Detection method for measuring silver content in crude copper by atomic absorption spectrometry

Through atomic absorption spectrometry, crude copper samples were treated with nitric acid, bromine water and hydrochloric acid, and mixed acid dissolution of ammonium hydrogen fluoride and nitrosulfur sulfur mixed acid, a silver working curve matching was prepared for copper matrix, which solved the uniformity and accuracy of sample detection of silver content in crude copper, achieved rapid and accurate silver content determination, and reduced detection cost.

CN120558878APending Publication Date: 2025-08-29JIANGXI COPPER
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510701963.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-28
Publication Date
2025-08-29

AI Technical Summary

Technical Problem

In the prior art, in the detection of silver content in crude copper, there are problems such as poor sample uniformity, inaccurate detection results, long process and high cost. Especially when the content of elements such as antimony, bismuth, tellurium, etc. is high, it is difficult to achieve rapid and accurate silver content measurement.

Method used

Atomic absorption spectrometry was used to weigh a certain amount of crude copper sample, dissolve it with nitric acid and bromine water and then add hydrochloric acid to treat it, filter the undissolved particles, and dissolve it at high temperature using ammonium hydrogen fluoride and nitrosulfur mixed acid to prepare a silver working curve matching with copper matrix, and use atomic absorption spectrometer to determine the silver content, reduce the separation steps, and improve detection efficiency and accuracy.

Benefits of technology

It improves the accuracy and precision of the test results, shortens the inspection process, reduces costs, ensures the representativeness of silver content and the rapidity of detection, and reduces the occupational harm caused by the lead-fire test method.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120558878A_ABST
    Figure CN120558878A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of spectrum chemical analysis, and particularly relates to a detection method for measuring the silver content in crude copper through atomic absorption spectrometry. The method comprises the following specific steps: dissolving with nitric acid, adding bromine water and hydrochloric acid, steaming to be nearly dry, and leaching with hydrochloric acid; if particles which are not completely dissolved exist only by using nitric acid and hydrochloric acid, filtering, adding a saturated ammonium bifluoride solution, nitric acid-sulfuric acid mixed acid and perchloric acid, heating and dissolving, smoking until smoke is exhausted, adding hydrochloric acid for leaching, transferring into a volumetric flask (not separately taken), taking hydrochloric acid as a medium, matching a copper matrix with a silver standard solution, acetylene as fuel gas and air as combustion-supporting gas, and performing gradient elution to obtain the copper-silver alloy. And measuring the silver content on an atomic absorption spectrometer. The method has the characteristics of simplicity in sample pretreatment, high detection result accuracy, good precision, simplicity in operation, high practicability and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of spectral chemical analysis, and in particular relates to a detection method for determining the amount of silver in crude copper by atomic absorption spectroscopy. Technical Background

[0002] Blister copper is an intermediate material in the copper smelting process, with an annual market volume exceeding millions of tons. Blister copper typically contains several hundred grams of silver per ton, making it highly valuable. Test results often differ beyond acceptable tolerances, a major source of disputes in the copper trade.

[0003] Since silver segregates significantly during the smelting process of crude copper, the uniformity of the crude copper sample is poor. It is necessary to increase the sample weight to improve the representativeness of the sample and the accuracy of the test results.

[0004] Currently, the primary method for detecting silver in blister copper is lead fire assay, which uses lead chemical reagents and is a source of occupational health risks associated with lead. Lead fire assay methods are divided into dry and wet fire assays and direct fire assays. The wet and dry fire assay involves acid dissolution to precipitate silver, filtration to separate the copper matrix, carbonization of the filter residue, and determination of the silver content by lead fire assay. This process takes two days. The direct fire assay, on the other hand, involves weighing the blister copper sample and determining the silver content by lead fire assay. This process also takes a full day. For samples containing high levels of elements such as antimony, bismuth, and tellurium, silver content must be determined using atomic absorption spectrometry or inductively coupled plasma emission spectrometry (ICPES) to calculate the silver content using the impurity difference subtraction method. Consequently, these methods are costly, time-consuming, and prone to underestimating the test results.

[0005] Therefore, in order to ensure the representativeness of the sample, shorten the detection process, improve the detection efficiency, and ensure the accuracy of the test results, choosing an atomic absorption spectrometry method to determine the amount of silver in crude copper is a key factor. Summary of the Invention

[0006] The invention discloses a method for detecting the amount of silver in crude copper by atomic absorption spectrometry, so as to solve any of the above and other potential problems in the prior art.

[0007] In order to solve the above technical problems, the technical solution of the present invention is: a detection method for determining the amount of silver in crude copper by atomic absorption spectrometry, the detection method specifically comprising the following steps:

[0008] S1) Weigh a certain amount of crude copper to be measured and dissolve it in nitric acid, then add bromine water and concentrated hydrochloric acid to remove sulfur, and evaporate to near dryness;

[0009] S2) adding concentrated hydrochloric acid to the sample treated in S1) for leaching, transferring it into a volumetric flask and adding water to make up to volume to obtain a solution to be tested;

[0010] S3) starting the atomic absorption spectrometer and setting the measurement parameters;

[0011] S4) preparing a silver working curve matching the copper matrix and measuring the solution to be tested;

[0012] S5) obtaining the mass concentration of silver from the silver working curve, and calculating the silver content in the crude copper.

[0013] Furthermore, the detection method further comprises the following steps:

[0014] After the hydrochloric acid leaching in S2), the crude copper sample is not completely dissolved and there are a small amount of particles. It is filtered with quick filter paper, washed with filter paper, and the filtrate is collected back into the original beaker. The filter paper and filter residue are placed in another 500mL beaker, 2mL~5mL of saturated ammonium bifluoride are added, shaken, and then 10mL~15mL of nitric acid and sulfuric acid mixture and 2mL~5mL of perchloric acid are added. Heat at low temperature to dissolve, smoke, until the smoke is gone. If there are still undissolved particles, repeat the above operation until it is completely dissolved.

[0015] Furthermore, the ratio between the various acids in the nitric-sulfuric acid mixture is HNO3:H2SO4:H2O=3:1:3;

[0016] The low temperature is 180℃~260℃.

[0017] Furthermore, the crude copper measured in S1) is weighed by weighting the upper and lower sieves to a weight of not less than 5.0 grams.

[0018] Furthermore, the specific steps of S1) are:

[0019] S1.1) Pour a certain amount of nitric acid into the crude copper sample to be measured in a beaker. Place it on the work surface and observe the reaction. Once the reaction stops, heat it on a hot plate to a low temperature of 110°C to 200°C and continue to observe the reaction. After the reaction stops, remove it and let it cool slightly.

[0020] S1.2) Add 2 mL of bromine water and 5 mL to 10 mL of concentrated hydrochloric acid, shake well, and continue heating to dissolve. If the sulfur has not been completely removed, add more bromine water until the sulfur is completely removed. Wait until the test solution is dissolved and clear. Continue heating and steaming until nearly dry, then remove and cool slightly.

[0021] Further, the specific steps of S2) are:

[0022] S2.1) Add 10 mL of concentrated hydrochloric acid to the sample obtained in S1), shake well, and heat on a hot plate to a low temperature of 110°C to 200°C. Once the soluble salt is completely dissolved, pipette water along the sides of the cup to a volume of at least 30 mL. Shake well, and continue heating until the solution is slightly boiling. Remove the sample and allow it to cool.

[0023] S2.2) Pre-fill a volumetric flask selected based on the silver content of the sample with concentrated hydrochloric acid, controlling the concentration of the hydrochloric acid medium to match the standard solution. Add water to the volumetric flask to a minimum of 60 mL, shake well, and label the flask.

[0024] S2.3) After the test solution treated in S2.2) has cooled to room temperature, transfer the test solution to a volumetric flask according to the operating instructions. Add water to the volumetric flask to the required volume, shaking the flask continuously during the process to obtain the test solution.

[0025] Furthermore, the S3) is summarized as follows: using hydrochloric acid as the medium and acetylene as the fuel gas,

[0026] Air is the combustion-supporting gas, and the measurement parameters of each instrument are set as follows: lamp current 3 mA, slit 3 nm, observation height 7 mm, gas flow rate 0.9 L / min to 1.2 L / min, and bubble-supporting flow rate 8.0 L / min.

[0027] Further, the specific steps of S4) are:

[0028] S4.1) Pipette 0.00 mL, 0.50 mL, 1.00 mL, 1.50 mL, 2.00 mL, and 2.50 mL of a 100 μg / mL silver standard solution into a 100 mL volumetric flask pre-filled with 10 mL of hydrochloric acid and shaken well. Add copper matrix to the sample according to its copper content. Dilute to the mark with water, shaking constantly during the addition of water. Mix thoroughly and label the solution as standard.

[0029] S4.2) Under the same conditions as for measuring the test solution, measure its absorbance according to the instrument operating procedures, subtract the absorbance of the "zero" concentration standard solution, and plot a working curve with silver concentration as the horizontal axis and absorbance as the vertical axis.

[0030] Furthermore, the calculation formula of silver in S5) is as follows:

[0031]

[0032] Where:

[0033] ρ—The mass concentration of silver found from the working curve, in micrograms per milliliter

[0034] (μg / mL);

[0035] V—volume of the solution to be tested, in milliliters (mL);

[0036] m0—mass of sample, in grams (g).

[0037] The calculation result is expressed to one decimal place.

[0038] Furthermore, the concentration of the concentrated hydrochloric acid is w≥30%.

[0039] In order to achieve the above purpose, the specific technical solution adopted by the present invention is:

[0040] The present invention provides a method for determining the amount of silver in crude copper by atomic absorption spectrometry, comprising the following steps:

[0041] a. Weigh 5.0 g of the sample using the weighted method of the upper and lower sieves, accurate to 0.0001 g; b. Add 50 mL of nitric acid (1+1), wait for the reaction to stop, and then place it on a hot plate and heat at low temperature.

[0042] (110℃~200℃), add 2mL of bromine water and 5mL~10mL of hydrochloric acid after the reaction stops, continue heating until the sample is completely dissolved, and evaporate to near dryness.

[0043] c. Take it out and cool it slightly, add 10% hydrochloric acid, shake it well, and heat it on a hot plate at low temperature (110℃~200℃

[0044] ℃), soluble salts are completely dissolved, add water to about 30 mL, heat to a slight boil, remove, and cool.

[0045] d. Select a volumetric flask based on the silver content of the sample, pre-fill it with concentrated hydrochloric acid, see Table 1 for details, add water to at least half the volumetric flask or reserve a volume of at least 60 mL, and mix thoroughly.

[0046] e. Transfer the solution to be tested that has been treated in step c to a volumetric flask and add water to make up the volume. This solution is the solution to be tested.

[0047] f. If sample b is not completely dissolved and there are a few particles, filter it with quick filter paper, wash it, collect the filtrate back into the original beaker and evaporate it at low temperature until it is almost dry, and put the filter paper and filter residue into another

[0048] In a 500mL beaker, add 2mL to 5mL of saturated ammonium bifluoride, shake well, and then add

[0049] Dissolve 10mL~15mL of nitric acid and sulfuric acid mixture and 2mL~5mL of perchloric acid by heating at low temperature until the smoke disappears, then follow steps c, d, and e.

[0050] g. Turn on the atomic absorption spectrometer in advance, light the silver hollow cathode lamp, preheat it, and stabilize it to the standby state.

[0051] h. Establish a detection method, using acetylene as the fuel gas and air as the auxiliary fuel gas, and set the measurement parameters of each instrument.

[0052] i. Measure the absorbance intensity of the silver element in the test solution, subtract the absorbance intensity of the blank solution accompanying the sample, and find the corresponding silver concentration from the working curve.

[0053] j. Drawing of silver working curve: 0.0 mL, 0.50 mL, 1.00 mL of silver standard solution with a concentration of 100 μg / mL were respectively placed in a 100 mL volumetric flask to which 10 mL of hydrochloric acid had been added.

[0054] mL, 1.50mL, 2.00mL, and 2.50mL were placed in 10mL of hydrochloric acid

[0055] Add the copper matrix to a 100mL volumetric flask, dilute to the mark with water, and mix well. k. Measure the absorbance intensity according to the instrument operating procedure under the same conditions as the solution to be tested.

[0056] Degree, subtract the absorbance intensity of the "zero" concentration standard solution, and draw a working curve with silver concentration as the horizontal axis and absorbance intensity as the vertical axis.

[0057] Further explanation: In step a, the sample should be stirred evenly before weighing, and multiple sampling points should be used.

[0058] Weigh 5.0 g of the sample to the nearest 0.0001 g using the down-weighting method, place it in a 500 mL beaker, and mark it.

[0059] Further, in step b, pour 50mL of nitric acid (1+1) at an angle and place it on the operating table.

[0060] Observe the reaction, wait for the reaction to stop, and then place it on a hot plate and heat at low temperature (110

[0061] ℃~200℃), continue to observe the reaction status; after the reaction stops, remove it, cool it slightly, add 2mL of bromine water and 5mL~10mL of concentrated hydrochloric acid (w≥30%), shake well, and continue to heat to dissolve; if the sulfur is not completely removed, add more bromine water until the sulfur is completely removed, wait until the test solution is dissolved and clear, continue to heat and evaporate until it is almost dry, remove it and cool it slightly.

[0062] Furthermore, in step c, add 10 mL of concentrated hydrochloric acid (w ≥ 30%), shake well, and place in an electric

[0063] Heat on a hot plate at low temperature (110℃~200℃) until the soluble salt is completely dissolved, blow water along the wall of the cup to about 30mL, shake well, continue heating at low temperature until the test solution is slightly boiling, remove and cool.

[0064] Further, in step d, a volumetric flask is selected according to the silver content of the sample, concentrated hydrochloric acid is pre-added, and the concentration is controlled.

[0065] The concentration of the hydrochloric acid medium should be consistent with that of the standard solution. Add water according to the size of the volumetric flask, leaving a volume of at least 60 mL, shake well, and mark the volumetric flask.

[0066] Further, in step e, after the solution to be tested is cooled to room temperature, the

[0067] The test solution is required to be transferred to a volumetric flask, and water is added to the volumetric flask to make up the volume. The solution needs to be shaken continuously during the process of adding water to make up the volume. This solution is the test solution.

[0068] Furthermore, in step f, if the sample in step b is not completely dissolved and a small amount of particles remain,

[0069] Filter with quick filter paper, wash the filter paper, collect the filtrate back into the original beaker, continue to operate according to step b, put the filter paper and filter residue into another 500mL beaker, add 2mL~5mL saturated ammonium bifluoride, shake well, and then add 10mL~15mL nitric acid and sulfuric acid mixture (HNO3:H2SO4:H2O

[0070] =3:1:3) and 2mL~5mL perchloric acid (ρ=1.76g / cm 3 ), heat at low temperature (180℃~260℃) to dissolve, smoke, until the smoke is gone. If there are still undissolved particles, repeat the above operation until it is completely dissolved, and then follow steps c, d, and e to obtain the solution to be tested.

[0071] Furthermore, in step g, the atomic absorption spectrometer is turned on in advance, and the silver hollow cathode lamp is lit.

[0072] The preheating time should be no less than 30 minutes until the device is in a stable standby state.

[0073] Furthermore, in step h, a detection method is established, acetylene is used as the fuel gas, and air is used as the auxiliary fuel gas.

[0074] Set the instrument measurement parameters: lamp current 3mA, slit 3nm, observation height 7mm,

[0075] Gas flow rate is 0.9L / min~1.2L / min, and bubble assist flow rate is 8.0L / min.

[0076] Further, in step i, the instrument is operated according to the operating procedures and the established detection method is used to determine

[0077] The absorbance intensity of the silver element in the test solution is subtracted from the absorbance intensity of the blank solution accompanying the sample, and the corresponding silver concentration is obtained from the working curve.

[0078] Furthermore, in step j, the silver working curve is drawn

[0079] Pipette 0.00mL, 0.50mL, 1.00mL of 100μg / mL silver standard solution

[0080] Place mL, 1.50mL, 2.00mL, and 2.50mL respectively into a 100mL volumetric flask that has been pre-added with 10mL of hydrochloric acid (w ≥ 30%) and shaken well. Add copper matrix according to the copper content of the sample and dilute to the scale with water. Shake and mix continuously during the water addition process. Affix a standard solution label and indicate the concentration, date, and information of the preparer.

[0081] Furthermore, in step k, the instrument is operated under the same conditions as those for measuring the solution to be tested.

[0082] The program measures its absorbance intensity, subtracts the absorbance intensity of the "zero" concentration standard solution, and plots a working curve with silver concentration as the horizontal axis and absorbance intensity as the vertical axis.

[0083] Compared with the prior art, the present invention has the following beneficial effects:

[0084] The present invention provides a method for detecting the silver content in blister copper, and the specific beneficial effects are as follows:

[0085] 1. The present invention weighs a sample of no less than 5.0 grams, and weighs 5 to 10 times the sample to improve the representativeness of the sample and eliminate the segregation effect of silver in the sample;

[0086] 2. The dissolved particles are treated with ammonium bifluoride, nitric acid, and perchloric acid to completely dissolve the sample and ensure that all the silver in the sample can enter the test solution;

[0087] 3. Hydrochloric acid medium can effectively complex silver ions and prevent silver precipitation;

[0088] 4. No need to dispense, just put it into the volumetric flask once, which can reduce the error caused by dispensing and volumetric flask;

[0089] 5. Direct atomic absorption spectrometry is used to determine the amount of silver. There is no need to remove the copper matrix. The silver standard solution is matched with the copper matrix. The silver spectral line has good sensitivity, which has less impact on the accuracy of the test results than the titration method for silver measurement. This shortens the test process and improves the test efficiency.

[0090] 6. Improve the accuracy of test results. The existing fire assay method has the problem of silver loss during the melting slag and ash blowing process.

[0091] The invention has the characteristics of high accuracy, good precision, simple operation, strong practicality, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0092] Figure 1 The present invention is a flowchart of a method for determining the amount of silver in crude copper by atomic absorption spectrometry. DETAILED DESCRIPTION

[0093] The embodiments described are only some of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without engaging in creative work, such as embodiments that only change the purpose without changing the basic principles of the claims, are also within the scope of protection of the present invention.

[0094] like Figure 1 As shown, the present invention provides a method for determining the amount of silver in crude copper by atomic absorption spectrometry, comprising the following steps:

[0095] a. Weigh 5.0 g of the sample using the weighted method of the upper and lower sieves, accurate to 0.0001 g; b. Add 50 mL of nitric acid (1+1), wait for the reaction to stop, and then place it on a hot plate and heat at low temperature.

[0096] (110℃~200℃), add 2mL of bromine water and 5mL~10mL of hydrochloric acid (w≥30%) after the reaction stops, continue heating until the sample is completely dissolved, and evaporate to near dryness.

[0097] c. Remove and cool slightly, add 10mL hydrochloric acid (w ≥ 30%), shake well, place on a hot plate and heat at low temperature (110℃~200℃) until the soluble salt is completely dissolved, blow water to about 30mL,

[0098] Remove from heat when it reaches a slight boil and let cool.

[0099] d. Select a volumetric flask according to the silver content of the sample, pre-add concentrated hydrochloric acid (w ≥ 30%), control the concentration of the hydrochloric acid medium to be consistent with the standard solution, add water to at least half the volumetric flask or reserve a volume of at least 60mL, and mix well.

[0100] e. Transfer the solution to be tested that has been treated in step c to a volumetric flask and add water to make up the volume. This solution is the solution to be tested.

[0101] f. If sample b is not completely dissolved and there are a few particles, filter it with quick filter paper and wash it.

[0102] Collect the filtrate back into the original beaker and evaporate at low temperature until it is almost dry. Put the filter paper and filter residue into another beaker, add 2mL-5mL saturated ammonium bifluoride, shake well, and add 10mL-15mL nitric acid and sulfuric acid mixture.

[0103] (HNO3:H2SO4:H2O=3:1:3) and 2mL~5mL perchloric acid (ρ=1.76g / cm 3 ),

[0104] Heat and dissolve at low temperature (180℃~260℃) until the smoke disappears, then follow steps c, d, and e. g. Turn on the atomic absorption spectrometer in advance, light the silver hollow cathode lamp, and preheat for at least 30

[0105] min, stabilize to standby state.

[0106] h. Establish a detection method, using acetylene as the fuel gas and air as the auxiliary fuel gas, and set the measurement parameters of each instrument.

[0107] i. Measure the absorbance intensity of the silver element in the test solution, subtract the absorbance intensity of the blank solution accompanying the sample, and find the corresponding silver concentration from the working curve.

[0108] j. Drawing of silver working curve

[0109] Pipette 0.0mL, 0.50mL, 1.00mL of 100μg / mL silver standard solution

[0110] mL, 1.50mL, 2.00mL, and 2.50mL were placed in 10mL of hydrochloric acid

[0111] (w≥30%), add copper matrix according to the copper content of the sample,

[0112] Dilute to volume with water and mix well.

[0113] k. Under the same conditions as those for measuring the solution to be tested, measure its absorbance intensity according to the instrument operating procedures, subtract the absorbance intensity of the "zero" concentration standard solution, and use the silver concentration as the horizontal axis.

[0114] The working curve is drawn with the absorbance intensity as the vertical axis.

[0115] Step a: Stir the sample evenly before weighing, take samples at multiple points, and weigh by weighting the sample above and below the sieve.

[0116] Take 5.0g of the sample, accurate to 0.0001g, and place it in a 500mL beaker, marking it. Step b: Pour 50mL of nitric acid (1+1) into the beaker at an angle, place it on the work surface, and observe the reaction. Once the reaction stops, heat it on a hot plate at a low temperature (110°C to 200°C) and continue to observe the reaction. After the reaction stops, remove the beaker, cool it slightly, add 2mL of bromine water and 5mL to 10mL of concentrated hydrochloric acid (w ≥ 30%), shake well, and continue heating to dissolve. If the sulfur has not been completely removed, add more bromine water until it is completely removed. Once the test solution is dissolved and clear, continue heating and steaming until it is nearly dry, then remove the beaker and cool it slightly.

[0117] Step c: Add 10 mL of concentrated hydrochloric acid (w ≥ 30%), shake well, and heat on a hot plate at low temperature.

[0118] (110℃~200℃), wait until the soluble salt is completely dissolved, blow water along the wall of the cup to about 30mL,

[0119] Shake well, continue heating at low temperature until the test solution is slightly boiling, remove and cool.

[0120] Step d: Select a volumetric flask according to the silver content of the sample, pre-add concentrated hydrochloric acid, and control the concentration of the hydrochloric acid medium.

[0121] The concentration is consistent with the standard solution, add water according to the size of the volumetric flask, and reserve a volume of at least 60

[0122] mL, shake well, and mark the volumetric flask.

[0123] Step e: After the solution to be tested has been cooled to room temperature,

[0124] Transfer the liquid to a volumetric flask, add water to the volumetric flask to make up the volume, and shake it constantly during the process of adding water to make up the volume.

[0125] This solution is the test solution.

[0126] Step f: If the sample in step b is not completely dissolved and there are a few particles, filter it with a quick filter paper.

[0127] Filter, wash the filter paper, collect the filtrate back to the original beaker, continue to operate according to step b, put the filter paper and filter residue into another 500mL beaker, add 2mL~5mL saturated ammonium bifluoride, shake well, and then add 10mL~15mL nitric acid and sulfuric acid (HNO3:H2SO4:H2O=3:1:3) and

[0128] 2mL~5mL perchloric acid (ρ=1.76g / cm 3 ), low temperature heating to dissolve (180℃~260

[0129] ℃), smoke, until the smoke is gone, if there are still undissolved particles, repeat the above operation until they are completely dissolved, and then follow steps c, d, and e to obtain the test solution.

[0130] Step g: Turn on the atomic absorption spectrometer in advance and light the silver hollow cathode lamp.

[0131] Less than 30 minutes until it is in a stable standby state.

[0132] Step h: Establish the detection method, acetylene as fuel gas, air as auxiliary fuel gas, and set up the instruments.

[0133] Measurement parameters: lamp current 3mA, slit 3nm, observation height 7mm, gas flow rate

[0134] 0.9L / min~1.2L / min, bubble-assisted flow rate 8.0L / min.

[0135] Step i: Follow the instrument operating procedures and determine the silver content in the test solution according to the established detection method.

[0136] The absorbance intensity of the element is subtracted from the absorbance intensity of the blank solution accompanying the sample, and the corresponding silver concentration is obtained from the working curve.

[0137] Step j: Drawing of silver working curve

[0138] Pipette 0.00mL, 0.50mL, 1.00mL of 100μg / mL silver standard solution

[0139] Place mL, 1.50mL, 2.00mL, and 2.50mL respectively into a 100mL volumetric flask that has been pre-added with 10mL of hydrochloric acid (w ≥ 30%) and shaken well. Add copper matrix according to the copper content of the sample and dilute to the scale with water. Shake and mix continuously during the water addition process. Affix a standard solution label and indicate the concentration, date, and information of the preparer.

[0140] Step k: Under the same conditions as the solution to be tested, measure the absorbance according to the instrument operating procedures.

[0141] Light intensity, minus the absorbance intensity of the "zero" concentration standard solution, draw a working curve with silver concentration as the horizontal axis and absorbance intensity as the vertical axis.

[0142] The calculation formula for silver is as follows:

[0143]

[0144] Where:

[0145] ρ—The mass concentration of silver found from the working curve, in micrograms per milliliter

[0146] (μg / mL);

[0147] V—volume of the solution to be tested, in milliliters (mL);

[0148] m0—mass of sample, in grams (g).

[0149] The calculation result is expressed to one decimal place.

[0150] The above schemes are only descriptions of several better implementation methods of the present application, but the scope of protection of the present application is not limited to this. Any changes or replacements that can be easily implemented by anyone familiar with the technology within the scope of the description of the present application without changing the basic principles involved in the claims should be covered by the scope of protection of the present application, that is, the scope of protection of the present application should be based on the scope of protection of the claims.

[0151] Example 1

[0152] A method for determining the amount of silver in crude copper using atomic absorption spectrometry comprises the following steps:

[0153] a. Weigh 5.0000g of the sample using the over-sieve and under-sieve weighting method, accurate to 0.0001g;

[0154] b. Add 50mL of nitric acid (1+1), wait for the reaction to stop, and then place it on a hot plate and heat at low temperature.

[0155] (110℃~200℃), add 2mL of bromine water and 5mL~10mL of hydrochloric acid (w≥30%) after the reaction stops, continue heating until the sample is completely dissolved, and evaporate to near dryness.

[0156] c. Remove and cool slightly, add 10% hydrochloric acid (w ≥ 30%), shake well, place on a hot plate and heat at low temperature (110℃~200℃) until the soluble salt is completely dissolved, blow water to about 30mL, heat to a slight boil, remove and cool.

[0157] d. Select a volumetric flask according to the silver content of the sample, pre-add concentrated hydrochloric acid (w ≥ 30%), control the concentration of the hydrochloric acid medium to be consistent with the standard solution, add water to at least half the volumetric flask or reserve a volume of at least 60mL, and mix well.

[0158] e. Transfer the solution to be tested that has been treated in step c to a volumetric flask and add water to make up the volume. This solution is the solution to be tested.

[0159] f. If sample b is not completely dissolved and there are a few particles, filter it with quick filter paper, wash it, collect the filtrate back into the original beaker and steam it at low temperature until it is almost dry, then put the filter paper and filter residue into another 500mL

[0160] In a beaker, add 2mL~5mL of saturated ammonium bifluoride, shake well, add 10mL~15mL of nitric acid and sulfuric acid mixture (HNO3:H2SO4:H2O=3:1:3) and 2mL~5mL of perchloric acid (ρ=

[0161] 1.76g / cm 3 ), heat at low temperature to dissolve (180℃~260℃) until the smoke disappears, then follow steps c, d, and e.

[0162] g. Turn on the atomic absorption spectrometer in advance, light the silver hollow cathode lamp, preheat it, and stabilize it to the standby state.

[0163] h. Establish a detection method, using acetylene as the fuel gas and air as the auxiliary fuel gas, and set the measurement parameters of each instrument.

[0164] i. Measure the absorbance intensity of the silver element in the test solution, subtract the absorbance intensity of the blank solution accompanying the sample, and find the corresponding silver concentration from the working curve.

[0165] j. Drawing of silver working curve

[0166] Pipette 0.0mL, 0.50mL, 1.00mL, 1.50mL, 2.00mL and 2.50mL of the silver standard solution with a concentration of 100μg / mL into a 10mL hydrochloric acid (w

[0167] ≥30%), add copper matrix according to the copper content of the sample, dilute to the scale with water, and mix well.

[0168] k. Under the same conditions as those for measuring the solution to be tested, measure its absorbance intensity according to the instrument operating procedures, subtract the absorbance intensity of the "zero" concentration standard solution, and draw a working curve with silver concentration as the horizontal axis and absorbance intensity as the vertical axis.

[0169] Precision experiment:

[0170] Repeat the above operation to obtain the silver test results of three crude copper samples as shown in Table 1.

[0171] Table 1

[0172]

[0173] From the data in Table 1, it can be seen that the relative standard deviations (RSDs) of the silver test results of the seven parallel cups are between 1.0% and 4.7%, all less than 5.0%, indicating that the precision of the test results is good.

[0174] Spike recovery experiment:

[0175] Different amounts of silver labels were added during the sample weighing process in step a of Example 1. The other steps were the same as in Example 1. The spiked recovery rate was calculated by analyzing the results to verify the accuracy of the method. The results are shown in Table 2, Spiked Recovery Data Table.

[0176] Table 2

[0177]

[0178]

[0179] From the data in Table 2, it can be concluded that two crude copper samples were dissolved in nitric acid, then added with bromine water and hydrochloric acid, evaporated to near dryness, leached with hydrochloric acid, filtered, and then dissolved in saturated ammonium bifluoride solution, a mixed solution of nitric and sulfuric acid, and perchloric acid until smoke disappeared. The sample was then leached with hydrochloric acid and transferred to a volumetric flask. The silver content was determined on an atomic absorption spectrometer using hydrochloric acid as the medium, acetylene as the fuel gas, and air as the auxiliary gas. The spiked silver recovery was between 94.0% and 103.0%, indicating the high accuracy of this detection method.

[0180] The present invention provides a detailed description of a method for determining the amount of silver in blister copper using atomic absorption spectrometry, as provided in the examples of this application. The above examples are intended only to facilitate understanding of the method and its core concept. Furthermore, those skilled in the art will appreciate that variations in the specific implementation and scope of application are possible based on the concepts of this application. Therefore, this specification should not be construed as limiting this application.

[0181] For example, certain words are used in the specification and claims to refer to specific components. Those skilled in the art should understand that hardware manufacturers may use different nouns to refer to the same component. This specification and claims do not use differences in names as a way to distinguish components, but use differences in the functions of components as the criteria for distinction. For example, "including" and "comprising" mentioned throughout the specification and claims are open-ended terms, so they should be interpreted as "including / including but not limited to". "Approximately" means that within an acceptable error range, those skilled in the art can solve the technical problems within a certain error range and basically achieve the technical effects. The subsequent description in the specification is a preferred embodiment of the present application, but the description is for the purpose of illustrating the general principles of the present application, and is not used to limit the scope of the present application. The scope of protection of the present application shall be as defined in the attached claims.

[0182] It should also be noted that the terms "include," "comprises," or any other variations thereof are intended to encompass non-exclusive inclusion, such that a product or system comprising a series of elements includes not only those elements but also other elements not explicitly listed, or elements inherent to such product or system. In the absence of further limitations, an element defined by the phrase "comprises a..." does not exclude the presence of other identical elements in the product or system comprising the element.

[0183] It should be understood that the term "and / or" as used herein is merely a description of the relationship between associated objects, indicating that three possible relationships exist. For example, "A and / or B" can represent: A exists alone, A and B exist simultaneously, or B exists alone. Furthermore, the character " / " in this document generally indicates that the associated objects are in an "or" relationship.

[0184] The above description shows and describes several preferred embodiments of the present application. However, as previously mentioned, it should be understood that the present application is not limited to the form disclosed herein and should not be construed as excluding other embodiments. Instead, the present application can be used in various other combinations, modifications, and environments and can be modified within the scope of the application concept described herein through the above teachings or technology or knowledge in the relevant field. Modifications and variations made by those skilled in the art that do not depart from the spirit and scope of the present application should be protected by the claims appended hereto.

Claims

1. A method for determining the amount of silver in crude copper by atomic absorption spectrometry, characterized in that: The detection method specifically comprises the following steps: S1) Weigh a certain amount of crude copper to be measured and dissolve it in nitric acid, then add bromine water and concentrated hydrochloric acid to remove sulfur, and evaporate to near dryness; S2) adding concentrated hydrochloric acid to the sample treated in S1) for leaching, transferring it to a volumetric flask and adding water to make up to volume, thereby obtaining a test solution; S3) starting the atomic absorption spectrometer and setting the measurement parameters; S4) preparing a silver working curve matching the copper matrix and measuring the solution to be tested; S5) obtaining the mass concentration of silver from the silver working curve, and calculating the silver content in the crude copper.

2. The detection method according to claim 1, wherein The detection method further comprises the following steps: After the hydrochloric acid leaching in S2), the crude copper sample is not completely dissolved and there are a small amount of particles. It is filtered with quick filter paper, washed with filter paper, and the filtrate is collected back into the original beaker. The filter paper and filter residue are placed in another 500mL beaker, 2mL~5mL of saturated ammonium bifluoride are added, shaken, and then 10mL~15mL of nitric acid and sulfuric acid mixture and 2mL~5mL of perchloric acid are added. Heat at low temperature to dissolve, smoke, until the smoke is gone. If there are still undissolved particles, repeat the above operation until it is completely dissolved.

3. The detection method according to claim 2, characterized in that The ratio between the various acids in the nitric-sulfuric acid mixture is HNO3:H2SO4:H2O=3:1:3; The low temperature is 180℃~260℃.

4. The detection method according to claim 1, wherein The crude copper measured in S1) is weighed by weighting the sieve and weighing the copper to a weight of not less than 5.0 g.

5. The detection method according to claim 1, wherein The specific steps of S1) are: S1.1) Pour a certain amount of nitric acid into the crude copper sample to be measured in a beaker. Place it on the work surface and observe the reaction. Once the reaction stops, heat it on a hot plate to a low temperature of 110°C to 200°C and continue to observe the reaction. After the reaction stops, remove it and let it cool slightly. S1.2) Add 2 mL of bromine water and 5 mL to 10 mL of concentrated hydrochloric acid, shake well, and continue heating to dissolve. If the sulfur has not been completely removed, add more bromine water until the sulfur is completely removed. Wait until the test solution is dissolved and clear. Continue heating and steaming until nearly dry, then remove and cool slightly.

6. The detection method according to claim 1, characterized in that The specific steps of S2) are: S2.1) Add 10 mL of concentrated hydrochloric acid to the sample obtained in S1), shake well, and heat on a hot plate to a low temperature of 110°C to 200°C. Once the soluble salt is completely dissolved, pipette water along the sides of the cup to a volume of at least 30 mL. Shake well, and continue heating until the solution is slightly boiling. Remove the sample and allow it to cool. S2.2) Pre-fill a volumetric flask selected based on the silver content of the sample with concentrated hydrochloric acid, controlling the concentration of the hydrochloric acid medium to match the standard solution. Add water to the volumetric flask to a minimum of 60 mL, shake well, and label the flask. S2.3) After the test solution treated in S2.2) has cooled to room temperature, transfer the test solution to a volumetric flask according to the operating instructions. Add water to the volumetric flask to the required volume, shaking the flask continuously during the process to obtain the test solution.

7. The detection method according to claim 1, characterized in that The S3) is summarized as follows: using hydrochloric acid as the medium, acetylene as the fuel gas, and air as the combustion-supporting gas, setting the measurement parameters of each instrument to be lamp current 3 mA, slit 3 nm, observation height 7 mm, fuel gas flow rate 0.9 L / min to 1.2 L / min, and bubble-supporting gas flow rate 8.0 L / min.

8. The detection method according to claim 1, wherein The specific steps of S4) are: S4.1) Pipette 0.00 mL, 0.50 mL, 1.00 mL, 1.50 mL, 2.00 mL, and 2.50 mL of a 100 μg / mL silver standard solution into a 100 mL volumetric flask pre-filled with 10 mL of hydrochloric acid and shaken well. Add copper matrix to the sample according to its copper content. Dilute to the mark with water, shaking constantly during the addition of water. Mix thoroughly and label the solution as standard. S4.2) Under the same conditions as for the test solution, measure its absorbance according to the instrument operating procedures, subtract the absorbance of the "zero" concentration standard solution, and plot a working curve with silver concentration as the horizontal axis and absorbance as the vertical axis.

9. The detection method according to claim 1, wherein The calculation formula of silver in the S5) is as follows: Where: ρ—The mass concentration of silver found from the working curve, in micrograms per milliliter (μg / mL); V—volume of the solution to be tested, in milliliters (mL); m0—mass of sample, in grams (g); The calculation result is expressed to one decimal place.

10. The detection method according to claim 1, characterized in that The concentration of the concentrated hydrochloric acid is w≥30%.