Method for manufacturing foam glass by recovering glass fibers from waste fan blades

Through the pyrolysis and preparation process, the waste fan blades are converted into foam glass, which solves the environmental pollution and resource utilization problems in the treatment of retired fan blades, and realizes the high-value utilization of glass fibers and the preparation of foam glass with excellent performance.

CN120553989APending Publication Date: 2025-08-29HUANENG WUHAN POWER GENERATION CO LTD +2
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202510640549.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-19
Publication Date
2025-08-29

AI Technical Summary

Technical Problem

In the prior art, the treatment of retired fan blades is mainly through incineration and landfill, which leads to environmental pollution and insufficient utilization of composite materials, and lacks high-value utilization methods.

Method used

By pyrolyzing the waste fan blades in an inert atmosphere, regenerated glass fibers are obtained, mixed with a foaming agent, a foam stabilizer and a binding agent and pressed into molding. Foaming glass is prepared after sintering, foaming and annealing.

Benefits of technology

Resource reuse of glass fibers is realized, production costs are reduced, and foam glass with excellent performance can be prepared, which can be used in thermal insulation materials in construction and industrial fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120553989A_ABST
    Figure CN120553989A_ABST
Patent Text Reader

Abstract

The embodiment of the invention provides a method for manufacturing foam glass by recovering glass fibers from waste fan blades. The method comprises the following steps: pyrolyzing the waste fan blades in an inert atmosphere; calcining the pyrolysis product of the waste fan blade in an oxygen-containing atmosphere to obtain regenerated glass fiber; carrying out grinding treatment on the obtained regenerated glass fiber; mixing the ground regenerated glass fiber powder with a foaming agent, a foam stabilizer and a binding agent, and performing compression molding to obtain a prefabricated blank; and sintering, foaming and annealing the prefabricated blank in sequence to obtain the foamed glass. The recycling of the fan blade reduces the waste of a landfill, realizes the recycling of the glass fiber, reduces the demand on raw materials, creates a new economic growth point by using the waste glass fiber for developing the foam glass market, and realizes the high-valued utilization of the recycled glass fiber.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The embodiments of the present disclosure belong to the technical field of solid waste resource utilization and high value creation, and specifically relate to a method for recycling glass fibers from discarded wind turbine blades to manufacture foam glass. Background Art

[0002] With the booming development of the wind power industry, the scale of retired wind turbines will continue to grow. How to effectively utilize retired blades on a large scale while ensuring environmental protection is key to achieving green and sustainable development for wind power companies.

[0003] In the past, the average annual blade processing volume in China was between 1,000 and 2,000 tons. Most retired wind turbine blades were disposed of mainly through incineration and landfill. The comprehensive utilization of composite materials was still in the engineering test stage and had a certain impact on the environment.

[0004] Wind turbine blades are the core components of wind turbines. Their outer shells are primarily composed of a composite material made from glass fiber and thermosetting resin. Recycling glass fiber from retired wind turbine blades through pyrolysis is gaining increasing attention, as it can be used as a resource and energy source. This invention recycles discarded wind turbine blades by extracting the glass fiber from them to produce foamed glass, providing a new avenue for further high-value utilization of recycled glass fiber. Summary of the Invention

[0005] The embodiments of the present disclosure aim to solve at least one of the technical problems existing in the prior art and provide a method for recycling glass fibers from discarded wind turbine blades to manufacture foam glass.

[0006] One aspect of an embodiment of the present disclosure provides a method for recycling glass fibers from waste fan blades to manufacture foam glass, comprising: pyrolyzing the waste fan blades in an inert atmosphere;

[0007] calcining the pyrolysis products of discarded fan blades in an oxygen-containing atmosphere to obtain regenerated glass fibers;

[0008] Grinding the obtained regenerated glass fiber;

[0009] The recycled glass fiber powder obtained after grinding is mixed with a foaming agent, a foam stabilizer and a binder and then pressed into shape to obtain a preform;

[0010] The prefabricated body is subjected to sintering, foaming and annealing treatments in sequence to obtain foamed glass.

[0011] Optionally, the waste fan blades are subjected to pyrolysis treatment at a temperature range of 500-600° C. for 20-40 minutes.

[0012] Optionally, the pyrolysis product of the waste fan blades is calcined at 500-600° C. for 20-40 minutes.

[0013] Optionally, the regenerated glass fiber material is ground into powder with a particle size of 0.07-0.1 mm using a ball mill, and then sieved.

[0014] Optionally, the components of the foaming agent include coke and coal powder, or limestone and soda ash; the components of the foam stabilizer include sodium pyrophosphate and sodium sulfate; and the binder includes industrial water glass or polyvinyl alcohol.

[0015] Optionally, before sintering the preform, the process further includes placing the preform in a high-temperature furnace and preheating the preform within a temperature range of 100° C. to 200° C. for 30 to 60 minutes.

[0016] Optionally, the preform is placed in a high-temperature furnace and sintered at a temperature range of 600-1000° C. at a heating rate of 5-10° C. / min for 1-3 hours.

[0017] Optionally, the block green body obtained after sintering is subjected to normal pressure foaming treatment at 700-900° C., and the foaming time lasts for 30-40 minutes.

[0018] Optionally, the foamed glass obtained by the foaming treatment is annealed within a temperature range of 500 to 700° C. and kept warm for 3 to 5 hours.

[0019] Optionally, after the annealing treatment, the method further comprises: subjecting the obtained foam glass to a standing cooling treatment for 8-24 hours.

[0020] The beneficial effects of the embodiments of the present disclosure include:

[0021] 1. Resource utilization and high value creation of solid waste: The recycling of wind turbine blades reduces waste in landfills, realizes the recycling and reuse of glass fiber, and reduces the demand for raw materials. At the same time, the use of waste glass fiber in the development of the foam glass market creates a new economic growth point and realizes the high value utilization of recycled glass fiber.

[0022] 2. Reduce costs: The present invention extracts and reuses glass fibers from discarded fan blades and uses them to make foam glass. Recycled materials are cheaper than new materials, which helps reduce production costs.

[0023] 3. Excellent performance: The foam glass made of glass fiber in the present invention has good strength and lightness, meets the standards, has excellent performance, and can be used as a thermal insulation material in construction and industrial fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 TG and DTA curves of coke and coal powder used as foaming agents in the embodiment of the present invention;

[0025] Figure 2 TG and DTA curves of limestone and soda ash as foaming agents in the embodiment of the present invention;

[0026] Figure 3 is a graph showing the relationship between the amount of foam stabilizer used and the volume density of glass foam in an embodiment of the present invention;

[0027] Figure 4 The present invention is a flow chart of a method for recycling glass fibers from discarded wind turbine blades to manufacture foam glass according to an embodiment of the present invention. DETAILED DESCRIPTION

[0028] In order to enable those skilled in the art to better understand the technical solutions of the present disclosure, the present disclosure is further described in detail below with reference to the accompanying drawings and specific implementation methods.

[0029] The following is a further detailed description of the embodiments of the present application in conjunction with the accompanying drawings and examples. The detailed descriptions and drawings of the following examples are used to illustrate the principles of the present application, but are not used to limit the scope of the present application, that is, the present application is not limited to the described embodiments. In the description of the present application, it should be noted that, unless otherwise specified, the meaning of "multiple" is more than two; the orientation or positional relationship indicated by the terms "upper", "lower", "left", "right", "inside", "outside", etc. is only for the convenience of describing the present application and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application. In addition, the terms "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying relative importance. "Vertical" is not perpendicular in the strict sense, but is within the allowable error range. "Parallel" is not parallel in the strict sense, but is within the allowable error range.

[0030] It should also be noted that, in the description of this application, unless otherwise specified or limited, the terms "installed," "connected," and "connected" should be understood broadly. For example, they can refer to fixed connections, detachable connections, or integral connections; they can refer to direct connections or indirect connections through an intermediary. Those skilled in the art will understand the specific meanings of these terms in this application based on the specific circumstances.

[0031] like Figure 4 As shown, a method for recycling glass fibers from discarded wind turbine blades to produce foam glass comprises:

[0032] S101, pyrolyzing the discarded fan blades in an inert atmosphere;

[0033] S102, calcining the pyrolysis product of the discarded fan blades in an oxygen-containing atmosphere to obtain regenerated glass fiber;

[0034] S103, grinding the obtained regenerated glass fiber;

[0035] S104, mixing the ground recycled glass fiber powder with a foaming agent, a foam stabilizer, and a binder, and then pressing and molding the mixture to obtain a preform;

[0036] S105 , sequentially sintering, foaming, and annealing the prefabricated body to obtain foamed glass.

[0037] In some embodiments, the waste wind turbine blades are pyrolyzed at a temperature in the range of 500-600° C. for 20-40 minutes.

[0038] In some embodiments, the pyrolysis product of waste wind turbine blades is calcined at 500-600° C. for 20-40 minutes.

[0039] In some embodiments, the regenerated glass fiber material is ground into powder with a particle size of 0.07-0.1 mm using a ball mill, and then sieved.

[0040] In some embodiments, the foaming agent comprises coke and soda ash, or limestone and soda ash, the foam stabilizer comprises sodium pyrophosphate and sodium sulfate, and the binder comprises industrial water glass or polyvinyl alcohol.

[0041] In one embodiment, the glass fiber powder is added in an amount of 30-50%, the coke and coal powder used as foaming agents are added in amounts of 1.5% and 2.5% respectively. The foam stabilizer is preferably added in an amount of 2%-3%. The binder is added in an amount of 5%-15%, and a mineral filler (such as quartz sand or talc) is added in an amount of 20-40%. The mold is then pressed into shape.

[0042] In some embodiments, before sintering the preform, the process further includes placing the preform in a high-temperature furnace and preheating the preform in a temperature range of 100° C. to 200° C. for 30 to 60 minutes.

[0043] In some embodiments, the preform is placed in a high-temperature furnace and sintered at a temperature range of 600-1000° C. at a heating rate of 5-10° C. / min for 1-3 hours.

[0044] In some embodiments, the block green body obtained after sintering is subjected to normal pressure foaming treatment at 700-900° C., and the foaming time lasts for 30-40 minutes.

[0045] In some embodiments, the foamed glass obtained by the foaming treatment is annealed at a temperature ranging from 500 to 700° C. and kept at this temperature for 3 to 5 hours.

[0046] In some embodiments, after the annealing treatment, the process further includes: subjecting the obtained foam glass to a static cooling treatment for 8-24 hours.

[0047] In some embodiments, the foam glass is demolded after the cooling treatment, and the product is quality tested to ensure that its performance meets the requirements.

[0048] The beneficial effects of the present invention include: 1. Resource utilization and high value creation of solid waste: The recycling of wind turbine blades reduces waste in landfills, realizes the recycling and reuse of glass fiber, reduces the demand for raw materials, and at the same time, uses waste glass fiber to develop the foam glass market, creates a new economic growth point, and realizes the high value utilization of recycled glass fiber.

[0049] 2. Reduce costs: The present invention extracts and reuses glass fibers from discarded fan blades and uses them to make foam glass. Recycled materials are cheaper than new materials, which helps reduce production costs.

[0050] 3. Excellent performance: The foam glass made of glass fiber in the present invention has good strength and lightness, meets the standards, has excellent performance, and can be used as a thermal insulation material in construction and industrial fields.

[0051] Specific methods and steps include:

[0052] (1) The retired fan blades were pyrolyzed in an inert atmosphere at a temperature of 550°C for 30 minutes, and then calcined in an oxygen-containing atmosphere at a temperature of 550°C for 30 minutes to obtain regenerated glass fibers.

[0053] (2) The regenerated glass fiber material obtained in (1) was ground into a powder with a particle size of 0.08 mm using a ball mill and sieved using a square hole sieve.

[0054] (3) The glass fiber powder (accounting for 40%) in (2) is mixed with a foaming agent (selected as coke and coal powder (1.5% and 2.5%), or limestone (2%) and soda ash (2%)), a foam stabilizer (selected as sodium pyrophosphate and sodium sulfate (2% each)), a binder (industrial water glass (10%) or polyvinyl alcohol (10%)) and quartz sand (40%), and then placed in a mold for pressing to obtain a prefabricated body.

[0055] (4) Place (3) in a high temperature furnace and maintain the temperature in the range of 150 degrees Celsius with residual heat, and the preheating time is 40 minutes.

[0056] (5) Use a high-temperature furnace (such as a tunnel furnace or a vertical furnace) to provide a uniform high-temperature environment. The sintering temperature range is 800°C. The temperature is increased at 10°C / min (to avoid cracking of the material due to excessive temperature increase) and sintering for 2 hours.

[0057] (6) After step (5), foaming is carried out in a foaming machine at a foaming temperature of 850° C. and a foaming time of 40 minutes under normal pressure.

[0058] (7) After step (6), annealing is performed. The annealing process is maintained at 650° C. (depending on the properties of the required foam glass) and kept warm for 3 hours.

[0059] (8) The obtained foam glass product is allowed to cool for 16 hours. The product is demoulded and quality tested to ensure that its performance meets the requirements.

[0060] Example 1

[0061] Retired fan blades were cut into blocks and placed in a tubular furnace for pyrolysis at 550°C for 30 minutes in a nitrogen atmosphere. The blocks were then calcined at 550°C for 30 minutes in an air atmosphere to remove the residual carbon, yielding apparently white, pure glass fibers.

[0062] The obtained glass fiber is ground into powder, and the glass fiber powder (45%), binder (10% industrial water glass), foaming agent (3% each of coke and coal powder), foam stabilizer (2% each of sodium pyrophosphate and sodium sulfate), and quartz sand (35%) are mixed in proportion and placed into a mold for pressing. Place it in a high-temperature furnace and preheat it at 200℃ for 40 minutes. Raise the temperature at 10℃ / min to maintain the temperature at 800℃ and sinter for 2 hours. After cooling, place it in a foaming machine for foaming treatment, maintain it at 850℃ under normal pressure for 45 minutes. Finally, anneal it and maintain it at 600℃ for 4 hours.

[0063] The obtained foam glass was cooled statically for 16 hours, demoulded, and subjected to quality inspection.

[0064] Example 2

[0065] The method of Example 1 was followed, except that limestone (accounting for 2%) and soda ash (accounting for 2%) were used as foaming agents in step (2).

[0066] Test Example 1

[0067] See Figure 1 , Figure 1 For the coke used in the embodiment of the present invention ( Figure 1 middle curves 1 and 1′) and pulverized coal ( Figure 1The TG and DTA (thermogravimetric analysis-differential thermal analysis, mainly used to study the thermal stability and composition of materials) curves of the mixture with pulverized coal as the foaming agent show that in the temperature range of 500-650°C, the DTA curve 1′ has an obvious exothermic peak, which is the result of the oxidation of fixed carbon in the coke, and its peak temperature is 591°C. Along with this exothermic effect, the batch material has an obvious weight loss process on the TG curve 1, and its weight loss rate is 1.94%. The weight loss before 120°C is mainly due to the removal of residual water, and the weight loss thereafter is caused by the decomposition and oxidation of the binder and foam stabilizer in the batch material. The TG and DTA curves of the batch material with pulverized coal as the foaming agent ( Figure 1 The shape of the middle curves (2 and 2') is similar to that of coke batch, except that the temperature range of oxidation exotherm and weight loss is wider than that of coke. The exothermic peak temperature on DTA curve 2' is 581°C, and the weight loss rate in the temperature range of 500-650°C is 1.67%.

[0068] Test Example 2

[0069] from Figure 2 It can be seen that Figure 2 For the limestone batch material used in the embodiment of the present invention ( Figure 2 Curves 1 and 1′) and soda ash ( Figure 2 Curves 2 and 2') are used as TG, DTA (thermogravimetric analysis-differential thermal analysis, mainly used to study the thermal stability and composition of materials) curves of the foaming agent. Below 100°C, due to the removal of residual water, an obvious weight loss process appears on the TG curve. The temperature at which soda ash begins to decompose is low, and the decomposition temperature range is wide. The soda ash batch begins to lose weight significantly from 290°C, and basically ends at around 700°C. The weight loss rate in this temperature range is 0.86% (curve 2). The limestone batch has an obvious weight loss process in the temperature range of 690-770°C, and its weight loss rate is 0.75% (curve 1). Due to the effect of other components in the batch, the thermal decomposition temperature of the limestone is reduced, and basically all of it decomposes and releases gas within this temperature range. In addition, from Figure 2 DTA curve 1′ shows a distinct endothermic process within the temperature range corresponding to the thermal decomposition of limestone TG curve 1. However, after the temperature reaches the upper limit of this temperature range, the endothermic valley is incomplete due to instrument baseline drift (DTA curve 1′). Soda ash has a low decomposition temperature, a wide decomposition temperature range, and a relatively small dosage, resulting in a less pronounced thermal effect (DTA curve 2′). Furthermore, due to the complex physical and chemical changes of other ingredients in the batch during heating, DTA curve 2′ exhibits more complex changes within this temperature range.

[0070] from Figure 1 and Figure 2 We can learn that:

[0071] Under the influence of other ingredients in the batch, the foaming agent actually begins to decompose or oxidize even before the batch is sintered. As the temperature rises and the sintering process continues, the gas pressure within the tiny bubbles increases due to continued gas release from the foaming agent, rising temperature, and the restraining effect of the sintered body. When the temperature reaches the foaming temperature, the glass gradually softens, reducing the resistance to cell wall movement, causing the bubbles to expand and the gas pressure within the bubbles to gradually decrease until the pressure within the bubbles balances with the external pressure. At this point, the volume of the foamed glass is at its maximum and its bulk density is at its lowest. After foaming, during the annealing process, the temperature drops, causing the volume of the gas within the bubbles to gradually decrease, resulting in a slight decrease in the volume of the foamed glass and a slight increase in its bulk density. Theoretically, when the temperature drops to the glass strain point, the migration and adjustment of particles in the glass are essentially impossible, and the volume of the foamed glass remains stable. In practice, the volume and shape of foamed glass are essentially fixed when the temperature drops to the glass transition point or slightly above.

[0072] from Figure 3 It can be seen that:

[0073] The relationship between the volume density of the foamed glass and the amount of the foam stabilizer obtained by using two foam stabilizers, sodium pyrophosphate and sodium sulfate, and fixing the amount of one of them at 2% and changing the amount of the other is shown in Figure 3 ( Figure 3 Curve A is a fixed dosage of 2% sodium sulfate, and curve B is a fixed dosage of 2% sodium pyrophosphate). Figure 3 As can be seen above, using only one foam stabilizer results in a high bulk density of the foamed glass, resulting in poor results. When both foam stabilizers are used together, with sodium sulfate at a 2% dosage, the foamed glass achieves its lowest bulk density. When sodium pyrophosphate dosage is below 1.5%, the foamed glass bulk density decreases significantly. Further increases in dosage result in a continued decrease in the bulk density, but the rate of decline slows. Considering both foamed glass quality and cost, the optimal dosage of sodium pyrophosphate and sodium sulfate is 2% each.

[0074] It is understood that the above embodiments are merely exemplary embodiments for illustrating the principles of the present disclosure, and the present disclosure is not limited thereto. Those skilled in the art may make various modifications and improvements without departing from the spirit and substance of the present disclosure, and such modifications and improvements are also considered to be within the scope of protection of the present disclosure.

Claims

1. A method for producing foam glass by recycling glass fibers from discarded fan blades, characterized in that: include: The waste fan blades are pyrolyzed in an inert atmosphere; calcining the pyrolysis products of discarded fan blades in an oxygen-containing atmosphere to obtain regenerated glass fibers; Grinding the obtained regenerated glass fiber; The recycled glass fiber powder obtained after grinding is mixed with a foaming agent, a foam stabilizer and a binder, and then pressed into shape to obtain a preform; The prefabricated body is subjected to sintering, foaming and annealing treatments in sequence to obtain foamed glass.

2. The method for producing foam glass by recycling glass fibers from discarded fan blades according to claim 1, characterized in that: The waste fan blades are pyrolyzed at a temperature range of 500-600°C for 20-40 minutes.

3. The method for producing foam glass by recycling glass fibers from discarded fan blades according to claim 1, characterized in that: The pyrolysis products of the waste fan blades are calcined at 500-600° C. for 20-40 minutes.

4. The method for producing foam glass by recycling glass fibers from discarded fan blades according to claim 1, characterized in that: The regenerated glass fiber material is ground into powder with a particle size of 0.07-0.1 mm using a ball mill and sieved.

5. The method for producing foam glass by recycling glass fibers from discarded fan blades according to claim 1, characterized in that: The foaming agent comprises coke and coal powder, or limestone and soda ash; the foam stabilizer comprises sodium pyrophosphate and sodium sulfate; and the binder comprises industrial water glass or polyvinyl alcohol.

6. The method for producing foam glass by recycling glass fibers from discarded fan blades according to claim 1, characterized in that: Before sintering the preform, the process further includes placing the preform in a high-temperature furnace and preheating the preform within a temperature range of 100° C. to 200° C. for 30 to 60 minutes.

7. The method for producing foam glass by recycling glass fibers from discarded fan blades according to claim 1, characterized in that: The preform body is placed in a high-temperature furnace and sintered at a temperature range of 600-1000° C. at a heating rate of 5-10° C. / min for 1-3 hours.

8. The method for producing foam glass by recycling glass fibers from discarded fan blades according to claim 1, characterized in that: The block green body obtained after sintering is subjected to normal pressure foaming treatment at 700-900° C., and the foaming time lasts for 30-40 minutes.

9. The method for producing foam glass by recycling glass fibers from discarded fan blades according to claim 1, characterized in that: The foamed glass obtained by the foaming treatment is annealed in a temperature range of 500 to 700° C. and kept warm for 3 to 5 hours.

10. The method for producing foam glass by recycling glass fibers from discarded fan blades according to claim 1, characterized in that: After the annealing treatment, the method further includes: subjecting the obtained foam glass to a static cooling treatment for 8-24 hours.

Citation Information

Cited By

  • Design method of GFRP cloth reinforced wall based on recovered fan blade glass fibers