Method for preparing superfine silver powder by using sulfate radical as protective agent

By introducing sulfate as a protective agent, the problem of polymer organic matter adhesion in traditional silver powder production was solved, the recycling of nitrate and the difficulty of wastewater treatment was achieved, and ultrafine silver powder with good dispersion and particle size distribution was prepared.

CN120516008APending Publication Date: 2025-08-22FUZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510813317.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-06-18
Publication Date
2025-08-22

AI Technical Summary

Technical Problem

When preparing silver powder by traditional liquid phase reduction method, polymer organic matter is closely attached to the surface of the silver powder, resulting in complex washing process and difficult to completely remove, affecting product quality, and producing high-concentration nitrate-organic compound mixed waste liquid, increasing the cost of wastewater treatment.

Method used

Use sulfate as a protective agent to precipitate silver ions through sulfate to form silver sulfate intermediates, realize nitrate recycling, avoid the use of polymer organic matter, and prepare ultrafine silver powder.

Benefits of technology

The recycling of nitrate is realized, production costs are reduced, wastewater treatment is simplified, and ultrafine silver powder with good dispersion and narrow particle size distribution is prepared.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120516008A_ABST
    Figure CN120516008A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing superfine silver powder by taking sulfate radical as a protective agent, which comprises the following steps: (1) precipitation: adding sulfuric acid into a silver nitrate aqueous solution, mixing, and performing solid-liquid separation to obtain silver sulfate precipitate and a mixed acid solution containing nitric acid and sulfuric acid; (2) circulation: adding the silver block into a mixed acid solution, and heating and stirring until the silver block is dissolved; (3) dissolving: adding the silver sulfate precipitate into an ammonia water solution to obtain a clear silver ammonia solution; and (4) reduction is conducted, specifically, the reducing agent solution is added into the silver-ammonia solution in the stirring state, filtering is conducted after stirring, sediment is cleaned till the conductivity is smaller than 25 microseconds / cm, and superfine silver powder is obtained after drying and powder screening are conducted. Sulfuric acid is introduced to precipitate silver ions in the silver nitrate solution, cyclic utilization of the nitrate solution is achieved, the production cost is reduced, the silver nitrate solution serves as a protective agent in the reduction preparation process of the silver powder, agglomeration and oxidation of the silver powder are effectively prevented, and the sphericity degree of the silver powder is good, and particle size distribution is uniform.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of ultrafine silver powder preparation, and in particular to a method for preparing ultrafine silver powder by using sulfate radical as a protective agent. Background Art

[0002] Silver powder, with its excellent electrical and thermal conductivity and chemical stability, is the most widely used precious metal powder in the electronics industry. It is widely used in electronic components such as sensors, solar cell electrodes, thick-film integrated circuits, and flexible circuits. In the solar photovoltaic industry in particular, silver powder accounts for approximately 32% of the non-silicon cost of solar cells and approximately 8% of the overall cell cost. Silver powder is a key factor in the preparation of silver paste (which primarily consists of silver powder, glass oxide, and an organic carrier). Its production technology is highly specialized, and any parameter changes can significantly affect the final product performance.

[0003] Currently, the industrial production of silver powder primarily relies on a liquid-phase reduction method, typically using silver nitrate as a silver precursor. Under the protection of polymers such as polyvinylpyrrolidone (PVP) and polyacrylic acid (PAA), reducing agents such as ascorbic acid, ethylene glycol, formaldehyde, and sodium borohydride are used. By manipulating solution parameters, silver powders of varying morphologies and particle sizes can be produced. This method offers advantages such as simple process equipment, good product controllability, high productivity, and ease of industrial production.

[0004] However, while the traditional liquid-phase reduction method for preparing silver powder using high-molecular-weight organic compounds as protective agents can effectively control the morphology and particle size of the silver powder, it also presents a series of challenges. The primary issue is that the organic matter adheres tightly to the surface of the silver powder, making the subsequent washing process complicated and difficult to completely remove, thus affecting product quality. Furthermore, the process produces a highly concentrated nitrate-organic mixed wastewater, posing a potential threat to the environment and ecosystems and increasing the cost of wastewater purification.

[0005] Therefore, in order to solve the various problems or obstacles caused by the use of organic additives in the traditional silver powder production process, it is urgent to propose a new method for preparing ultrafine silver powder. Summary of the Invention

[0006] To address the above technical issues, the present invention proposes a low-cost method for preparing ultrafine silver powder using sulfate as a protective agent. This method introduces sulfuric acid to precipitate silver ions from a silver nitrate solution, thereby synthesizing a silver sulfate intermediate and achieving nitrate recycling. The precipitated silver sulfate solid is dissolved in ammonia water to form a silver ammonia solution, followed by the addition of a reducing agent to produce ultrafine silver powder. The resulting silver powder exhibits excellent sphericity, good dispersibility, and a narrow particle size distribution.

[0007] To achieve the above object, the present invention provides the following technical solutions: A method for preparing ultrafine silver powder at low cost by using sulfate as a protective agent, the method comprising the following steps: A method for preparing ultrafine silver powder using sulfate as a protective agent comprises the following steps: (1) Precipitation: Add sulfuric acid to a 20-100 g / L silver nitrate aqueous solution, mix, and separate the solid and liquid to obtain a silver sulfate precipitate and a mixed acid solution containing nitric acid and sulfuric acid; (2) Circulation: Add the silver block to the mixed acid solution, heat to 70 ~ 90 °C, and stir until the silver block dissolves; (3) Dissolution: adding the silver sulfate precipitate to an ammonia solution to obtain a clear silver ammonia solution, wherein the silver ion concentration in the silver ammonia solution is 10 to 50 g / L; (4) Reduction: Add a reducing agent solution with a concentration of 10 ~ 50 g / L to the silver ammonia solution in a stirring state, maintain the stirring temperature at 20 ~ 80 ℃. After the reaction is completed, filter and wash the precipitate until the conductivity is less than 25 μs / cm. After drying and sieving, ultrafine silver powder is obtained.

[0008] Furthermore, the concentration of the sulfuric acid solution in step (1) is 5 to 50 g / L.

[0009] Furthermore, the purity of the silver block in step (2) is 99.999%, and the solid-liquid ratio of the silver block to the mixed acid solution is 1 g:200 mL.

[0010] Furthermore, the concentration of the ammonia solution in step (3) is 1 to 5 mol / L, and the solid-to-liquid ratio of the silver sulfate precipitate to the ammonia solution is 10 g:140 mL.

[0011] Furthermore, in step (4), the reducing agent is one or more combinations of ethanol, ascorbic acid, hydrazine hydrate, sodium borohydride, sodium bisulfite, and glucose, and the reducing agent solution is prepared by dissolving the reducing agent in a 5% by mass ammonia aqueous solution.

[0012] Furthermore, in step (4), the reducing agent solution is added to the silver ammonia solution at a rate of 5 to 10 L / min.

[0013] Furthermore, the stirring speed in step (4) is 500-1000 r / min, the drying temperature is 50-70°C, and the drying time is 9-11 hours.

[0014] The tap density of the ultrafine silver powder prepared by the above preparation method is 5 ~ 6 g / cm 3 , particle size distribution D 10 At 0.3-0.4 μm, D 50 At 0.7-1.0 μm, D90 At 1.2-1.4μm.

[0015] This invention innovatively proposes a low-cost method for preparing ultrafine silver powder using sulfate as a protective agent. The introduction of sulfate not only enables the recycling of nitrate, alleviating the burden of wastewater treatment and reducing production costs, but also acts as a protective agent during the reduction process, preventing silver powder from agglomerating and oxidizing. The resulting silver powder exhibits excellent dispersibility, sphericity, and uniform particle size distribution. Compared to existing silver powder preparation methods, the advantages and benefits of this invention are: (1) Secondary utilization of resources: By introducing sulfuric acid to precipitate silver ions, the mixing of nitrate and organic matter is avoided, so that the nitrate solution can be used again to dissolve silver blocks, reducing production costs; (2) Reduce the difficulty of wastewater treatment: Under the action of sulfate protective agent, there is no need to add high molecular organic matter as a protective agent, which reduces the organic matter content in the wastewater and reduces the difficulty of wastewater treatment. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 Schematic diagram of the process of the present invention.

[0017] Figure 2 This is a scanning electron microscope image of the silver powder obtained in Example 1 of the present invention at a magnification of 30,000 times.

[0018] Figure 3 This is a scanning electron microscope image of the silver powder obtained in Example 2 of the present invention at a magnification of 30,000 times.

[0019] Figure 4 This is a scanning electron microscope image of the silver powder obtained in Example 3 of the present invention at a magnification of 30,000 times. DETAILED DESCRIPTION

[0020] In order to make the contents of the present invention easier to understand, the technical solutions of the present invention are further described below in conjunction with specific implementation methods, but the present invention is not limited thereto.

[0021] Example 1 The steps for preparing ultrafine silver powder at low cost using sulfate as a protective agent in the embodiment of the present invention are as follows: (1) Weigh 169.87 g of silver nitrate and dissolve it in 1000 mL of deionized water to obtain a silver nitrate solution with a silver concentration of 1 mol / L.

[0022] (2) Add 100 mL of 5 mol / L sulfuric acid solution to the above silver nitrate solution, stir for 5 minutes, and filter to obtain the silver sulfate precipitate and the solution containing nitrate and sulfate.

[0023] (3) Add 5 g of 99.999% silver to the 1000 mL of the above solution containing nitrate and sulfate, heat the solution to 80 °C, and stir for 5 h to dissolve.

[0024] (4) Add 72.27 g of silver sulfate precipitate to 1000 mL of 5 mol / L ammonia solution to prepare a silver ammonia complex ion solution with a silver ion concentration of 50 g / L.

[0025] (5) Weigh 25 g of ascorbic acid and dissolve it in 1000 mL of deionized water to obtain a solution with an ascorbic acid concentration of 25 g / L.

[0026] (6) Using a peristaltic pump, the ascorbic acid solution was pumped into the silver ammonia complex ion solution at a flow rate of 5 L / min and stirred at a speed of 1000 r / min. The solution was reacted for 10 min. The solution was then filtered and washed until the conductivity was less than 25 μs / cm. The solution was dried at 60 °C for 10 h and crushed and sieved to obtain ultrafine silver powder.

[0027] Example 2 (1) Weigh 169.87 g of silver nitrate and dissolve it in 1000 mL of deionized water to obtain a silver nitrate solution with a silver concentration of 1 mol / L.

[0028] (2) Add 100 mL of 5 mol / L sulfuric acid solution to the above silver nitrate solution, stir for 5 minutes, and filter to obtain the silver sulfate precipitate and the solution containing nitrate and sulfate.

[0029] (3) Add 5 g of 99.999% silver to 1000 mL of the above solution containing nitrate and sulfate, heat the solution to 90 °C, and stir for 5 h to dissolve.

[0030] (4) Add 72.27 g of silver sulfate precipitate to 1000 mL of 5 mol / L ammonia solution to prepare a silver ammonia complex ion solution with a silver ion concentration of 50 g / L.

[0031] (5) Weigh 25 g of sodium borohydride and dissolve it in 1000 mL of deionized water to obtain a solution with a sodium borohydride concentration of 25 g / L.

[0032] (6) Using a peristaltic pump, the sodium borohydride solution was pumped into the silver ammonia complex ion solution at a flow rate of 5 L / min and stirred at a speed of 1000 r / min. The reaction was continued for 10 min. The solution was then filtered and washed until the conductivity was less than 25 μs / cm. The solution was dried at 60 °C for 10 h and then crushed and sieved to obtain ultrafine silver powder.

[0033] Example 3 (1) Weigh 169.87 g of silver nitrate and dissolve it in 1000 mL of deionized water to obtain a silver nitrate solution with a silver concentration of 1 mol / L.

[0034] (2) Add 100 mL of 5 mol / L sulfuric acid solution to the above silver nitrate solution, stir for 5 minutes, and filter to obtain the silver sulfate precipitate and the solution containing nitrate and sulfate.

[0035] (3) Add 5 g of 99.999% silver to the 1000 mL of the above solution containing nitrate and sulfate, heat the solution to 90 °C, and stir to dissolve for 5 h.

[0036] (4) Add 72.27 g of silver sulfate precipitate to 1000 mL of 5 mol / L ammonia solution to prepare a silver ammonia complex ion solution with a silver ion concentration of 50 g / L.

[0037] (5) Weigh 25 g of sodium bisulfite and dissolve it in 1000 mL of 5% ammonia solution to obtain a sodium bisulfite solution with a concentration of 25 g / L.

[0038] (6) Use a peristaltic pump to pump the sodium bisulfite solution into the silver ammonia complex ion solution at a flow rate of 5 L / min at a stirring speed of 1000 r / min, and react for 10 minutes; then filter and wash the precipitate until the conductivity is less than 25 μs / cm, dry it at 60 °C for 10 hours, and obtain ultrafine silver powder after crushing and screening.

[0039] Comparative Example 1 (1) Weigh 169.87 g of silver nitrate and dissolve it in 1000 mL of deionized water to obtain a silver nitrate solution with a silver concentration of 1 mol / L.

[0040] (2) Add 15 g of 99.999% silver to the silver nitrate solution, heat the solution to 80 °C, stir and dissolve for 5 h, and then filter to obtain the undissolved silver and silver nitrate solution.

[0041] (3) Add the ammonia solution to the silver nitrate solution to form a silver ammonia complex ion solution with an ammonia concentration of 5 mol / L and a silver ion concentration of 50 g / L.

[0042] (4) Weigh 25 g of ascorbic acid and dissolve it in 1000 mL of 5% ammonia solution to obtain a solution with an ascorbic acid concentration of 25 g / L.

[0043] (5) Use a peristaltic pump to pump the ascorbic acid solution into the silver ammine complex ion solution at a flow rate of 5 L / min and stir at a speed of 1000 r / min, and react for 10 minutes; then filter and wash the precipitate until the conductivity is less than 25 μs / cm, dry it at 60 °C for 10 hours, and obtain ultrafine silver powder after crushing and screening.

[0044] Comparative Example 2 The same as Comparative Example 1, except that the reducing agent was changed to 25 g of sodium borohydride.

[0045] Comparative Example 3 The same as Comparative Example 1, except that the reducing agent was changed to 25 g of sodium bisulfite.

[0046] Calculation of secondary utilization rate of nitrate: Where, C 0 、C 1 are the nitrate concentrations in the solution before and after the silver block is dissolved, mol / L; V 0 、V 1 are the volume of solution before and after silver block dissolution, L; The performance comparison of Examples 1 to 3 and Comparative Examples 1 to 3 is shown in Table 1 below: Table 1 Performance test data of Examples 1 to 3 and Comparative Examples 1 to 3 As can be seen from Table 1, the secondary utilization rate of nitrate in Examples 1 to 3 of the present invention is more than 33%, and the tap density of the prepared samples is 5 g / cm 3 Above, the particle size distribution range is narrow, the particle size distribution D 10 At 0.3-0.4 μm, D 50 At 0.7-1.0 μm, D 90 At 1.2-1.4μm; combined Figure 2 、 3 , 4 The corresponding silver powder has good sphericity and dispersibility.

[0047] The embodiments described above are merely descriptions of preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Without departing from the spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by persons skilled in the art should fall within the scope of protection defined by the claims of the present invention.

Claims

1. A method for preparing ultrafine silver powder using sulfate as a protective agent, characterized in that: The following steps are involved: (1) Precipitation: Add sulfuric acid to a 20-100 g / L silver nitrate aqueous solution, mix, and separate the solid and liquid to obtain a silver sulfate precipitate and a mixed acid solution containing nitric acid and sulfuric acid; (2) Circulation: Add the silver block to the mixed acid solution, heat to 70 ~ 90 °C, and stir until the silver block dissolves; (3) Dissolution: adding the silver sulfate precipitate to an ammonia solution to obtain a clear silver ammonia solution, wherein the silver ion concentration in the silver ammonia solution is 10 to 50 g / L; (4) Reduction: Add a reducing agent solution with a concentration of 10 ~ 50 g / L to the silver ammonia solution in a stirring state, maintain the stirring temperature at 20 ~ 80 ℃. After the reaction is completed, filter and wash the precipitate until the conductivity is less than 25 μs / cm. After drying and sieving, ultrafine silver powder is obtained.

2. The preparation method according to claim 1, wherein: The concentration of the sulfuric acid solution in step (1) is 5-50 g / L.

3. The preparation method according to claim 1, wherein: The purity of the silver block in step (2) is 99.999%, and the solid-liquid ratio of the silver block to the mixed acid solution is 1 g:200 mL.

4. The preparation method according to claim 1, wherein: The concentration of the ammonia solution in step (3) is 1 to 5 mol / L, and the solid-liquid ratio of the silver sulfate precipitate to the ammonia solution is 10 g:140 mL.

5. The preparation method according to claim 1, wherein: In step (4), the reducing agent is one or more combinations of ethanol, ascorbic acid, hydrazine hydrate, sodium borohydride, sodium bisulfite, and glucose, and the reducing agent solution is prepared by dissolving the reducing agent in a 5% by mass ammonia aqueous solution.

6. The preparation method according to claim 1, wherein: In step (4), the reducing agent solution is added to the silver ammonia solution at a rate of 5 to 10 L / min.

7. The preparation method according to claim 1, wherein: The stirring speed in step (4) is 500-1000 r / min, the drying temperature is 50-70°C, and the drying time is 9-11 hours.

8. An ultrafine silver powder obtained by the preparation method according to any one of claims 1 to 7.

9. The ultrafine silver powder according to claim 8, characterized in that: The tap density of the ultrafine silver powder is 5 to 6 g / cm 3 , particle size distribution D 10 At 0.3-0.4 μm, D 50 At 0.7-1.0 μm, D 90 At 1.2-1.4μm.