Carbon dioxide absorbent and preparation method thereof

By combining modified mesoporous silica with diethylenetriamine and introducing polyamine groups, the problems of insufficient adsorption capacity and stability of existing carbon dioxide absorbers were solved, and efficient carbon dioxide capture was achieved.

CN120714587AActive Publication Date: 2025-09-30HEFEI ZHONGHAI LANHANG TECH CO LTD

Patent Information

Application Number
CN202511189293.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-08-25
Publication Date
2025-09-30
Estimated Expiration
2045-08-25

AI Technical Summary

Technical Problem

The mesoporous silica of existing carbon dioxide absorbers has a disordered pore structure, limited specific surface area, and a lack of functional groups on the surface, resulting in low amine loading, insufficient adsorption capacity and stability.

Method used

Modified mesoporous silica is combined with diethylenetriamine, and polyamine groups are introduced through chemical grafting to form amino clusters. The cage structure of the modified mesoporous silica provides high specific surface area and ordered pores, thereby enhancing the adsorption effect of carbon dioxide.

Benefits of technology

The adsorption capacity and stability of the carbon dioxide absorbent are improved, achieving efficient carbon dioxide capture capabilities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120714587A_ABST
    Figure CN120714587A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of carbon dioxide capture, and discloses a carbon dioxide absorbent and a preparation method thereof, and the carbon dioxide absorbent comprises the following components by weight: 10-15 parts of diethylenetriamine and 2-3 parts of modified mesoporous silica. According to the invention, through a synergistic adsorption mechanism of diethylenetriamine and modified mesoporous silica, a relatively good CO2 capture capability is realized; the cage-shaped structure of the modified mesoporous silica has a high specific surface area and ordered pore channels, and provides sufficient loading sites and diffusion channels for diethylenetriamine; meanwhile, an amino auxiliary (containing a plurality of primary amine and secondary amine groups) introduced in the modification process and a polyamine structure of diethylenetriamine form an amino cluster, and a better adsorption effect is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of carbon dioxide capture, and in particular to a carbon dioxide absorbent and a preparation method thereof. Background Art

[0002] In recent years, human society has experienced rapid industrialization. The use of large amounts of fossil fuels has resulted in the emission of large amounts of greenhouse gases such as carbon dioxide. Excessive greenhouse gases will create a greenhouse effect and subsequently trigger global warming, changing the ecological balance and threatening human survival. Carbon dioxide capture and storage technology is one of the key means to address global climate change, and has important applications in industrial flue gas treatment, natural gas purification, and confined space environmental control. At present, carbon dioxide absorbents are mainly divided into two categories: liquid absorbents (such as alcohol amines) and solid adsorbents (such as amine-functionalized mesoporous materials). However, existing technologies still have significant defects: the pore structure of ordinary mesoporous silica is disordered, the specific surface area is limited, and the surface lacks functional groups, making it difficult to form stable bonds with amine groups, resulting in low amine loading and limiting the increase in adsorption capacity; at the same time, the pores of non-cage structures are prone to collapse due to amine agglomeration, further reducing the stability of the material; therefore, how to avoid this phenomenon is the key to solving the problem. Summary of the Invention

[0003] (1) Technical problems solved In view of the deficiencies of the prior art, the present invention provides a carbon dioxide absorbent and a preparation method thereof, which has a good absorption effect on carbon dioxide.

[0004] (2) Technical solution To achieve the above object, the present invention provides the following technical solution: a carbon dioxide absorbent comprising the following components by weight: 10-15 parts by weight of diethylenetriamine and 2-3 parts by weight of modified mesoporous silica.

[0005] Furthermore, the preparation method of the modified mesoporous silica is: S1. Under a nitrogen atmosphere, 5-6 g of glycidyl methacrylate, 4.3-5 g of itaconic acid, 0.10-0.11 g of triphenylphosphine, and 0.052-0.055 g of 4-methoxyphenol were added to a reactor. The reactor was placed in an oil bath and the temperature was raised for 1-1.5 h. After completion, the crude product was vacuum distilled at 85-90°C for 0.8-1 h to obtain alkenyl intermediate 1. S2. Diethanolamine and alkenyl intermediate 1 were added to N,N-dimethylformamide solvent, stirred and mixed, and p-toluenesulfonic acid catalyst was added thereto. The reaction was carried out at 85-90 ° C for 6-7h. After the reaction, the mixture was distilled under reduced pressure, washed, and dried to obtain intermediate 2; S3. To 40-50mL of N,N-dimethylformamide solvent was added 4.5-6.3mml of intermediate 2, stirred and dispersed, and then 18-25.2mmol of mercaptoethylamine and 0.2-0.3mmol of benzoin dimethyl ether photoinitiator were added thereto, and irradiated with ultraviolet light at 365nm at 20-30°C, and then centrifuged, washed and dried to obtain an amino auxiliary agent; S4. Add the amino auxiliary agent to anhydrous ethanol, stir and dissolve at room temperature, then add cage-type mesoporous silica molecular sieve, continue stirring, and dry at 70-80°C to obtain modified mesoporous silica.

[0006] Furthermore, the temperature of the temperature-raising reaction in S1 is 80-90°C.

[0007] Furthermore, the usage ratio of diethanolamine, alkenyl intermediate 1, N,N-dimethylformamide, and p-toluenesulfonic acid catalyst in S2 is 3-5 mmol: 6-10 mmol: 50-60 mL: 0.1-0.2 mmol.

[0008] Furthermore, the ultraviolet light irradiation time in S3 is 2-2.5h.

[0009] Furthermore, the usage ratio of the amino auxiliary agent, anhydrous ethanol, and cage-type mesoporous silica molecular sieve in S4 is 3-5 mmol: 20-30 mL: 1-1.3 g.

[0010] Furthermore, the drying time in S4 is 20-24 hours.

[0011] Furthermore, the preparation method of the carbon dioxide absorbent is: adding diethylenetriamine and modified mesoporous silica into a stirrer, stirring for 10-16 minutes, drying, and then taking out and pressing into tablets at 5-6 MPa to obtain the carbon dioxide absorbent.

[0012] (3) Beneficial technical effects In the above reaction process, the epoxy group in glycidyl methacrylate and one end carboxyl group in itaconic acid undergo a ring-opening reaction to generate a hydroxyl group, and at the same time, an alkenyl group and a carboxyl group are introduced to obtain an alkenyl intermediate 1; the dihydroxyl group in diethanolamine and the carboxyl group in the alkenyl intermediate 1 undergo an esterification reaction (increasing the degree of substitution of the alkenyl and hydroxyl groups) to obtain intermediate 2; the alkenyl group in intermediate 2 and the thiol group in mercaptoethylamine undergo a click reaction to introduce an amino group to obtain an amino auxiliary agent; the amino auxiliary agent and cage-type mesoporous silica are stirred and blended to obtain modified mesoporous silica.

[0013] The present invention achieves superior CO2 capture capacity through a synergistic adsorption mechanism between diethylenetriamine and modified mesoporous silica. The cage-like structure of the modified mesoporous silica possesses a high specific surface area and ordered pores, providing ample loading sites and diffusion channels for diethylenetriamine. Furthermore, the amino-based additive (containing multiple primary and secondary amine groups) introduced during the modification process forms an "amine cluster" with the polyamine structure of diethylenetriamine, resulting in superior adsorption. A click reaction between the alkenyl groups in intermediate 2 and the thiol groups in mercaptoethylamine introduces a large number of amino groups, increasing the degree of substitution and enhancing carbon dioxide absorption. During the synthesis of the modified mesoporous silica, the alkenyl groups in intermediate 2 are chemically grafted onto the amine groups in mercaptoethylamine, forming a covalent bond that secures the amino-based additive within the cage-like pores. Furthermore, the spatial confinement of the cage-like pores inhibits amine molecule aggregation, resulting in enhanced carbon dioxide absorption. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 is the reaction formula of intermediate 2. DETAILED DESCRIPTION

[0015] To make the objectives, technical solutions, and advantages of the embodiments of the present invention more clear, the technical solutions in the embodiments of the present invention are clearly and completely described. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. All other embodiments derived by persons of ordinary skill in the art based on the embodiments of the present invention without inventive effort are within the scope of protection of the present invention.

[0016] In order to better understand the above technical solution, the above technical solution will be described in detail below with reference to the accompanying drawings and specific embodiments.

[0017] The preparation method for cage-type mesoporous silica molecular sieves is as follows: Referring to the literature "Preparation, Characterization, and Carbon Dioxide Adsorption Behavior of Polyethyleneimine-Modified Cage-Type Mesoporous Molecular Sieves," 0.5 g of triblock copolymer (polyoxyethylene-polyoxypropylene-polyoxyethylene copolymer), 0.6 g of trimethylbenzene, and 2.5 g of KCl were dissolved in 30 mL of 2 mol / L HCl and stirred at 15°C for 2 hours. 2.08 g of tetraethoxysilane was then added and stirred for a further 24 hours. The reaction mixture was transferred to a reactor and reacted at 100°C for 24 hours. The resulting reaction product was cooled, filtered, washed with water, and dried at room temperature. Finally, the organic template was removed by sintering at 550°C for 6 hours to obtain the cage-type mesoporous silica molecular sieve.

[0018] Example 1 S1. Under a nitrogen atmosphere, 5 g of glycidyl methacrylate, 4.3 g of itaconic acid, 0.10 g of triphenylphosphine, and 0.052 g of 4-methoxyphenol were added to a reactor. The reactor was placed in an oil bath and heated to 80°C for 1 h. After reaction, the crude product was vacuum distilled at 85°C for 0.8 h to obtain alkenyl intermediate 1. S2. 3 mmol of diethanolamine and 6 mmol of alkenyl intermediate 1 were added to 50 mL of N,N-dimethylformamide solvent, stirred and mixed, and 0.1 mmol of p-toluenesulfonic acid catalyst was added thereto. The reaction was carried out at 85°C for 6 h. After the reaction, the reaction was carried out by vacuum distillation, washed, and dried to obtain intermediate 2. S3. To 40 mL of N, N-dimethylformamide solvent was added 4.5 mml of intermediate 2, stirred and dispersed, and then 18 mmol of mercaptoethylamine and 0.2 mmol of benzoin dimethyl ether photoinitiator were added thereto. The mixture was irradiated with ultraviolet light at 365 nm for 2 h at 20 ° C. After the mixture was centrifuged, washed and dried to obtain an amino auxiliary agent. S4. Add 3 mmol of the amino additive to 20 mL of anhydrous ethanol and stir at room temperature to dissolve. Then add 1 g of cage-type mesoporous silica and continue stirring. Dry at 70°C for 20 h to obtain modified mesoporous silica. S5. 10 parts by weight of diethylenetriamine and 2 parts by weight of modified mesoporous silica were added to a blender, stirred for 10 min, dried, and then taken out and pressed under 5 MPa to obtain a carbon dioxide absorbent.

[0019] Example 2 S1. Under a nitrogen atmosphere, 6 g of glycidyl methacrylate, 5 g of itaconic acid, 0.11 g of triphenylphosphine, and 0.055 g of 4-methoxyphenol were added to a reactor. The reactor was placed in an oil bath and heated to 90°C for 1.5 h. After reaction, the crude product was vacuum distilled at 90°C for 1 h to obtain alkenyl intermediate 1. S2. 5 mmol of diethanolamine and 10 mmol of the alkenyl intermediate 1 were added to 60 mL of N,N-dimethylformamide solvent, stirred and mixed, and 0.2 mmol of p-toluenesulfonic acid catalyst was added thereto. The reaction was carried out at 90°C for 7 h. After the reaction, the reaction was carried out under reduced pressure distillation, washed, and dried to obtain intermediate 2; S3. To 50 mL of N, N-dimethylformamide solvent was added 6.3 mml of intermediate 2, stirred and dispersed, and then 25.2 mmol of mercaptoethylamine and 0.3 mmol of benzoin dimethyl ether photoinitiator were added thereto. The mixture was irradiated with ultraviolet light at 365 nm for 2.5 h at 30 ° C. After the reaction, the mixture was centrifuged, washed and dried to obtain an amino auxiliary agent. S4. 5 mmol of the amino additive was added to 30 mL of anhydrous ethanol and stirred at room temperature to dissolve. 1.3 g of cage-type mesoporous silica was then added and stirred continuously. The mixture was dried at 80 ° C for 24 h to obtain modified mesoporous silica. S5. 15 parts by weight of diethylenetriamine and 3 parts by weight of modified mesoporous silica were added to a blender, stirred for 16 minutes, dried, and then taken out and pressed at 6 MPa to obtain a carbon dioxide absorbent.

[0020] Example 3 S1. Under a nitrogen atmosphere, 5.5 g of glycidyl methacrylate, 4.7 g of itaconic acid, 0.10 g of triphenylphosphine, and 0.053 g of 4-methoxyphenol were added to a reactor. The reactor was placed in an oil bath and heated to 85°C for 1.2 h. After reaction, the crude product was vacuum distilled at 87°C for 0.9 h to obtain alkenyl intermediate 1. S2. 4 mmol of diethanolamine and 8 mmol of alkenyl intermediate 1 were added to 55 mL of N,N-dimethylformamide solvent, stirred and mixed, and 0.15 mmol of p-toluenesulfonic acid catalyst was added thereto. The reaction was carried out at 87°C for 6.5 h. After the reaction, the reaction was carried out by vacuum distillation, washed, and dried to obtain intermediate 2. S3. To 46 mL of N,N-dimethylformamide solvent was added 5.3 mml of intermediate 2, stirred and dispersed, and then 21.6 mmol of mercaptoethylamine and 0.25 mmol of benzoin dimethyl ether photoinitiator were added thereto. The mixture was irradiated with ultraviolet light at 365 nm for 2.2 h at 26 ° C. After the reaction, the mixture was centrifuged, washed and dried to obtain an amino auxiliary agent. S4. 4 mmol of the amino additive was added to 25 mL of anhydrous ethanol and stirred at room temperature to dissolve. 1.2 g of cage-type mesoporous silica was then added and stirred continuously. The mixture was dried at 75°C for 22 h to obtain modified mesoporous silica. S5. 13 parts by weight of diethylenetriamine and 2.5 parts by weight of modified mesoporous silica were added to a blender, stirred for 13 minutes, dried, and then taken out and pressed at 5 MPa to obtain a carbon dioxide absorbent.

[0021] Example 4 S1. Under a nitrogen atmosphere, 5 g of glycidyl methacrylate, 4.3 g of itaconic acid, 0.10 g of triphenylphosphine, and 0.052 g of 4-methoxyphenol were added to a reactor. The reactor was placed in an oil bath and heated to 80°C for 1 h. After reaction, the crude product was vacuum distilled at 85°C for 0.8 h to obtain alkenyl intermediate 1. S2. 3 mmol of diethanolamine and 6 mmol of alkenyl intermediate 1 were added to 50 mL of N,N-dimethylformamide solvent, stirred and mixed, and 0.1 mmol of p-toluenesulfonic acid catalyst was added thereto. The reaction was carried out at 85°C for 6 h. After the reaction, the reaction was carried out by vacuum distillation, washed, and dried to obtain intermediate 2. S3. To 50 mL of N, N-dimethylformamide solvent was added 6.3 mml of intermediate 2, stirred and dispersed, and then 25.2 mmol of mercaptoethylamine and 0.3 mmol of benzoin dimethyl ether photoinitiator were added thereto. The mixture was irradiated with ultraviolet light at 365 nm for 2.5 h at 30 ° C. After the reaction, the mixture was centrifuged, washed and dried to obtain an amino auxiliary agent. S4. 4 mmol of the amino additive was added to 25 mL of anhydrous ethanol and stirred at room temperature to dissolve. 1.2 g of cage-type mesoporous silica was then added and stirred continuously. The mixture was dried at 75°C for 22 h to obtain modified mesoporous silica. S5. 13 parts by weight of diethylenetriamine and 2.5 parts by weight of modified mesoporous silica were added to a blender, stirred for 13 minutes, dried, and then taken out and pressed at 5 MPa to obtain a carbon dioxide absorbent.

[0022] Example 5 S1. Under a nitrogen atmosphere, 6 g of glycidyl methacrylate, 5 g of itaconic acid, 0.11 g of triphenylphosphine, and 0.055 g of 4-methoxyphenol were added to a reactor. The reactor was placed in an oil bath and heated to 90°C for 1.5 h. After reaction, the crude product was vacuum distilled at 90°C for 1 h to obtain alkenyl intermediate 1. S2. 5 mmol of diethanolamine and 10 mmol of the alkenyl intermediate 1 were added to 60 mL of N,N-dimethylformamide solvent, stirred and mixed, and 0.2 mmol of p-toluenesulfonic acid catalyst was added thereto. The reaction was carried out at 90°C for 7 h. After the reaction, the reaction was carried out under reduced pressure distillation, washed, and dried to obtain intermediate 2; S3. To 46 mL of N,N-dimethylformamide solvent was added 5.3 mml of intermediate 2, stirred and dispersed, and then 21.6 mmol of mercaptoethylamine and 0.25 mmol of benzoin dimethyl ether photoinitiator were added thereto. The mixture was irradiated with ultraviolet light at 365 nm for 2.2 h at 26 ° C. After the reaction, the mixture was centrifuged, washed and dried to obtain an amino auxiliary agent. S4. Add 3 mmol of the amino additive to 20 mL of anhydrous ethanol and stir at room temperature to dissolve. Then add 1 g of cage-type mesoporous silica and continue stirring. Dry at 70°C for 20 h to obtain modified mesoporous silica. S5. 10 parts by weight of diethylenetriamine and 2 parts by weight of modified mesoporous silica were added to a blender, stirred for 10 min, dried, and then taken out and pressed under 5 MPa to obtain a carbon dioxide absorbent.

[0023] Comparative Example 1 Compared with Example 5, this comparative example differs in that Intermediate 2 is used instead of modified mesoporous silica.

[0024] Comparative Example 2 Compared with Example 5, this comparative example differs in that cage-type mesoporous silica is used instead of modified mesoporous silica.

[0025] Performance Testing The performance of the carbon dioxide absorbents prepared in Examples 1-5 and Comparative Examples 1-2 was tested. The testing method included the following steps: placing 20 mg of carbon dioxide absorbent supported by quartz wool in the constant temperature heating zone of a fixed bed reactor, introducing CO2 (50 mL / min) gas at room temperature to adsorb it, and testing it with an online gas analyzer. After the carbon dioxide absorbent was saturated with adsorption (adsorption time was 30 min), the carbon dioxide adsorption amount was calculated.

[0026] Table 1: Carbon dioxide adsorption test.

[0027]

[0028] As can be seen from Table 1, Examples 1-5 of the present invention have better adsorption effects than Comparative Examples 1-2.

[0029] The process of rapidly preparing high-performance carbon capture membranes in batches by combining carbon dioxide adsorbents with membrane materials is as follows: First, the adsorbent is selected according to the parameters in Examples 1-5; Next, MOF-808 was selected as the inorganic filler for membrane preparation due to its pore size (approximately 1.8 nm) suitable for CO2 molecules and its abundant unsaturated metal sites, which are beneficial for improving the membrane's CO2 permeability and selectivity. To shorten the MOF synthesis cycle and obtain uniformly sized nanoparticles, microwave heating was used instead of traditional hydrothermal synthesis, leveraging the rapid and uniform heating properties of microwaves to complete MOF crystal growth in a short period of time. Simultaneously, a silane coupling agent (KH-560) and polyethyleneimine (PEI) were introduced to modify the MOF surface, aiming to improve the dispersion of the MOF particles in the polymer and increase their chemical affinity for CO2.

[0030] Microwave Synthesis of MOF-808: MOF-808 nanoparticles were rapidly synthesized using a microwave-assisted method. The specific steps are as follows: a zirconium source (e.g., ZrOCl2·8H2O) was dissolved in a mixture of N,N-dimethylformamide (DMF) and formic acid (volume ratio approximately 1:1). The organic ligand, trimesic acid (H3BTC), was added in a stoichiometric ratio (Zr:trimesic acid ≈ 3:1). Stirring was performed at room temperature for 10–20 minutes to form a clear, transparent precursor solution. The solution was then transferred to a polytetrafluoroethylene-lined microwave reactor (filling level not exceeding 60%), sealed, and placed in the microwave reactor. Heating was performed using a 2.45 GHz single-mode microwave with the following power-time program: the temperature was increased to 120°C over 2 minutes at 600 W, then maintained at 120°C for 10 minutes at 400 W. The microwave was then turned off and allowed to cool naturally to below 60°C. The total reaction time was approximately 25 minutes. The resulting white precipitate was centrifuged and washed twice with DMF and twice with anhydrous ethanol to remove unreacted ligands and zirconium salts. The product was then vacuum-dried at 80°C for 4 hours to obtain MOF-808 nanopowder. X-ray diffraction (XRD) and scanning electron microscopy (SEM) were used to characterize the product and confirm its crystal structure and particle size distribution. The microwave-synthesized MOF-808 exhibited a typical crystal structure with uniform particle sizes of approximately 50–80 nm, significantly reducing the preparation time compared to the traditional hydrothermal method, which requires over 24 hours.

[0031] Microwave-assisted rapid synthesis of MOF-808 nanoparticles Surface Functionalization of MOF-808: To improve the dispersibility of MOF in polymers and enhance its CO2 adsorption capacity, MOF-808 was surface functionalized. MOF-808 nanoparticles were dispersed in deionized water. A silane coupling agent, KH-560 (γ-glycidoxypropyltrimethoxysilane), and polyethyleneimine (PEI) were added. The concentrations of KH-560 and PEI ranged from 4.17 to 13.6 g / L and 0.91 to 1.67 g / L, respectively. The mixture was stirred at 80°C for 12 hours. The silane coupling agent hydrolyzed and bonded to the hydroxyl groups on the MOF surface, while the PEI adhered to the MOF surface through electrostatic or covalent bonds. After the reaction, the particles were centrifuged and washed several times with deionized water to remove unreacted reagents. The mixture was then dried in a vacuum oven at 80°C. The modified MOF-808 surface is grafted with amino and epoxy groups, which not only improves the compatibility with the polymer matrix, but also increases the chemical affinity sites for CO2, which is beneficial to improving the CO2 selectivity of the membrane.

[0032] Coating solution preparation and composite membrane fabrication: Surface-functionalized MOF-808 and PEI were mixed in a mass ratio of 1:5, and an appropriate amount of deionized water was added to prepare a coating solution with a solids content of 0.25% to 1.0% (mass fraction). This low-solids formulation facilitates the formation of a uniform, ultrathin liquid film during ultrasonic spraying and reduces material waste. During spraying, parameters such as nozzle-to-substrate distance, spraying speed, and solution flow rate were controlled to achieve a wet film thickness of approximately 70–100 μm. After spraying, the membrane was dried at room temperature for 2 hours to evaporate the solvent and form a dense MOF / PEI composite selective layer. The resulting composite membrane is the carbon capture membrane.

[0033] It should be noted that, in this document, the terms "comprise," "include," or any other variations thereof are intended to encompass non-exclusive inclusion, such that a process, method, article, or apparatus comprising a series of elements includes not only those elements but also other elements not explicitly listed, or elements inherent to such process, method, article, or apparatus. In the absence of further limitations, an element defined by the phrase "comprises a ..." does not preclude the presence of other identical elements in the process, method, article, or apparatus comprising the element.

[0034] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the various embodiments of the present invention.

[0035] Those skilled in the art should understand that the above descriptions are only some specific embodiments of the present invention, rather than all embodiments.

Claims

1. A carbon dioxide absorbent, characterized in that The invention comprises the following components by weight: 10-15 parts by weight of diethylenetriamine and 2-3 parts by weight of modified mesoporous silica.

2. The carbon dioxide absorbent according to claim 1, characterized in that The preparation method of the modified mesoporous silica is: S1. Under a nitrogen atmosphere, 5-6 g of glycidyl methacrylate, 4.3-5 g of itaconic acid, 0.10-0.11 g of triphenylphosphine, and 0.052-0.055 g of 4-methoxyphenol were added to a reactor. The reactor was placed in an oil bath and the temperature was raised for 1-1.5 h. After completion, the crude product was vacuum distilled at 85-90°C for 0.8-1 h to obtain alkenyl intermediate 1. S2. Diethanolamine and alkenyl intermediate 1 were added to N,N-dimethylformamide solvent, stirred and mixed, and p-toluenesulfonic acid catalyst was added thereto. The reaction was carried out at 85-90 ° C for 6-7h. After the reaction, the mixture was distilled under reduced pressure, washed, and dried to obtain intermediate 2; S3. To 40-50mL of N,N-dimethylformamide solvent was added 4.5-6.3mml of intermediate 2, stirred and dispersed, and then 18-25.2mmol of mercaptoethylamine and 0.2-0.3mmol of benzoin dimethyl ether photoinitiator were added thereto, and irradiated with ultraviolet light at 365nm at 20-30°C, and then centrifuged, washed and dried to obtain an amino auxiliary agent; S4. Add the amino auxiliary agent to anhydrous ethanol, stir and dissolve at room temperature, then add cage-type mesoporous silica molecular sieve, continue stirring, and dry at 70-80°C to obtain modified mesoporous silica.

3. The carbon dioxide absorbent according to claim 2, characterized in that The temperature of the reaction in S1 is 80-90°C.

4. The carbon dioxide absorbent according to claim 2, characterized in that The usage ratio of diethanolamine, alkenyl intermediate 1, N,N-dimethylformamide, and p-toluenesulfonic acid catalyst in S2 is 3-5 mmol: 6-10 mmol: 50-60 mL: 0.1-0.2 mmol.

5. The carbon dioxide absorbent according to claim 2, characterized in that The ultraviolet light irradiation time in S3 is 2-2.5h.

6. The carbon dioxide absorbent according to claim 2, characterized in that The usage ratio of the amino auxiliary agent, anhydrous ethanol, and cage-type mesoporous silica molecular sieve in the S4 is 3-5 mmol: 20-30 mL: 1-1.3 g.

7. The carbon dioxide absorbent according to claim 1, characterized in that The drying time in S4 is 20-24 hours.

8. A method for preparing the carbon dioxide absorbent according to any one of claims 1 to 7, characterized in that: The preparation method of the carbon dioxide absorbent comprises the following steps: adding diethylenetriamine and modified mesoporous silica into a stirrer, stirring for 10-16 minutes, drying, and then taking out and pressing into tablets at 5-6 MPa to obtain the carbon dioxide absorbent.

Citation Information

Patent Citations

  • Modified mesoporous silica material based on mixed mode, preparation method and application thereof

    CN115254008A

  • Flexible floating roof assembly for demineralized water tank and carbon dioxide isolation device

    CN117902178A

  • Polyamine type porous polymer as well as preparation method and application thereof

    CN120441796A

  • Hierarchically porous amine-silica monolith and preparation method thereof

    US20150251160A1

Cited By

  • Organic amine absorbent suitable for cement kiln flue gas carbon capture and preparation method and application thereof

    CN121695641A

  • Organic amine absorbent suitable for carbon capture from cement kiln flue gas and preparation method and application thereof