, centrifuged, and the product is washed with ethanol to obtain core-shell structured mesoporous silica; S5: 1 mg of core-shell structured mesoporous silica is added to 1 mg of essential oil nanoemulsion, stirred at room temperature for 12 h, and heated to 45 °C and stirred for 3 h to obtain a core material solution; S6: Using ethylene-vinyl acetate copolymer as the bursting bead wall material and the core material solution as the core material, the capsules dropped by the dropper are solidified and formed in a coolant, filtered, and washed to obtain the bursting bead 3; wherein, the melt viscosity of the ethylene-vinyl acetate copolymer is 200 MPa·s, the coolant temperature is 25 °C, the core material temperature is 65 °C, and the capsule dropping height is 1 cm; S7: Prepare an adhesive layer on the surface of the film lamination 1 by the dispensing process, place the perforated sponge 2 on the adhesive layer, place the bursting bead 3 in the holes of the perforated sponge 2, bond the upper fabric 4 with the film lamination 1 to form a structure with the upper fabric 4, the middle core material, and the bottom fabric from top to bottom, perform ultrasonic pressing and cutting to prepare the bursting bead blister.

[0030] Comparative Example 2: A method for preparing a bursting bead blister, comprising the following steps: S1: Add 4 mmol of benzalkonium chloride, 0.25 mmol of ammonia water, and 125 mL of deionized water to a reaction vessel, stir evenly, add 1 mmol of tetraethyl orthosilicate, stir evenly, heat to 80 °C and react for 72 h, filter, wash the solid product with deionized water, and dry it under vacuum at 50 - 55 °C to obtain antibacterial mesoporous silica; S2: Add 0.2 g of antibacterial mesoporous silica and 0.5 g of 3-aminopropyltriethoxysilane to toluene, stir evenly, under an argon atmosphere, heat to 125 °C and react for 24 h, centrifuge, wash the product with ethanol, and dry it under vacuum at 50 °C to obtain amino-functionalized mesoporous silica; S3: Add 46 mg of amino-functionalized mesoporous silica, 0.324 mmol of RAFT reagent, and 1 equivalent of 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride to dry dichloromethane, stir at room temperature for 24 h under an argon atmosphere, centrifuge, wash the product with ethanol, and dry it under vacuum at 50 °C to obtain RAFT reagent-modified mesoporous silica; S4: Add 40 mg of RAFT reagent-modified mesoporous silica, 80 mmol of 2-(2-methoxyethoxy)ethyl methacrylate, 20 mmol of methoxypolyethylene glycol methacrylate, and 4 mmol% of ethylene glycol dimethacrylate to ethanol, disperse ultrasonically, add azobisisobutyronitrile, stir at room temperature for 45 min under an argon atmosphere, heat to 70 °C and react for 24 h, centrifuge, and wash the product with ethanol to obtain core-shell structured mesoporous silica; S5: Add 1 mg of core-shell structured mesoporous silica to 1 mg of essential oil nanoemulsion, stir at room temperature for 12 h, and heat to 45 °C and stir for 3 h to obtain the core material solution; S6: Use ethylene-vinyl acetate copolymer as the bursting bead wall material and the core material solution as the core material, solidify the capsules dropped by the dropper head in the coolant, filter and wash to obtain the bursting bead 3; wherein, the melt viscosity of the ethylene-vinyl acetate copolymer is 200 MPa·s, the coolant temperature is 25 °C, the core material temperature is 65 °C, and the capsule dropping height is 1 cm; S7: A glue layer is prepared on the surface of the lamination film 1 through a dispensing process. The perforated sponge 2 is placed on the glue layer, the bursting bead 3 is placed in the holes of the perforated sponge 2, and the upper fabric 4 is laminated with the lamination film 1 to form a structure consisting of the upper fabric 4, the middle core material, and the bottom fabric from top to bottom. Ultrasonic pressing and cutting are performed to prepare the bursting bead blister.

[0031] Comparative Example 3: A method for preparing a bursting bead blister, comprising the following steps: S1: 4 mmol of benzalkonium chloride, 0.25 mmol of ammonia water, and 125 mL of deionized water are added to a reaction vessel, stirred evenly, 1 mmol of tetraethyl orthosilicate is added, stirred evenly, heated to 80 °C and reacted for 72 h, filtered, the solid product is washed with deionized water, and vacuum dried at 50 - 55 °C to obtain antibacterial mesoporous silica; S2: 0.2 g of antibacterial mesoporous silica and 0.5 g of 3-aminopropyltriethoxysilane are added to toluene, stirred evenly, heated to 125 °C and reacted for 24 h under an argon atmosphere, centrifuged, the product is washed with ethanol, and vacuum dried at 50 °C to obtain amino-functionalized mesoporous silica; S3: 46 mg of amino-functionalized mesoporous silica, 0.324 mmol of RAFT reagent, and 1 equivalent of 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride are added to dry dichloromethane, stirred at room temperature for 24 h under an argon atmosphere, centrifuged, the product is washed with ethanol, and vacuum dried at 50 °C to obtain RAFT reagent-modified mesoporous silica; S4: 40 mg of RAFT reagent-modified mesoporous silica, 92 mmol of 2-(2-methoxyethoxy)ethyl methacrylate, and 8 mmol of methoxypolyethylene glycol methacrylate are added to ethanol, ultrasonically dispersed, azobisisobutyronitrile is added, stirred at room temperature for 45 min under an argon atmosphere, heated to 70 °C and reacted for 24 h, centrifuged, and the product is washed with ethanol to obtain core-shell structured mesoporous silica; S5: 1 mg of core-shell structured mesoporous silica is added to 1 mg of essential oil nanoemulsion, stirred at room temperature for 12 h, and heated to 45 °C and stirred for 3 h to obtain the core material solution; S6: Using ethylene-vinyl acetate copolymer as the bursting bead wall material and the core material solution as the core material, the capsules dropped by the dropper are solidified and formed in the coolant, filtered, and washed to obtain the bursting bead 3; wherein, the melt viscosity of the ethylene-vinyl acetate copolymer is 200 MPa·s, the coolant temperature is 25 °C, the core material temperature is 65 °C, and the capsule dropping height is 1 cm; S7: A glue layer is prepared on the surface of the lamination film 1 through a dispensing process. The perforated sponge 2 is placed on the glue layer, the bursting bead 3 is placed in the holes of the perforated sponge 2, and the upper fabric 4 is laminated with the lamination film 1 to form a structure consisting of the upper fabric 4, the middle core material, and the bottom fabric from top to bottom. Ultrasonic pressing and cutting are performed to prepare the bursting bead blister.

[0032] Comparative Example 4: A preparation method of a pearl essence blister, comprising the following steps: S1: Add 8 mmol of benzalkonium chloride, 0.25 mmol of ammonia water, and 125 mL of deionized water into a reaction vessel, stir evenly, add 1 mmol of tetraethyl orthosilicate, stir evenly, heat to 80 °C and react for 72 h, filter, wash the solid product with deionized water, and dry it under vacuum at 50 - 55 °C to obtain antibacterial mesoporous silica; S2: Add 0.2 g of antibacterial mesoporous silica and 0.5 g of 3-aminopropyltriethoxysilane into toluene, stir evenly, under an argon atmosphere, heat to 125 °C and react for 24 h, centrifuge, wash the product with ethanol, and dry it under vacuum at 50 °C to obtain amino-functionalized mesoporous silica; S3: Add 46 mg of amino-functionalized mesoporous silica, 0.324 mmol of RAFT reagent, and 1 equivalent of 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride into dry dichloromethane, stir at room temperature for 24 h under an argon atmosphere, centrifuge, wash the product with ethanol, and dry it under vacuum at 50 °C to obtain RAFT reagent-modified mesoporous silica; S4: Add 40 mg of RAFT reagent-modified mesoporous silica, 92 mmol of 2-(2-methoxyethoxy)ethyl methacrylate, 8 mmol of methoxypolyethylene glycol methacrylate, and 4 mmol% of ethylene glycol dimethacrylate into ethanol, disperse by ultrasonic wave, add azobisisobutyronitrile, stir at room temperature for 45 min under an argon atmosphere, heat to 70 °C and react for 24 h, centrifuge, wash the product with ethanol to obtain core-shell structured mesoporous silica; S5: Add 1 mg of core-shell structured mesoporous silica into 1 mg of essential oil nanoemulsion, stir at room temperature for 12 h, and heat to 45 °C and stir for 3 h to obtain a core material solution; S6: Using ethylene-vinyl acetate copolymer as the blister wall material and the core material solution as the core material, solidify the capsules dropped by the dropper head in the coolant, filter and wash to obtain pearl essence 3; wherein, the melt viscosity of the ethylene-vinyl acetate copolymer is 200 MPa·s, the coolant temperature is 25 °C, the core material temperature is 65 °C, and the capsule dropping height is 1 cm; S7: Prepare an adhesive layer on the surface of the coating film 1 through a dispensing process, place the perforated sponge 2 on the adhesive layer, place the pearl essence 3 in the holes of the perforated sponge 2, bond the upper fabric 4 with the coating film 1 to form a structure composed of the upper fabric 4, the middle core material, and the bottom fabric from top to bottom, ultrasonically press and cut to prepare a pearl essence blister.

[0033] Experiment: Temperature Responsiveness Test: Centrifuge the core material solution prepared in the above-mentioned examples and comparative examples to obtain mesoporous silica loaded with essential oil nanoemulsion; place the mesoporous silica in ultrapure water, test the temperature range from 20 to 50 °C, and the heating rate is 0.5 °C / min, and compare the release rates of the essential oil nanoemulsion at 20 °C and 50 °C.

[0034] The experimental data are shown in Table 1 below.

[0035]

[0036] Conclusion: The characteristics of the prepared bursting beads blister of the present invention with low temperature (20 °C) retention and high temperature (50 °C) release can match the working temperature (40 - 50 °C) of steam hot compress eye masks, hot compress warm care patches, hot compress warm neck patches, hot compress warm knee patches, hot compress waist and abdomen patches, hot compress ankle patches, and hot compress wrist patches. Combined with the antibacterial properties of benzalkonium chloride on the surface of mesoporous silica, the service life of the bursting beads blister is greatly extended, and the application scenarios of the bursting beads blister are broadened.

[0037] During the preparation process of Comparative Example 1, the amount of 2-(2-methoxyethoxy)ethyl methacrylate was increased and the amount of methoxypolyethylene glycol methacrylate was decreased, resulting in a decrease in low-temperature retention performance.

[0038] During the preparation process of Comparative Example 2, the amount of 2-(2-methoxyethoxy)ethyl methacrylate was decreased and the amount of methoxypolyethylene glycol methacrylate was increased, resulting in a decrease in high-temperature release performance.

[0039] During the preparation process of Comparative Example 3, ethylene glycol dimethacrylate was not added, lacking the copolymerization of the bisacrylate group with the polymer chain segment to form a three-dimensional chemical cross-linking network, resulting in a decrease in the extrusion effect when the network collapses and a decrease in high-temperature release performance.

[0040] During the preparation process of Comparative Example 4, the amount of benzalkonium chloride added was too much, and the amount of template agent added was too much, resulting in too large pores in the mesoporous silica and a lack of structure, resulting in a decrease in low-temperature retention and high-temperature release performance.

[0041] For those skilled in the art, it is obvious that the present invention is not limited to the details of the above-mentioned exemplary embodiments, and can be implemented in other specific forms without departing from the spirit or basic characteristics of the present invention. Therefore, from any point of view, the embodiments should be regarded as exemplary and non-limiting. The scope of the present invention is defined by the appended claims rather than the above description. Therefore, all changes falling within the meaning and scope of the equivalent elements of the claims are intended to be included in the present invention. Any reference signs in the claims should not be regarded as limiting the claims involved.

Claims

1. A popping bead blister, characterized in that: The bead blister structure includes: an upper fabric (4), a middle core material, and a bottom fabric; the middle core material is composed of a perforated sponge (2) and beads (3) embedded in the holes of the perforated sponge (2); the bottom fabric is composed of a coating (1) and an adhesive layer prepared by a dotting process on the surface of the coating (1).

2. The popping bead blister according to claim 1, characterized in that: The preparation method of the beads (3), comprises the following steps: S1: Add benzalkonium chloride, ammonia water, and deionized water into a reaction vessel, stir evenly, add tetraethyl orthosilicate, stir evenly, heat to 80 - 85 °C and react for 72 h, filter, wash the solid product with deionized water, and vacuum dry at 50 - 55 °C to obtain antibacterial mesoporous silica; S2: Add the antibacterial mesoporous silica and 3-aminopropyltriethoxysilane into toluene, stir evenly, under an argon atmosphere, heat to 125 - 130 °C and react for 24 h, centrifuge, wash the product with ethanol, and vacuum dry at 50 - 55 °C to obtain amino-functionalized mesoporous silica; S3: Add the amino-functionalized mesoporous silica, RAFT reagent, and 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride into dry dichloromethane, under an argon atmosphere, stir at room temperature for 24 h, centrifuge, wash the product with ethanol, and vacuum dry at 50 - 55 °C to obtain RAFT reagent-modified mesoporous silica; S4: Add the RAFT reagent-modified mesoporous silica, 2-(2-methoxyethoxy)ethyl methacrylate, methoxypolyethylene glycol methacrylate, and ethylene glycol dimethacrylate into ethanol, ultrasonically disperse, add azobisisobutyronitrile, under an argon atmosphere, stir at room temperature for 45 - 60 min, heat to 70 - 75 °C and react for 24 h, centrifuge, wash the product with ethanol to obtain core-shell structured mesoporous silica; S5: Add the core-shell structured mesoporous silica into an essential oil nanoemulsion, stir at room temperature for 12 - 24 h, heat to 45 - 50 °C and stir for 3 - 4 h to obtain a core material solution; S6: Using ethylene-vinyl acetate copolymer as the bead wall material and the core material solution as the core material, solidify the capsules dropped by the dropper head in a coolant, filter and wash to obtain the beads (3).

3. A popping bead blister according to claim 1, characterized in that: During the preparation of the antibacterial mesoporous silica, the molar ratio of tetraethyl orthosilicate:benzalkonium chloride:ammonia water is (1 - 1.25):(4 - 6):(0.25 - 0.3).

4. A popping bead blister according to claim 1, characterized in that: During the preparation of the amino-functionalized mesoporous silica, the mass ratio of the antibacterial mesoporous silica to 3-aminopropyltriethoxysilane is (0.1 - 0.2):(0.5 - 1).

5. A bursting bead blister according to claim 1, characterized in that: During the preparation of the RAFT reagent-modified mesoporous silica, 0.324 - 0.346 mmol of the RAFT reagent is added to every 46 mg of the amino-functionalized mesoporous silica; the RAFT reagent is 3-benzylthio thiocarbonylthiopropionic acid.

6. The bursting bead blister according to claim 1, wherein: During the preparation of the core-shell structured mesoporous silica, the molar ratio of 2-(2-methoxyethoxy)ethyl methacrylate to methoxypolyethylene glycol methacrylate is (90 - 92):(8 - 10); the addition amount of ethylene glycol dimethacrylate is 4 - 5% of the total molar amount of the monomers.

7. A popping bead blister according to claim 1, characterized in that: During the preparation of the core material solution, 1 mL of essential oil nanoemulsion is added to every 0.5 - 1 mg of core - shell structured mesoporous silica.

8. A popping bead blister according to claim 1, characterized in that: During the preparation of the bursting beads (3), the melt viscosity of the ethylene - vinyl acetate copolymer is 150 - 250 MPa·s, the temperature of the coolant is 20 - 25 °C, the temperature of the core material is 60 - 65 °C, and the dropping height of the capsules is 0.9 - 1.1 cm.

9. A preparation method of a bursting bead blister, characterized in that: It includes the following steps: A glue layer is prepared on the surface of the film - laminating (1) through a dispensing process. The perforated sponge (2) is placed on the glue layer, the bursting beads (3) are placed in the holes of the perforated sponge (2), the upper fabric (4) is laminated with the film - laminating (1) to form a structure with the upper fabric (4), the middle - layer core material, and the bottom fabric from top to bottom, and then ultrasonic pressing and cutting are carried out to prepare the bursting bead blister.

10. The application of a popping bead blister in a self-heating patch according to claim 1, wherein: The application includes any one of a steam hot compress eye mask, a hot compress warming patch, a hot compress neck patch, a hot compress knee patch, a hot compress waist - abdomen patch, a hot compress ankle patch, and a hot compress wrist patch.