Silver powder with high twin crystal ratio and preparation method and application thereof
Through the synergistic effect of carboxylic acid ligands and initiators, combined with a specific process sequence, the twin ratio of silver powder is regulated, solving the problems of low twin ratio and wide particle size distribution in the preparation of traditional twinned silver powder, achieving efficient and environmentally friendly silver powder production, and meeting the high conductivity and printing stability requirements of TOPCon batteries.
Patent Information
- Application Number
- CN202510793517.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-06-13
- Publication Date
- 2025-09-26
AI Technical Summary
The supersaturation of silver ions in the preparation of traditional twinned silver powder is difficult to accurately control, resulting in a low twin ratio and a wide particle size distribution, which affects the printing stability and sintering consistency of the silver paste. The process is also complex and costly.
By using the synergistic effect of carboxylic acid ligands and initiators, the nucleation and crystal growth of silver ions are controlled, combined with non-stirring rapid feeding and aging treatment, the proportion of silver powder twins is regulated, a low supersaturation environment is formed, and the orderly formation of twin structures is promoted.
Significantly increase the twin ratio to 20-55%, ensure uniformity of silver powder particles and narrow particle size distribution, meet the high conductivity and printing accuracy requirements of TOPCon batteries, and reduce production costs.
Smart Images

Figure CN120696434A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of silver powder, and in particular to a silver powder with a high twinning ratio, and a preparation method and application thereof. Background Art
[0002] With the advancement of high-efficiency photovoltaic cell technology, the performance requirements for silver powder, a core electrode material, have significantly changed. The ultra-fine gridline printing and high conductivity requirements of TOPCon cells are driving the development of silver powders with high specific surface area, low contact resistance, and high sintering activity. Twinned silver powder, due to its unique crystal structure, offers significant advantages in printing precision and sintering activity, making it a mainstream material for meeting the requirements of TOPCon cells. However, during the traditional twinned silver powder preparation process, the silver ion supersaturation is difficult to precisely control, which can easily lead to secondary nucleation or uneven crystal growth rates. This results in a generally low twinning ratio and a wide particle size distribution, compromising the printing stability and sintering consistency of the silver paste. Patent CN202111532484.0 discloses a method for preparing quasi-spherical silver powder. Nanosilver seeds are prepared using a high-temperature hydrothermal method to induce particle size control. A secondary dispersant is then added to the reaction system to prevent particle aggregation. The resulting silver powder exhibits good overall uniformity, but the twinning ratio is low (less than 10%). The process is complex, time-consuming, and expensive.
[0003] Therefore, there is an urgent need for an efficient, environmentally friendly, and scalable method for producing silver powder with a high twinning ratio to meet client application needs. Summary of the Invention
[0004] In view of this, the present application provides a silver powder with a high twinning ratio and a preparation method and application thereof, which are used to solve the problem of how to increase the twinning ratio of silver powder.
[0005] In order to achieve the above technical objectives, this application adopts the following technical solutions: In a first aspect, the present application provides a method for preparing silver powder with a high twinning ratio, comprising the following steps: S1. A carboxylic acid ligand is added to the silver source solution to obtain a silver precursor solution; a dispersant and an initiator are sequentially added to the reducing agent solution to obtain a reaction bottom solution; S2. After adding the silver precursor solution to the reaction base liquid for redox reaction, the mixture was aged to obtain a mixed mother liquor; S3. The mixed mother liquor was filtered, washed, dispersed and dried to obtain a high twin ratio silver powder; The initiator includes one or more of sulfate, carbonate and nitrate.
[0006] Preferably, the mass ratio of the carboxylic acid ligand to the initiator is (0.2-0.5): (0.001-0.005).
[0007] Preferably, the carboxylic acid ligand includes one or more of ethylenediaminetetraacetic acid, tartaric acid, tryptophan, tyrosine, and aspartic acid.
[0008] Preferably, the initiator includes one or more of sodium sulfate, copper sulfate, potassium sulfate, magnesium sulfate, sodium bicarbonate, sodium carbonate, potassium carbonate, sodium nitrate, and potassium nitrate.
[0009] Preferably, the dispersant includes one or more of polyvinyl pyrrolidone, gelatin, and polyethylene glycol; the mass ratio of the dispersant to the silver source is (0.08-0.2):1.
[0010] Preferably, the reducing agent includes one or more of ascorbic acid, glucose, and hydrazine hydrate; and the mass ratio of the initiator, the reducing agent, and the silver source is (0.001-0.005): (0.6-2): 1.
[0011] Preferably, the specific operation of step S2 is: pouring the silver precursor solution into the reaction base liquid within 10-30 seconds without stirring to carry out redox reaction, and then standing and aging for 15-30 minutes to obtain a mixed mother liquor.
[0012] Preferably, in step S3, the mixed mother liquor is filtered and then washed with deionized water until the conductivity is ≤15 μs / cm to obtain a wet powder, which is then dispersed with an ethanol solution containing a coating agent, filtered and dried to obtain a silver powder with a high twinning ratio.
[0013] In a second aspect, the present application provides a high twinning ratio silver powder, wherein the twinning ratio is 20-55%.
[0014] In a third aspect, the present application provides an application of high twin ratio silver powder in the preparation of TOPCon conductive paste.
[0015] The beneficial effects of the present application are as follows: the present application effectively regulates the nucleation and crystal growth behavior of silver ions through the synergistic effect of the initiator and the carboxylic acid ligand, combined with a specific process sequence. The initiator increases the ionic strength of the solution, controls the reduction rate, and competes with the ligand for adsorption, thereby promoting the preferential growth of silver nuclei on the {111} plane; the ligand achieves a "slow-release effect" by forming a stable complex, and selectively adsorbs on a specific crystal plane, further promoting the formation of twin interfaces; the process adopts rapid feeding and aging without stirring to ensure a kinetic path of nucleation followed by growth, avoiding heterogeneous growth, and the two synergistically construct a low supersaturation environment to induce silver powder to grow along the {111} plane. <110> Direction-selective growth significantly increases the twin ratio. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 This is an electron microscope photograph of the silver powder in Example 1; Figure 2This is an electron microscope photograph of the silver powder of Example 2; Figure 3 This is an electron microscope photograph of the silver powder of Example 3; Figure 4 This is an electron microscope photograph of the silver powder in Comparative Example 1. DETAILED DESCRIPTION
[0017] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0018] The present application provides a method for preparing silver powder with a high twinning ratio, comprising the following steps: S1. A carboxylic acid ligand is added to the silver source solution to obtain a silver precursor solution; a dispersant and an initiator are sequentially added to the reducing agent solution to obtain a reaction bottom solution; S2. After adding the silver precursor solution to the reaction base liquid for redox reaction, the mixture was aged to obtain a mixed mother liquor; S3. The mixed mother liquor was filtered, washed, dispersed and dried to obtain a high twin ratio silver powder; The initiator includes one or more of sulfate, carbonate and nitrate.
[0019] This application achieves an increase in the proportion of silver powder twins through the combination of raw materials and processes. The specific mechanism is as follows: From the perspective of raw materials, the initiator of the present application increases the nucleation ion strength of the solution. This high ionic strength helps to control the reduction rate of silver ions, avoids excessive nucleation leading to the formation of non-uniform particles, and thus provides a relatively stable environment for subsequent crystal growth. At the same time, the initiator changes the energy state distribution on the surface of the silver nucleus by competitive adsorption with the carboxylic acid ligand, prompting the nucleus to grow preferentially in certain directions, so that the silver ions are more exposed to the {111} plane, which is a favorable crystal plane for the formation of twin structures; the carboxylic acid ligand of the present application can react with Ag + Form a stable complex and delay the + The reduction rate is reduced to prevent instantaneous large-scale nucleation leading to amorphous or disordered structure. This "slow-release effect" helps to achieve a more controllable crystal growth process and lays the foundation for the orderly formation of twin structures. In addition, the ligand can selectively adsorb on specific crystal planes (such as {100}), inhibiting the growth rate of these crystal planes, while the relatively unadsorbed crystal planes (such as {111}) become the main growth planes, promoting the appearance of twin interfaces; Therefore, the present application can effectively regulate the free Ag in the system through the synergistic effect of the initiator and the ligand. +The concentration of silver ions is reduced to form a low supersaturation environment, in which the silver nuclei are more likely to grow along a specific direction and form twin interfaces. At the same time, the release rate of silver ions and the preferred orientation and crystal surface exposure state of the nuclei are adjusted, thus constructing an environment that is conducive to {111} surface exposure and {111} surface exposure. <110> The twinning ratio is greatly increased by creating an environment for directional growth.
[0020] From the perspective of process sequence, the design of no stirring, rapid feeding, and aging treatment during the entire reaction process of this application ensures a kinetic path of nucleation before growth, avoids heterogeneous growth caused by the overlap of nucleation and growth processes, and provides basic conditions for the orderly formation of twin structures. Replacing the order causes some mechanisms to fail, affecting the results. Specifically: in step S1, a ligand is added and mixed evenly with the silver nitrate solution to ensure that a stable silver ion complex is formed in the preparation stage of the silver precursor solution. When this solution is quickly added to the reaction base liquid containing the initiator, the ligand and the initiator begin to interact, affecting the release rate of silver ions and the selective growth direction of the crystal nucleus. The aging stage further enhances the effect of this interaction, allowing the silver crystal nucleus to grow in a specific direction under a low supersaturation environment, providing time for the silver ions to initially reorganize under the joint action of the initiator and the ligand, thereby increasing the twin ratio.
[0021] In some embodiments, the mass ratio of the carboxylic acid ligand to the initiator is (0.2-0.5): (0.001-0.005).
[0022] In this embodiment, the initiator stabilizes the nucleation environment through high ionic strength, and competitively adsorbs with the ligand to precisely control the surface energy state of the silver nucleus, promoting the full exposure of the {111} facets. The ligand forms a stable complex at an appropriate concentration, achieving a "slow-release effect" and inhibiting the growth of unnecessary crystal faces. When the mass ratio of the carboxylic acid ligand to the initiator is controlled within the above range, the synergistic effect of the two is optimal, maintaining the solution at an ideal low supersaturation, guiding the silver nucleus to form a stable complex. <110> The orderly growth in the direction greatly increases the twin ratio. Compared with the ratio outside this range, it has significant advantages in the efficiency of twin structure formation and crystal growth quality.
[0023] In some embodiments, the carboxylic acid ligand comprises one or more of ethylenediaminetetraacetic acid, tartaric acid, tryptophan, tyrosine, and aspartic acid. In some embodiments, the initiator comprises one or more of sodium sulfate, copper sulfate, potassium sulfate, magnesium sulfate, sodium bicarbonate, sodium carbonate, potassium carbonate, sodium nitrate, and potassium nitrate. Preferably, the initiator is copper sulfate, and the silver source comprises silver nitrate.
[0024] In this embodiment, the high charge density of sulfate and carbonate can significantly enhance the ionic strength of the solution, followed by nitrate; when aminocarboxyl ligands (such as EDTA) are used in combination with sulfate, their carboxyl groups preferentially form a competitive adsorption layer with SO4²⁻, forcing silver ions to be more exposed to the twin active surface (the proportion of {111} surface increases to 85%, while Cu 2+ The / EDTA complex can act as an atomic-scale template to induce silver atoms to <110> The preferential growth direction significantly improves the twin ratio.
[0025] In some embodiments, the dispersant includes one or more of polyvinyl pyrrolidone, gelatin, and polyethylene glycol; the mass ratio of the dispersant to the silver source is (0.08-0.2):1.
[0026] In this embodiment, the introduction of the dispersant forms an electrostatic steric barrier layer on the particle surface, inhibits particle agglomeration, assists in crystal plane control, ensures that the prepared silver powder particles are uniform and independent, and is beneficial to the stability of the twin structure; the introduction of the dispersant is conducive to forming a narrower particle size distribution, so that the prepared conductive paste has better thixotropy, meeting the fine line printing requirements of TOPCon batteries.
[0027] In some embodiments, the reducing agent includes one or more of ascorbic acid, glucose, and hydrazine hydrate; the mass ratio of the initiator, the reducing agent, and the silver source is (0.001-0.005): (0.6-2): 1.
[0028] In some embodiments, the specific operation of step S2 is: in a non-stirring state, pouring the silver precursor solution into the reaction base liquid within 10-30 seconds to perform an oxidation-reduction reaction, and then standing and aging for 15-30 minutes to obtain a mixed mother liquor.
[0029] In some embodiments, in step S3, the mixed mother liquor is filtered and then washed with deionized water until the conductivity is ≤15 μs / cm to obtain a wet powder. The wet powder is dispersed with an ethanol solution containing a coating agent, filtered and dried to obtain a silver powder with a high twinning ratio.
[0030] The present application provides a high twinning ratio silver powder with a twinning ratio of 20-55%. The twinning structure consists of 2-4 silver particles and is gourd-shaped or pod-shaped. It is worth noting that the higher the twinning ratio, the better. An appropriate amount of twinning structure can improve conductivity through low-resistance grain boundaries. At the same time, the support of the twinning structure helps to achieve fine grid line requirements. However, excessive twinning will lead to increased contact resistance fluctuations and deterioration of the slurry rheology, which may cause problems such as excessive viscosity or poor printability.
[0031] The present application provides an application of high twin ratio silver powder in the preparation of TOPCon conductive paste.
[0032] The present invention is further described below through specific examples.
[0033] Example 1 A method for preparing silver powder with a high twinning ratio comprises the following steps: S1. 50g of silver nitrate was dissolved in 600ml of deionized water to prepare a silver nitrate solution, to which 15g of ethylenediaminetetraacetic acid (EDTA) was added and stirred with a glass rod to obtain a silver precursor solution for later use; 30g of ascorbic acid was dissolved in an appropriate amount of deionized water to prepare a reducing agent solution, to which 4g of polyvinyl pyrrolidone was dissolved in a dispersant solution and 0.05g of sodium sulfate, stirred and mixed to obtain a reaction bottom solution for later use; S2. The reaction mixture was placed in a reactor and the silver precursor solution was quickly poured into the reaction mixture. The entire addition process was controlled within 10s without stirring. After the addition was complete, the reaction system was allowed to mature for 15 minutes to obtain a mixed mother liquor. S3. The obtained mixed mother liquor is filtered through a solid-liquid separator, and then washed with deionized water until the conductivity of the washing liquid is ≤15μs / cm to obtain a wet powder. The wet powder is placed in a high-speed disperser, and an anhydrous ethanol solution containing a coating agent is added and dispersed for 30 minutes. After filtering again, it is placed on a plate and placed in a blast drying oven for drying to obtain a silver powder with a high twin ratio. The mixed mother liquor is filtered, washed, dispersed and dried to obtain a silver powder with a high twin ratio.
[0034] The high twin ratio silver powder obtained in this embodiment has a D50 of 1.5 μm and a particle size distribution span of 0.96. Figure 1 As shown, the silver powder particles have a distinct twin structure, most of which are pod-shaped, with a twinning ratio of approximately 50%. The silver powder prepared in this example was mixed with an organic resin, a binder, and other organic carriers in a mass ratio of 88:12 to form a conductive silver paste. This paste was screen-printed onto TOPCon solar cells, dried, and sintered at high temperature. The printed and sintered electrode line widths were measured using a high-precision optical microscope, revealing an average line width of 22.7 μm. The line edges were neat and smooth, with no noticeable jagged edges or burrs. The contact resistance was also measured to be 17.2 mΩ·cm².
[0035] Example 2 A method for preparing silver powder with a high twinning ratio comprises the following steps: S1. Dissolve 50g of silver nitrate in 600ml of deionized water to prepare a silver nitrate solution. Add 25g of ethylenediaminetetraacetic acid (EDTA) to the solution and stir with a glass rod to mix thoroughly. This will produce a silver precursor solution, which will be used for later use. Dissolve 100g of ascorbic acid in an appropriate amount of deionized water to prepare a reducing agent solution. Add a dispersant solution containing 10g of gelatin and 0.25g of copper sulfate to the solution, stirring thoroughly to obtain a reaction base solution, which will be used for later use. S2. Place the reaction mixture in a reaction vessel and quickly pour the silver precursor solution into the reaction mixture. The entire addition process is controlled within 15 seconds without stirring. After the addition is completed, let the reaction system mature for 30 minutes to obtain a mixed mother liquor. S3. The resulting mixed mother liquor is filtered through a solid-liquid separator and then washed with deionized water until the conductivity of the washing liquid is ≤15 μs / cm, thereby obtaining a wet powder. The wet powder is placed in a high-speed disperser, and an anhydrous ethanol solution containing a coating agent is added and dispersed for 30 minutes. The powder is filtered again, placed on a plate, and dried in a forced air drying oven to obtain a silver powder with a high twinning ratio. The mixed mother liquor is filtered, washed, dispersed, and dried to obtain a silver powder with a high twinning ratio.
[0036] The high twin ratio silver powder obtained in this example has a D50 of 1.8 μm and a particle size distribution span of 1.02. Figure 2 As shown, the silver powder particles have a distinct twin structure, most of which are gourd-shaped, with a twinning ratio of approximately 30%. The silver powder prepared in this example was mixed with an organic resin, binder, and other organic carriers in a mass ratio of 88:12 to form a conductive silver paste. This paste was then screen-printed onto TOPCon cells, dried, and sintered at high temperature. The printed and sintered electrode line widths were measured using a high-precision optical microscope, revealing an average line width of 26.4 μm. The line edges were neat and smooth, with no noticeable jagged edges or burrs. The contact resistance was also measured to be 19.8 mΩ·cm².
[0037] Example 3 A method for preparing silver powder with a high twinning ratio comprises the following steps: S1. 50g of silver nitrate was dissolved in 600ml of deionized water to prepare a silver nitrate solution, to which 10g of tartaric acid was added and stirred with a glass rod to obtain a silver precursor solution for later use; 60g of ascorbic acid was dissolved in an appropriate amount of deionized water to prepare a reducing agent solution, to which 7g of polyethylene glycol dispersant solution and 0.15g of potassium carbonate were successively added and stirred to obtain a reaction base solution for later use; S2. Place the reaction mixture in a reactor and quickly pour the silver precursor solution into the reaction mixture. The entire addition process is controlled within 30 seconds without stirring. After the addition is completed, let the reaction system mature for 30 minutes to obtain a mixed mother liquor. S3. The resulting mixed mother liquor is filtered through a solid-liquid separator and then washed with deionized water until the conductivity of the washing liquid is ≤15 μs / cm, yielding a wet powder. The wet powder is then placed in a high-speed disperser and dispersed in an anhydrous ethanol solution containing a coating agent for 30 minutes. The powder is then filtered again, plated, and dried in a forced air drying oven to yield a silver powder with a high twinning ratio.
[0038] The high twin ratio silver powder obtained in this example has a D50 of 2.0 μm and a particle size distribution span of 1.05. Figure 3 As shown, most of the particles are regular gourd-shaped, with a twinning ratio of approximately 40%. The silver powder prepared in this example was mixed with an organic resin, binder, and other organic carriers in a mass ratio of 88:12 to form a conductive silver paste. This paste was screen-printed onto TOPCon cells, dried, and sintered at high temperature. The printed and sintered electrode line widths were measured using a high-precision optical microscope, revealing an average line width of 23.4 μm. The line edges were neat and smooth, with no noticeable jagged edges or burrs. The contact resistance was also measured to be 18.3 mΩ·cm².
[0039] Examples 4-6 A method for preparing silver powder with a high twinning ratio, the other contents are the same as those in Example 3, except that the amounts of the complexing agent tartaric acid are 15g, 20g, and 25g, respectively.
[0040] In Example 4, the silver powder produced had a D50 of 1.8 μm, a particle size distribution span of 0.98, and a twinning ratio of approximately 45%. When formulated into a conductive silver paste, the printed electrodes had an average line width of 22.1 μm and a contact resistance of 17.8 mΩ·cm². The lines had smooth, burr-free edges, and the paste exhibited excellent rheological properties.
[0041] In Example 5, the silver powder produced had a D50 of 1.6 μm, a particle size distribution span of 0.95, and a twinning ratio of 50%. When used in conductive paste, the printed line width averaged 21.5 μm, with a contact resistance as low as 16.9 mΩ·cm², meeting the fine-line printing requirements for TOPCon batteries.
[0042] In Example 6, the silver powder produced had a D50 of 1.4 μm, a particle size distribution span of 1.03, and a twinning ratio reduced to 38%. The conductive paste printed with an average line width of 24.3 μm and a contact resistance of 19.5 mΩ·cm² exhibited slightly high viscosity, resulting in no noticeable jagged edges or burrs.
[0043] Comparative Example 1 A method for preparing silver powder, the other contents of which are the same as those of Example 3, except that a ligand is not added in step S1; in step S2, a silver precursor solution is placed in a reactor, and a reducing agent-dispersant-initiator mixed solution is quickly added thereto, the entire feeding process is controlled within 30 seconds, and no stirring is performed during the process. After the feeding is completed, the reaction system is allowed to mature for 30 minutes; in step S3, the obtained mixed mother liquor is filtered through a solid-liquid separator, and then washed with deionized water until the conductivity of the washing liquid reaches ≤15μs / cm to obtain a wet powder, which is placed in a high-speed disperser, and an anhydrous ethanol solution containing a coating agent is added and dispersed for 30 minutes. After filtering again, the solution is placed on a plate and dried in a forced air drying oven to obtain a finished silver powder.
[0044] After testing, the silver powder obtained in this comparative example has a D50 of 2.2 μm and a particle size distribution span of 1.7. Figure 4 As shown in the figure, the electron microscope shows that the particle morphology is uneven and there is almost no twin structure. The silver powder prepared in this comparative example is mixed with organic carriers such as organic resin and binder in a mass ratio of 88:12 to prepare a conductive silver paste. The paste is printed on the TOPCon solar cell using a screen printer, dried and sintered at a high temperature. The electrode line width after printing and sintering is measured using a high-precision optical microscope. The average line width is 31.4μm, and burrs appear on the line edges. The contact resistance value is tested to be 25.6mΩ・cm².
[0045] Comparative Example 2 A method for preparing silver powder is otherwise identical to Example 3, except that no initiator is added. The resulting silver powder has a D50 of 2.8 μm and a particle size distribution span of 1.32. Due to the lack of an initiator, the solution's nucleation ionic strength is insufficient, leading to uncontrolled silver ion reduction rates and non-uniform nucleation and disordered growth. The silver powder particles are uneven in size, making it difficult to form twin structures, with a twinning ratio of only 8%. After preparing the conductive silver paste, the printed electrodes exhibited an average line width of 31.2 μm and a contact resistance of 25.6 mΩ cm². The line edges were rough and exhibited significant agglomeration.
[0046] Comparative Example 3 A method for preparing silver powder is otherwise identical to Example 3, except that sodium chloride is used as the initiator. The resulting silver powder has a D50 of 2.5 μm and a particle size distribution span of 1.18. Due to the low charge density of chloride ions in sodium chloride, the solution's ionic strength cannot be effectively increased, and competitive adsorption with the complexing agent is not possible. This results in a failure to regulate the surface energy state distribution of the silver nuclei, significantly reducing the twinning induction effect and resulting in a twinning ratio of approximately 13%. After printing, the average electrode line width was 28.7 μm, the contact resistance was 22.3 mΩ·cm², the slurry rheology deteriorated, and jagged defects appeared on the printed edges.
[0047] This application effectively regulates the nucleation and crystal growth behavior of silver ions through the synergistic effect of initiators and carboxylic acid ligands, combined with a specific process sequence. The initiator increases the ionic strength of the solution, controls the reduction rate, and competes with the ligand for adsorption, prompting the silver nucleus to preferentially grow on the {111} surface; the ligand achieves a "slow release effect" by forming a stable complex, and selectively adsorbs on a specific crystal surface, further promoting the formation of twin interfaces. The process adopts rapid feeding and aging without stirring to ensure the kinetic path of nucleation first and then growth, avoiding heterogeneous growth. The two work together to build a low supersaturation environment to induce silver powder to grow along the {111} surface. <110> Direction-selective growth significantly increases the twin ratio.
[0048] The above are only preferred specific embodiments of the present invention, but the scope of protection of the present invention is not limited thereto. Any changes or replacements that can be easily thought of by any technician familiar with this technical field within the technical scope disclosed by the present invention should be covered by the scope of protection of the present invention.
Claims
1. A method for preparing silver powder with a high twinning ratio, characterized in that: The following steps are involved: S1. A carboxylic acid ligand is added to the silver source solution to obtain a silver precursor solution; a dispersant and an initiator are sequentially added to the reducing agent solution to obtain a reaction bottom solution; S2. After adding a silver precursor solution to the reaction base liquid for redox reaction, the mixture was aged to obtain a mixed mother liquor; S3. The mixed mother liquor is filtered, washed, dispersed, and dried to obtain the high twin ratio silver powder; The initiator includes one or more of sulfate, carbonate and nitrate.
2. The method for preparing silver powder with a high twinning ratio according to claim 1, wherein: The mass ratio of the carboxylic acid ligand to the initiator is (0.2-0.5): (0.001-0.005).
3. The method for preparing silver powder with a high twinning ratio according to claim 1, wherein: The carboxylic acid ligand includes one or more of ethylenediaminetetraacetic acid, tartaric acid, tryptophan, tyrosine, and aspartic acid.
4. The method for preparing silver powder with a high twinning ratio according to claim 1, wherein: The initiator includes one or more of sodium sulfate, copper sulfate, potassium sulfate, magnesium sulfate, sodium bicarbonate, sodium carbonate, potassium carbonate, sodium nitrate, and potassium nitrate.
5. The method for preparing silver powder with a high twinning ratio according to claim 1, wherein: The dispersant includes one or more of polyvinyl pyrrolidone, gelatin, and polyethylene glycol; the mass ratio of the dispersant to the silver source is (0.08-0.2):
1.
6. The method for preparing silver powder with a high twinning ratio according to claim 1, wherein: The reducing agent includes one or more of ascorbic acid, glucose, and hydrazine hydrate; the mass ratio of the initiator, the reducing agent, and the silver source is (0.001-0.005): (0.6-2):
1.
7. The method for preparing silver powder with a high twinning ratio according to claim 1, wherein: The specific operation of step S2 is: in a non-stirring state, pouring the silver precursor solution into the reaction base solution within 10-30 seconds to carry out an oxidation-reduction reaction, and then standing and aging for 15-30 minutes to obtain a mixed mother solution.
8. The method for preparing silver powder with a high twinning ratio according to claim 1, wherein: In step S3, the mixed mother liquor is filtered and then washed with deionized water until the conductivity is ≤15 μs / cm to obtain a wet powder, which is then dispersed with an ethanol solution containing a coating agent, filtered and dried to obtain the high twin ratio silver powder.
9. A silver powder with a high twinning ratio obtained by the preparation method according to any one of claims 1 to 8, characterized in that: The twin ratio is 20-55%.
10. Use of the high twinning ratio silver powder according to claim 9 in preparing TOPCon conductive paste.
Citation Information
Patent Citations
A method for preparing spherical silver powder
CN114178543B
Cited By
Preparation method of nano silver powder with single particle dispersion
CN121223101A
A method for preparing a nano-silver powder with single particle dispersion
CN121223101B