Method for additive forming of high-performance Ti2AlNb three-period minimal curved surface lattice structure in nitrogen atmosphere
By performing L-PBF forming under a nitrogen-argon reaction atmosphere, the Ti2AlNb alloy is strengthened by using nitrogen atom gap solid solution and nitride precipitation, the strength and plastic matching problems of the three-period extremely small curved surface lattice structure are solved, and high-performance aerospace structural parts design is achieved.
Patent Information
- Application Number
- CN202510619852.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-14
- Publication Date
- 2025-08-26
AI Technical Summary
In the prior art, it is difficult to achieve a good match of strength, plasticity and toughness in three-period extremely small curved lattice structures in additive manufacturing. The effects of traditional particle strengthening and solid solution strengthening are limited, and there are problems with temperature field, stress field and component field complexity in the printing process of the lattice structure.
The laser powder bed melt forming was carried out under a nitrogen-argon reaction atmosphere, and the Ti2AlNb alloy was strengthened by nitrogen atom gap solid solution and nitride precipitation. The TPMS configuration was designed using implicit function modeling, and the L-PBF energy density parameter was optimized to achieve coordinated strength of the lattice structure.
It realizes high-performance forming of Ti2AlNb three-cycle extremely small curved lattice structure, with good matching strength and plasticity, meeting the lightweight and high-performance design needs of aerospace structural parts, and has high forming accuracy and compact structure without defects.
Smart Images

Figure CN120542073A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of additive manufacturing technology, and specifically relates to a method for additively forming a high-performance Ti2AlNb three-periodic minimal surface lattice structure under a nitrogen atmosphere. Background Art
[0002] Triple Periodic Minimal Surfaces (TPMS) lattice structures possess high porosity, high specific surface area, and mathematically controllable geometric topology. These properties endow them with exceptional physical and mechanical properties, such as high specific strength, high energy absorption capacity, and excellent fatigue resistance. Therefore, they hold broad application prospects in fields such as aerospace, where weight reduction is crucial. Furthermore, the smooth surface with zero mean curvature avoids the stress concentration at the nodes that is common in truss-like lattice structures, resulting in a more uniform stress distribution during load-bearing, attracting increasing attention. In recent years, additive manufacturing (AM) technologies, such as laser powder bed fusion (L-PBF), have rapidly developed, offering advantages such as fast forming speed, high precision, and the ability to fabricate complex geometric structures. Furthermore, AM-fabricated TPMS lattice structures offer a novel approach for the lightweight and high-performance design of aerospace components.
[0003] Studies have shown that the extremely high temperature gradient and cooling rate during L-PBF forming often lead to large residual stress in the printed samples, thereby deteriorating the mechanical properties of the TPMS lattice structure. At present, researchers eliminate residual stress by annealing the printed samples, but this inevitably reduces the strength of the lattice structure (YJ Liu, SJ Li, LC Zhang, et.al. Microstructure, defects and mechanical behavior of beta-type titanium porous structures manufactured by electron beam melting and selective laser melting [J]. Acta Materialia, 2016, 113: 56-67.); in addition, researchers use solution treatment + aging heat treatment to obtain a high volume fraction of strengthening phases such as O-Ti2AlNb phase, and use hot isostatic pressing to close the pores inside the lattice structure and achieve densification of the lattice structure. The alloy structure can also be regulated by heat treatment to reduce the influence of residual stress (XCYan, SJ Yue, JGGe, et.al. Microstructure and mechanical optimization of selective laser melted Ti6Al4V lattices: Effect of hotisostatic pressing [J]. Journal of Manufacturing Process, 2022, 77: 151-162.). However, both of the above methods precipitate a large amount of brittle α2 phase during the slow cooling process, which reduces the plasticity of the material and has limited effect on improving the mechanical properties of the material. Therefore, it is urgent to find a new strengthening method for Ti2AlNb three-periodic minimal surface lattice structure.
[0004] Since nitrogen has a high solid solubility in titanium alloys, and based on the laser in-situ nitriding strengthening method, that is, by precisely controlling the gas atmosphere ratio (nitrogen-argon, i.e., N2-Ar reaction atmosphere) during the L-PBF forming process, the microstructure of the Ti2AlNb alloy during the L-PBF forming process is regulated by the interstitial solid solution of nitrogen atoms into the matrix and the reaction precipitation of nitrides, thereby achieving synergistic strengthening and toughening of the TPMS lattice structure. (LTLiu, CYChen, RXZhao, et.al. In-situ nitrogen strengthening of selective laser melted Ti6Al4V with superior mechanical performance[J]. Additive Manufacturing, 2021, 46: 102142.). In addition, during the L-PBF forming process, the Ti2AlNb pre-alloyed powder inside the laser working area is completely melted, and it is in full contact with the reactive atmosphere (N2) to achieve complete alloying. Macroscopically, it manifests as nitrogen atoms or nitrides uniformly distributed in each printed layer (DWWang, YHZhou, M.Yan, et.al. Selective laser melting under the reactive atmosphere: A convenient and efficient approach to fabricate ultrahighstrength commercially pure titanium without sacrificing ductility[J]. Materials Science and Engineering A, 2019, 762: 138078.). Currently, researchers have achieved synergistic strengthening of Ti2AlNb bulk alloys by nitrogen interstitial solid solution and reaction precipitation during the L-PBF forming process by designing an argon-nitrogen reaction atmosphere. This has increased the yield strength and tensile strength of Ti2AlNb bulk alloys from 932 MPa and 947 MPa to 1080 MPa and 1099 MPa, respectively, at room temperature (Han Yongdian, Chen Qiang, Xu Lianyong, et al. A powder additive manufacturing method for strengthening Ti2AlNb alloys by nitrogen interstitial solid solution [P]. Publication No. CN 118854104 A). In summary, laser in-situ atmosphere strengthening is expected to yield high-performance Ti2AlNb three-periodic minimal surface lattice structures.However, compared with bulk alloys formed by L-PBF, the temperature field, stress field and composition field of the TPMS lattice structure during the printing process are more complex. In order to meet the requirements of forming high-performance Ti2AlNb lattice structures with dense and defect-free organization, high forming precision and good mechanical properties under a reaction atmosphere, it is necessary to conduct in-depth research on the L-PBF energy density parameter matching such as laser power and scanning speed, as well as the mechanical properties of the prepared materials under the corresponding parameters.
[0005] Based on the above reasons, the present invention proposes to perform L-PBF forming in a nitrogen-argon reaction atmosphere, strengthen the Ti2AlNb alloy through interstitial solid solution of nitrogen atoms and precipitation of nitrides, and achieve synergistic strengthening and toughening of the lattice structure. Summary of the Invention
[0006] The technical problem solved by the present invention is to provide a method for additively forming a high-performance Ti2AlNb three-periodic minimal surface lattice structure under a nitrogen atmosphere. In order to meet the design requirements of lightweight and high-performance key structural parts in fields such as aerospace, the present invention uses implicit function modeling to design a Ti2AlNb lattice structure with a TPMS configuration. In a nitrogen-argon reaction atmosphere, the Ti2AlNb lattice structure with a TPMS configuration is formed by L-PBF, thereby solving the problems of uneven reinforcement distribution and limited solid solution strengthening effect in traditional particle strengthening, and achieving a good match between the strength, plasticity and toughness of the lattice structure.
[0007] In order to achieve the above object, the technical solution adopted by the present invention is:
[0008] A method for additively forming a high-performance Ti2AlNb three-periodic minimal surface lattice structure in a nitrogen atmosphere comprises the following steps:
[0009] Step 1) Implicit function modeling of the TPMS configuration: Design a CAD model of the TPMS configuration and export it as an STL file;
[0010] Step 2) Pre-processing of L-PBF Ti2AlNb lattice structure: Slice the STL file and set the process parameters;
[0011] Step 3) L-PBF forming of a Ti2AlNb lattice structure: forming a Ti2AlNb lattice structure by L-PBF technology in a nitrogen-argon mixed atmosphere;
[0012] Step 4) Surface treatment is performed on the TPMS configuration Ti2AlNb lattice structure.
[0013] In the above step 1), the TPMS configuration is selected from one of Gyroid, Diamond or Primitive, and implicit function modeling is performed using nTopology software to obtain a CAD model of the lattice structure. The model for L-PBF forming is exported as an STL model file.
[0014] The volume fraction of the lattice structure is 7.5%-50%.
[0015] In step 2) above, first, the STL model file of the lattice structure obtained in step 1) is imported into Materialise Magics software for layered slicing. Then, the processed SCAN file is imported into a laser powder bed fusion device. Secondly, a titanium alloy substrate is placed in the forming chamber of the laser powder bed fusion device, and the position of the substrate is adjusted so that the upper surface of the substrate is covered with a uniform and complete layer of Ti2AlNb powder. Finally, a mixture of nitrogen and argon is used to dilute and exhaust the oxygen in the forming cavity and pipeline, so that the oxygen content in the forming cavity is less than 200 ppm.
[0016] The Ti2AlNb powder used above is dried at a temperature of 80-100°C for 2 hours. The thickness of the slice layer of the lattice structure is 0.03 mm, and the proportion of nitrogen during the printing process is controlled to be 1-10 vol.%.
[0017] In the above step 3), the L-PBF forming of the lattice structure is achieved by adjusting the laser input energy density; after the substrate temperature is cooled to room temperature, the Ti2AlNb lattice structure is cut from the substrate, ultrasonically cleaned and dried for later use;
[0018] The L-PBF process parameters include: laser power of 150-250W, scanning speed of 800-1400mm / s, scanning spacing of 0.05-0.15mm, and layer thickness of 0.02-0.05mm; the laser scanning strategy is checkerboard scanning, and the scanning direction between adjacent layers is rotated 67°; the preheat temperature of the titanium alloy substrate is 90°.
[0019] In the above step 4), the surface treatment includes sandblasting or electrolytic polishing.
[0020] The Ti2AINb powder used for L-PBF forming is prepared by the plasma rotating electrode method. Its chemical composition is: AI: 22-25at.%, Nb: 20-30at.%, Ta: 0-7at.%, and the balance is Ti. The powder particle size used for printing is 15-53μm.
[0021] The advantages of the present invention compared with the prior art are:
[0022] 1. This solution uses L-PBF to form a TPMS-shaped Ti2AlNb lattice structure in a nitrogen-argon reaction atmosphere, thereby solving the problems of uneven reinforcement distribution and limited solid solution strengthening in traditional particle reinforcement. This helps achieve a good match between the strength, plasticity, and toughness of the lattice structure, providing a new approach for the lightweight and high-performance design and preparation of aerospace structural parts.
[0023] 2. This solution takes into account that nitrogen has a higher thermal conductivity than argon, resulting in a larger temperature gradient within the molten pool under a nitrogen atmosphere. Therefore, compared with the Ti2AlNb alloy formed by L-PBF in a pure argon atmosphere, the Ti2AlNb alloy formed in a nitrogen-argon reaction atmosphere has a finer grain structure and a more significant strengthening effect;
[0024] 3. Compared with bulk alloys formed by L-PBF, the temperature field, stress field, and composition field of the TPMS lattice structure during the printing process are more complex in this scheme. The L-PBF energy density parameters are optimized, and the mechanical properties of the prepared materials under the corresponding parameters are evaluated to meet the requirements of forming high-performance Ti2AlNb lattice structures with dense and defect-free organization, high forming accuracy, and good mechanical properties under the reaction atmosphere. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 Schematic diagram of the Ti2AlNb three-periodic minimal surface lattice structure formed by additive manufacturing under a nitrogen atmosphere in the present invention;
[0026] Figure 2 CAD model diagram and macroscopic morphology photos of the Ti2AlNb lattice structure under different L-PBF process parameters in the present invention;
[0027] Figure 3 This is a SEM photograph of the L-PBF formed lattice structure in the present invention under a nitrogen-argon reaction atmosphere;
[0028] Figure 4 Figure 2 shows the room temperature compressive stress-strain curves of Ti2AlNb lattice structure under different L-PBF forming process parameters in nitrogen-argon reaction atmosphere. DETAILED DESCRIPTION
[0029] The following will clearly and completely describe the technical solutions in the embodiments of the present invention in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of the present invention.
[0030] In order to meet the lightweight and high-performance design requirements of key structural parts in fields such as aerospace, the present invention designs and prepares a Ti2AlNb three-periodic minimal surface lattice structure that is additively formed in a nitrogen atmosphere. First, a Ti2AlNb lattice structure with a TPMS configuration is designed using implicit function modeling; then, in a nitrogen-argon reaction atmosphere, a Ti2AlNb lattice structure with a TPMS configuration is formed by L-PBF, thereby solving the problems of uneven reinforcement distribution and limited solid solution strengthening effect in traditional particle reinforcement, which is conducive to achieving a good match between the strength, plasticity and toughness of the lattice structure, and providing a new idea for the lightweight and high-performance design of aerospace structural parts. For details, please refer to Figure 1-4 , details the embodiments of the present invention.
[0031] Example 1:
[0032] The Ti2AlNb powder used for L-PBF forming in this embodiment is prepared by a plasma rotating electrode method, and its chemical composition is: AI (22-25 at.%), Nb (20-30 at.%), Ta (0-7 at.%), and the remainder is Ti. The powder particle size used for printing is 15-53 μm.
[0033] This embodiment involves a high-performance Ti2AlNb three-periodic minimal surface structure formed by additive manufacturing in a nitrogen atmosphere. The printing process diagram is shown in FIG. Figure 1 The specific process is as follows:
[0034] Step 1): Implicit function modeling of TPMS configuration.
[0035] In this embodiment, a typical sheet-like Gyroid lattice structure is selected as the research object, and implicit function modeling is performed using nTopology commercial software to obtain a CAD model of the lattice structure, as shown in FIG. Figure 2 The model used for L-PBF forming is exported as an STL model file. The Gyroid surface can be described by the following expression:
[0036] φ G (x,y,z)=cos(X)·sin(Y)+cos(Y)·sin(Z)+cos(Z)·sin(X)-C (1)
[0038] Where X = 2πx / l, Y = 2πy / l, and Z = 2πz / l, with l being the unit length in the x, y, and z directions. The CAD model parameters for the aforementioned sheet-like Gyroid lattice structure include a unit cell size of 5 mm × 5 mm × 5 mm, with six unit cells along each of the x, y, and z axes, and a volume fraction (VF = volume of the lattice structure divided by the volume of the corresponding block) of approximately 30%.
[0039] Step 2): Pre-treatment of L-PBF-formed Ti2AlNb lattice structure.
[0040] First, the STL model file of the lattice structure obtained above was imported into Materialise Magics software for layered slicing. The cubic lattice structure had a side length of 30 mm, and the slice layer thickness was 0.03 mm, for a total of 1000 layers. The processed SCAN file was then imported into a laser powder bed fusion machine (FF-M140C). A titanium alloy substrate was placed in the build chamber, and the position of the substrate was adjusted to ensure a uniform and complete layer of powder covering the upper surface. Finally, a mixture of nitrogen and argon was used to dilute and exhaust oxygen from the build chamber and piping until the oxygen content in the chamber was below 200 ppm.
[0041] The Ti2AlNb powder used was dried in a vacuum oven (80-100°C for 2 hours). The slice layer thickness of the lattice structure was 0.03mm. The nitrogen ratio during printing was controlled at 3 vol.% (nitrogen:argon = 3:97).
[0042] Step 3): Formation of L-PBF with Ti2AlNb lattice structure.
[0043] By adjusting the laser input energy density, mainly including laser power and scanning speed, the L-PBF forming of the lattice structure is achieved. After the printing is completed, wait for the substrate temperature to cool to room temperature, and cut the Ti2AlNb lattice structure from the substrate by wire electrospark cutting, ultrasonically clean it and dry it for later use. Figure 2 b shows the macroscopic morphology of the Ti2AlNb lattice structure formed by L-PBF.
[0044] In this example, the laser power was 150 W, the scanning speed was 800 mm / s, the scanning pitch was fixed at 0.1 mm, and the powder layer thickness was 0.03 mm. The laser scanning strategy was a checkerboard scan, with the scanning direction rotated 67° between adjacent layers. The titanium alloy substrate was preheated to 90°.
[0045] Step 4): Surface treatment of the TPMS-configured Ti2AlNb lattice structure.
[0046] The Ti2AlNb lattice structure of the TPMS formed by L-PBF is sandblasted or electropolished to remove unmelted powder particles adhering to the surface of the lattice structure during the forming process.
[0047] The elastic modulus and yield strength of the Gyroid lattice structure prepared under the L-PBF process parameters in this embodiment are 5138.6±53.2MPa and 155.6±0.9MPa, respectively. Figure 4 As shown in a.
[0048] Example 2:
[0049] The Ti2AlNb powder used for L-PBF forming in this embodiment is prepared by the plasma rotating electrode method, and its chemical composition is: AI (22-25 at.%), Nb (20-30 at.%), Ta (0-7 at.%), and the balance is Ti. The powder particle size used for printing is 15-53 μm.
[0050] This embodiment involves a high-performance Ti2AlNb three-periodic minimal surface structure formed by additive manufacturing in a nitrogen atmosphere. The printing process diagram is shown in FIG. Figure 1 The specific process is as follows:
[0051] Step 1): Implicit function modeling of TPMS configuration.
[0052] In this embodiment, a typical sheet-like Gyroid lattice structure is selected as the research object, and implicit function modeling is performed using nTopology commercial software to obtain a CAD model of the lattice structure, as shown in FIG. Figure 2 The model used for L-PBF forming is exported as an STL model file. The Gyroid surface can be described by the following expression:
[0053] φ G (x,y,z)=cos(X)·sin(Y)+cos(Y)·sin(Z)+cos(Z)·sin(X) - C (1)
[0054] Where X = 2πx / l, Y = 2πy / l, and Z = 2πz / l, with l being the unit length in the x, y, and z directions. The CAD model parameters for the aforementioned sheet-like Gyroid lattice structure include a unit cell size of 5 mm × 5 mm × 5 mm, with six unit cells along each of the x, y, and z axes, and a volume fraction (VF = volume of the lattice structure divided by the volume of the corresponding block) of approximately 30%.
[0055] Step 2): Pre-treatment of L-PBF-formed Ti2AlNb lattice structure.
[0056] First, the STL model file of the lattice structure obtained above was imported into the Materialise Magics software for layered slicing. The side length of the cubic lattice structure was 30 mm, and the slice layer thickness was 0.03 mm, for a total of 1000 layers. Then, the processed SCAN file was imported into the laser powder bed fusion equipment (FF-M140C). Secondly, the titanium alloy substrate was placed in the forming chamber, and the position of the substrate was adjusted to ensure that a uniform and complete layer of powder was covered on the upper surface of the substrate. Finally, a mixture of nitrogen and argon was used to dilute and exhaust the oxygen in the forming cavity and pipeline until the oxygen content in the cavity was less than 200 ppm.
[0057] The Ti2AlNb powder used was dried in a vacuum oven (80-100°C for 2 hours). The slice layer thickness of the lattice structure was 0.03mm. The nitrogen ratio during printing was controlled at 3 vol.% (nitrogen:argon = 3:97).
[0058] Step 3): Formation of L-PBF with Ti2AlNb lattice structure.
[0059] By adjusting the laser input energy density, mainly including laser power and scanning speed, the L-PBF forming of the lattice structure is achieved. After the printing is completed, wait for the substrate temperature to cool to room temperature, and cut the Ti2AlNb lattice structure from the substrate by wire electrospark cutting, ultrasonically clean it and dry it for later use. Figure 2 b shows the macroscopic morphology of the Ti2AlNb lattice structure formed by L-PBF.
[0060] In this embodiment, the laser power was 150W, the scanning speed was 1000 mm / s, the scanning pitch was fixed at 0.1 mm, and the powder layer thickness was 0.03 mm. The laser scanning strategy was a checkerboard scanning pattern, with the scanning direction rotated 67° between adjacent layers. The titanium alloy substrate was preheated to 90°C.
[0061] Step 4): Surface treatment of the TPMS-configured Ti2AlNb lattice structure.
[0062] The Ti2AlNb lattice structure of the TPMS formed by L-PBF is sandblasted or electropolished to remove unmelted powder particles adhering to the surface of the lattice structure during the forming process.
[0063] The elastic modulus and yield strength of the Gyroid lattice structure prepared under the L-PBF process parameters in this embodiment are 4961.6±82.0MPa and 151.5±4.0MPa, respectively. Figure 4 As shown in b.
[0064] Example 3:
[0065] The Ti2AlNb powder used for L-PBF forming in this embodiment is prepared by the plasma rotating electrode method, and its chemical composition is: AI (22-25 at.%), Nb (20-30 at.%), Ta (0-7 at.%), and the balance is Ti. The powder particle size used for printing is 15-53 μm.
[0066] This embodiment involves a high-performance Ti2AlNb three-periodic minimal surface structure formed by additive manufacturing in a nitrogen atmosphere. The printing process diagram is shown in FIG. Figure 1 The specific process is as follows:
[0067] Step 1): Implicit function modeling of TPMS configuration.
[0068] In this embodiment, a typical sheet-like Gyroid lattice structure is selected as the research object, and implicit function modeling is performed using nTopology commercial software to obtain a CAD model of the lattice structure, as shown in FIG. Figure 2 The model used for L-PBF forming is exported as an STL model file. The Gyroid surface can be described by the following expression:
[0069] φ G (x,y,z)= cos(X)·sin(Y)+ cos(Y)·sin(Z)+cos(Z)·sin(X)-C (1)
[0070] Where X = 2πx / l, Y = 2πy / l, and Z = 2πz / l, with l being the unit length in the x, y, and z directions. The CAD model parameters for the aforementioned sheet-like Gyroid lattice structure include a unit cell size of 5 mm × 5 mm × 5 mm, with six unit cells along each of the x, y, and z axes, and a volume fraction (VF = volume of the lattice structure divided by the volume of the corresponding block) of approximately 30%.
[0071] Step 2): Pre-treatment of L-PBF-formed Ti2AlNb lattice structure.
[0072] First, the STL model file of the lattice structure obtained above was imported into the Materialise Magics software for layered slicing. The side length of the cubic lattice structure was 30 mm, and the slice layer thickness was 0.03 mm, for a total of 1000 layers. Then, the processed SCAN file was imported into the laser powder bed fusion equipment (FF-M140C). Secondly, the titanium alloy substrate was placed in the forming chamber, and the position of the substrate was adjusted to ensure that a uniform and complete layer of powder was covered on the upper surface of the substrate. Finally, a mixture of nitrogen and argon was used to dilute and exhaust the oxygen in the forming cavity and pipeline until the oxygen content in the cavity was less than 200 ppm.
[0073] The Ti2AlNb powder used was dried in a vacuum oven (80-100°C for 2 hours). The slice layer thickness of the lattice structure was 0.03mm. The nitrogen ratio during printing was controlled at 3 vol.% (nitrogen:argon = 3:97).
[0074] Step 3): Formation of L-PBF with Ti2AlNb lattice structure.
[0075] By adjusting the laser input energy density, mainly including laser power and scanning speed, the L-PBF forming of the lattice structure is achieved. After the printing is completed, wait for the substrate temperature to cool to room temperature, and cut the Ti2AlNb lattice structure from the substrate by wire electrospark cutting, ultrasonically clean it and dry it for later use. Figure 2 b shows the macroscopic morphology of the Ti2AlNb lattice structure formed by L-PBF.
[0076] In this example, the laser power was 175 W, the scanning speed was 1200 mm / s, the scanning pitch was fixed at 0.1 mm, and the powder layer thickness was 0.03 mm. The laser scanning strategy was a checkerboard scan, with the scanning direction rotated 67° between adjacent layers. The titanium alloy substrate was preheated to 90°.
[0077] Step 4): Surface treatment of the TPMS-configured Ti2AlNb lattice structure.
[0078] The Ti2AlNb lattice structure of the TPMS formed by L-PBF is sandblasted or electropolished to remove unmelted powder particles adhering to the surface of the lattice structure during the forming process.
[0079] The elastic modulus and yield strength of the Gyroid lattice structure prepared under the L-PBF process parameters in this embodiment are 5122.7±25.9MPa and 159.4±4.1MPa, respectively. Figure 4 As shown in c.
[0080] Example 4:
[0081] The Ti2AlNb powder used for L-PBF forming in this embodiment is prepared by the plasma rotating electrode method, and its chemical composition is: AI (22-25 at.%), Nb (20-30 at.%), Ta (0-7 at.%), and the balance is Ti. The powder particle size used for printing is 15-53 μm.
[0082] This embodiment involves a high-performance Ti2AlNb three-periodic minimal surface structure formed by additive manufacturing in a nitrogen atmosphere. The printing process diagram is shown in FIG. Figure 1 The specific process is as follows:
[0083] Step 1: Implicit function modeling of TPMS configuration.
[0084] In this embodiment, a typical sheet-like Gyroid lattice structure is selected as the research object, and implicit function modeling is performed using nTopology commercial software to obtain a CAD model of the lattice structure, as shown in FIG. Figure 2 The model used for L-PBF forming is exported as an STL model file. The Gyroid surface can be described by the following expression:
[0085] φ G (x,y,z)=cos(X)·sin(Y)+cos(Y)·sin(Z)+cos(Z)·sin(X) - C (1)
[0086] Where X = 2πx / l, Y = 2πy / l, and Z = 2πz / l, with l being the unit length in the x, y, and z directions. The CAD model parameters for the aforementioned sheet-like Gyroid lattice structure include a unit cell size of 5 mm × 5 mm × 5 mm, with six unit cells along each of the x, y, and z axes, and a volume fraction (VF = volume of the lattice structure divided by the volume of the corresponding block) of approximately 30%.
[0087] Step 2): Pre-treatment of L-PBF-formed Ti2AlNb lattice structure.
[0088] First, the STL model file of the lattice structure obtained above was imported into the Materialise Magics software for layered slicing. The side length of the cubic lattice structure was 30 mm, and the slice layer thickness was 0.03 mm, for a total of 1000 layers. Then, the processed SCAN file was imported into the laser powder bed fusion equipment (FF-M140C). Secondly, the titanium alloy substrate was placed in the forming chamber, and the position of the substrate was adjusted to ensure that a uniform and complete layer of powder was covered on the upper surface of the substrate. Finally, a mixture of nitrogen and argon was used to dilute and exhaust the oxygen in the forming cavity and pipeline until the oxygen content in the cavity was less than 200 ppm.
[0089] The Ti2AlNb powder used was dried in a vacuum oven (80-100°C for 2 hours). The slice layer thickness of the lattice structure was 0.03mm. The nitrogen ratio during printing was controlled at 3 vol.% (nitrogen:argon = 3:97).
[0090] Step 3): Formation of L-PBF with Ti2AlNb lattice structure.
[0091] By adjusting the laser input energy density, mainly including laser power and scanning speed, the L-PBF forming of the lattice structure is achieved. After the printing is completed, wait for the substrate temperature to cool to room temperature, and cut the Ti2AlNb lattice structure from the substrate by wire electrospark cutting, ultrasonically clean it and dry it for later use. Figure 2 b shows the macroscopic morphology of the Ti2AlNb lattice structure formed by L-PBF.
[0092] In this example, the laser power was 250 W, the scanning speed was 1200 mm / s, the scanning pitch was fixed at 0.1 mm, and the powder layer thickness was 0.03 mm. The laser scanning strategy was a checkerboard scan, with the scanning direction rotated 67° between adjacent layers. The titanium alloy substrate was preheated to 90°.
[0093] Step 4): Surface treatment of the TPMS-configured Ti2AlNb lattice structure.
[0094] The Ti2AlNb lattice structure of the TPMS formed by L-PBF is sandblasted or electropolished to remove unmelted powder particles adhering to the surface of the lattice structure during the forming process.
[0095] The elastic modulus and yield strength of the Gyroid lattice structure prepared under the L-PBF process parameters in this embodiment are 5419.1±79.5MPa and 174.4±2.0MPa, respectively. Figure 4 As shown in d.
[0096] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the invention can be embodied in other specific forms without departing from the spirit or essential characteristics of the invention. Therefore, the embodiments should be considered in all respects as illustrative and non-restrictive, and the scope of the invention is defined by the appended claims, not the foregoing description, and all variations within the meaning and range of equivalents of the claims are intended to be included therein. Any reference sign in a claim should not be construed as limiting the claim to which it relates.
[0097] In addition, it should be understood that although this specification is described in terms of implementation methods, not every implementation method contains only one independent technical solution. This narrative method of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment can also be appropriately combined to form other implementation methods that can be understood by those skilled in the art.
Claims
1. A method for additively forming a high-performance Ti2AlNb three-periodic minimal surface lattice structure in a nitrogen atmosphere, characterized by: The following steps are involved: Step 1) Implicit function modeling of the TPMS configuration: Design a CAD model of the TPMS configuration and export it as an STL file; Step 2) Pre-processing of L-PBF Ti2AlNb lattice structure: Slice the STL file and set the process parameters; Step 3) L-PBF forming of a Ti2AlNb lattice structure: forming a Ti2AlNb lattice structure by L-PBF technology in a nitrogen-argon mixed atmosphere; Step 4) Surface treatment is performed on the TPMS configuration Ti2AlNb lattice structure.
2. The method for additively forming a high-performance Ti2AlNb three-periodic minimal surface lattice structure in a nitrogen atmosphere according to claim 1, characterized in that: In the above step 1), the TPMS configuration is selected from one of Gyroid, Diamond or Primitive, and implicit function modeling is performed using nTopology software to obtain a CAD model of the lattice structure. The model for L-PBF forming is exported as an STL model file.
3. The method for additively forming a high-performance Ti2AlNb three-periodic minimal surface lattice structure under a nitrogen atmosphere according to claim 2, characterized in that: The volume fraction of the lattice structure is 7.5%-50%.
4. The method for additively forming a high-performance Ti2AlNb three-periodic minimal surface lattice structure in a nitrogen atmosphere according to claim 3, characterized in that: In step 2) above, first, the STL model file of the lattice structure obtained in step 1) is imported into Materialise Magics software for layered slicing. Then, the processed SCAN file is imported into a laser powder bed fusion device. Secondly, a titanium alloy substrate is placed in a forming chamber of the laser powder bed fusion device, and the position of the substrate is adjusted so that the upper surface of the substrate is covered with a uniform and complete layer of Ti2AlNb powder. Finally, a mixture of nitrogen and argon is used to dilute and exhaust the oxygen in the forming cavity and pipeline, so that the oxygen content in the forming cavity is less than 200 ppm.
5. The method for additively forming a high-performance Ti2AlNb three-periodic minimal surface lattice structure in a nitrogen atmosphere according to claim 4, characterized in that: The Ti2AlNb powder used above is dried at a temperature of 80-100°C for 2 hours. The thickness of the slice layer of the lattice structure is 0.03 mm, and the proportion of nitrogen during the printing process is controlled to be 1-10vol.%.
6. The method for additively forming a high-performance Ti2AlNb three-periodic minimal surface lattice structure in a nitrogen atmosphere according to claim 5, characterized in that: In the above step 3), the L-PBF forming of the lattice structure is achieved by adjusting the laser input energy density; after the substrate temperature is cooled to room temperature, the Ti2AlNb lattice structure is cut from the substrate, ultrasonically cleaned and dried for later use; The L-PBF process parameters include: laser power of 150-250W, scanning speed of 800-1400mm / s, scanning spacing of 0.05-0.15mm, and layer thickness of 0.02-0.05mm; the laser scanning strategy is checkerboard scanning, and the scanning direction between adjacent layers is rotated 67°; the preheat temperature of the titanium alloy substrate is 90°.
7. The method for additively forming a high-performance Ti2AlNb three-periodic minimal surface lattice structure in a nitrogen atmosphere according to claim 6, characterized in that: In the above step 4), the surface treatment includes sandblasting or electrolytic polishing.
8. The method for additively forming a high-performance Ti2AlNb three-periodic minimal surface lattice structure under a nitrogen atmosphere according to claim 7, characterized in that: The chemical composition of the Ti2AINb powder is: Al: 22-25 at.%, Nb: 20-30 at.%, Ta: 0-7 at.%, and the balance is Ti.
Citation Information
Patent Citations
Powder additive manufacturing method for nitrogen atom interstitial solution strengthening Ti2AlNb alloy
CN118854104A
Cited By
A lightweight method for 3D printing aluminum-lithium alloy supports for aerospace applications
CN122400593A
Astronautical aluminum-lithium alloy brace 3D printing light weight method
CN122400593B