Method for improving illumination stability of perovskite through post-treatment and application

By low-temperature calcination and grinding with post-processing additives, a passivation layer is formed to eliminate the photoinduced defects of perovskite nanocrystals, solving the stability problem of high-temperature solid-state synthesized perovskite luminescent bodies under light, and realizing its wide applicability in light-stimulated applications.

CN120718648APending Publication Date: 2025-09-30INST OF WENZHOU ZHEJIANG UNIV +1

Patent Information

Application Number
CN202410367506.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-03-28
Publication Date
2025-09-30

AI Technical Summary

Technical Problem

High-temperature solid-state synthesized perovskite light emitters are prone to irreversible photoinduced defects when exposed to strong external light, limiting their development in application areas that require light excitation.

Method used

The perovskite nanocrystal precursor is mixed with the micro/mesoporous template by calcining below the collapse temperature of the micro/mesoporous template, grinding the additives and annealing under light to form a passivation layer to eliminate photoinduced defects.

Benefits of technology

The photostability of perovskite light emitters has been improved, making them resistant to water, oxygen, heat and light-induced defects, making them suitable for applications such as LEDs and light conversion coatings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004764637320000121
    Figure BDA0004764637320000121
Patent Text Reader

Abstract

The invention provides a method for improving the illumination stability of perovskite through post-treatment. The method comprises the following steps: S1, preparing a perovskite illuminant; s2, grinding and diffusing; and S3, inducing exposure and passivation of photoinduced defects. According to the invention, the light stability of the perovskite illuminant synthesized in a temperature solid state can be improved, so that the perovskite illuminant is applicable to wider application fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of post-processing of perovskite luminous bodies, and in particular relates to a method and application for improving the light stability of perovskite through post-processing. Background Art

[0002] Metal halide perovskite (hereinafter referred to as perovskite) luminescent materials are a new type of luminescent material. They have excellent luminous efficiency, narrow emission half-width, high color purity, and tunable visible light bands. They are also simple to prepare, low-cost, and easily scalable. They are expected to become key luminescent layer materials in future displays and have broad application prospects in light-emitting diodes (LEDs), solar cells, lasers, and other fields. However, because perovskite is an ionic compound with a soft lattice, high humidity, high temperature, and strong light exposure in the external environment can easily induce perovskite defects, thereby impairing its luminescent properties.

[0003] High-temperature solid-state synthesis methods are commonly used to prepare perovskite emitters, offering advantages such as suitability for large-scale synthesis, high controllability, and a simple process. Perovskite emitters obtained through high-temperature solid-state synthesis exhibit a certain degree of resistance to water, oxygen, and high temperatures. For example, our company's prior Chinese patent application, published as CN116752116A, discloses a method for growing halide perovskite nanocrystals via in situ chemical vapor deposition. This high-temperature solid-state synthesis method primarily involves two steps: 1) mixing a perovskite precursor with a micro / mesoporous template; and 2) calcining the precursor mixture, which reacts and melts the perovskite precursor at high temperatures and then supercools and crystallizes within the micro / mesoporous template to form perovskite nanocrystals. Due to the encapsulation of the micro / mesoporous template, these perovskite nanocrystals are shielded from water, oxygen, and external heat, demonstrating stability against water and high temperatures. However, exposure to strong external light can still easily cause irreversible photoinduced defects in these perovskite nanocrystals, hindering the further development of perovskite emitters in applications requiring external light excitation, such as LEDs and light-conversion coatings.

[0004] Therefore, it is necessary to develop a post-processing technology to improve the photostability of warm solid-state synthesized perovskite light-emitting bodies so that they can be used in a wider range of applications. Summary of the Invention

[0005] The present invention aims to address the problems and shortcomings of the prior art and provide a method and application for improving the light stability of perovskite through post-processing.

[0006] To achieve the above objectives, the present invention adopts a technical solution: a method for improving the light stability of perovskite by post-processing, comprising the following steps:

[0007] S1. Preparation of perovskite light emitter:

[0008] Mixing a perovskite nanocrystal precursor and a micro / mesoporous template to obtain a mixture; calcining the mixture at a temperature lower than the collapse temperature of the micro / mesoporous template to generate perovskite nanocrystals in the pores of the micro / mesoporous template;

[0009] S2, grinding and diffusion;

[0010] The perovskite light emitting body prepared in step S1 is mixed with a post-treatment additive, and subjected to a grinding process, so that part of the post-treatment additive is accumulated in the pores of the micro / mesoporous template through grinding diffusion, thereby obtaining a post-treatment mixed powder;

[0011] S3. Exposure and passivation of photoinduced defects:

[0012] The post-processed mixed powder obtained in step S2 is annealed under light, wherein the photon energy of the light is greater than the energy corresponding to the band gap width of the perovskite nanocrystal, thereby causing the perovskite nanocrystal to reach an excited state to generate photoinduced defects; the annealing temperature is 100-300°C to promote the reaction between the post-processing additive and the perovskite nanocrystal to form a passivation layer to eliminate the photoinduced defects of the perovskite nanocrystal.

[0013] By adopting the above technical solution, the calcination temperature in step S1 must be below the pore collapse temperature of the micro / mesoporous template. The high-temperature calcination process decomposes the perovskite precursor and forms perovskite nanocrystals within the pores of the micro / mesoporous template, but the calcination temperature does not cause the pores to collapse. Therefore, the coating structure still retains the nanopores of the micro / mesoporous template, providing a mass transfer path for additives during post-processing.

[0014] During the grinding process in step S2, the impact of grinding can force the post-treatment additive into the micropores of the template, allowing it to come into contact with the surface of the perovskite nanocrystals. The localized high temperatures generated by the friction during grinding promote the diffusion and reaction of the post-treatment additive on the surface of the perovskite light emitter.

[0015] In step S3, the energy of the applied light photons must be greater than the energy corresponding to the perovskite band gap width, thereby causing the perovskite to reach an excited state. Under illumination, the perovskite will produce photoinduced defects. The relationship between photon energy and wavelength can be expressed as follows: energy (eV) = 1240 / wavelength (nm).

[0016] Take the CsPbBr3 perovskite structure with a wavelength of 530nm as an example. The energy corresponding to the band gap width of CsPbBr3 is about 2.3eV, so the photon energy of the illumination must be greater than 2.3eV. It should be noted that: as shown in the above formula, due to the different emission wavelengths of different perovskite structures, there are different energies corresponding to the perovskite band gap widths. Therefore, the technical concept of the present invention also covers CsPb I3, CsPbBr y I3-y and other metal halide perovskite structures.

[0017] Furthermore, the annealing temperature is maintained in the range of 100-300°C to encourage the post-treatment additives to react with the perovskite, forming a passivation layer to eliminate the perovskite defects generated by the exposure of photoinduced defects. The technical essence of the present invention lies in first inducing photoinduced defects and then passivating them to overcome the defects.

[0018] Furthermore, the perovskite nanocrystal precursor includes a CsPbX3 perovskite structure precursor, where X is at least one of Br, Cl, and I. For example, CsPbBr3, CsPb I3, CsPbBr y I 3-y Perovskite structure.

[0019] Furthermore, the CsPbX3 perovskite nanocrystal precursor is composed of a Cs source precursor, a Pb source precursor and a halogen source precursor;

[0020] Wherein: the Cs source precursor includes one or more of cesium halide and cesium carbonate;

[0021] The Pb source precursor includes one or more of lead halide and lead acetate;

[0022] The halogen source precursor includes one or more of cesium halide, lead halide, zinc halide, potassium halide, sodium halide, lithium halide, ammonia halide, calcium halide, strontium halide, and barium halide.

[0023] Furthermore, the micro / mesoporous template is a microporous material and / or a mesoporous material, specifically a type of micro / mesoporous inorganic material with nano-space pores;

[0024] The microporous material is a microporous molecular sieve, microporous silica, microporous titania, microporous alumina, microporous transition metal oxide, microporous sulfide, microporous silicate, microporous aluminate or microporous transition metal nitride;

[0025] The mesoporous material is mesoporous molecular sieve, mesoporous silica, mesoporous titania, mesoporous alumina, mesoporous carbon, mesoporous transition metal oxide, mesoporous sulfide, mesoporous silicate, mesoporous aluminate or mesoporous transition metal nitride.

[0026] Furthermore, the calcination temperature of the perovskite nanocrystal precursor and the micro / mesoporous template is less than 600° C. to prevent the pore structure of the micro / mesoporous template from collapsing.

[0027] In the process of preparing perovskite nanocrystalline materials, the maximum calcination temperature used in the present invention is preferably such as to ensure that the pores of the micro / mesoporous material do not collapse. However, the collapse temperatures of different micro / mesoporous materials are different, and the collapse temperatures of the same material with different structures are also different, but it can be determined that in order to achieve better results, the calcination temperature must not be higher than the lowest collapse temperature of the material. For example, in the micro / mesoporous material exemplified above, the collapse temperature is at least 300°C. In practice, generally speaking, 300 to 2000°C can ensure that most commonly used micro / mesoporous materials collapse. For example, mesoporous silica (such as MCM-41) collapses at 600°C, mesoporous titanium dioxide begins to collapse at 800°C, and so on.

[0028] In addition, the “calcination under conditions lower than the collapse temperature of the micro / mesoporous template” defined in the present invention should also include the use scenario of using a flux. For example, the Chinese patent application number ZL202211559323.5 also introduces a mesoporous material collapse agent in an attempt to lower the collapse temperature of the micro / mesoporous material and achieve size control of the perovskite nanocrystals by avoiding agglomeration. It should be pointed out that even if a flux or collapse agent is added, the calcination temperature of the present application in the preparation of perovskite nanocrystals still needs to be “calcined under conditions lower than the collapse temperature of the micro / mesoporous template” to retain the existence of the pores.

[0029] Furthermore, the post-treatment additive includes one of fluoride, phosphate, pyrophosphate, and pyrosulfate.

[0030] Furthermore, the fluoride is selected from NH4F, NH4HF2, KF, CsF, NaF, NaAlF6, AlFK, KBF4, KALF4, (C3F 60 )xC5F 120 、CrF3、C8F 18 , CeF3, SnF2, F4V, F4T i, BeF2, KPF6 and combinations thereof;

[0031] Phosphate selected from Bo4P, KPO3, Na5P3O 10 , Ba3(PO4)2, Ba(H2PO4)2, Ca(H2PO4)2, K3PO4, Na3PO4, (NaPO3) n , KPF6, NH4H2PO4, (NH4)2HPO4, Ca(H2PO4)2, KH2PO4, K2HPO4, K5O 10 P3, Na2HPO4, Na5P3O 10 , NaH2PO2, MgHPO4, Mg3(PO4)2, Al Na3(PO4)2, CaHPO4 and combinations thereof;

[0032] The pyrophosphate is selected from the group consisting of K4P2O7, Sn2P2O7, Ca2P2O7, Na4P2O7, Fe4(P2O7)3, Na8Fe4(P2O7)5·xH2O, Mg2P2O7, Cu2P2O7, and combinations thereof;

[0033] The pyrosulfate salt is selected from the group consisting of Na2S2O7, K2S2O7, H8N2O7S2 and combinations thereof.

[0034] By adopting the above scheme, anions such as phosphate ions, pyrophosphate ions, pyrosulfate ions, and fluoride ions can bond with unpaired Pb2+ ions on the perovskite surface, thereby passivating the surface defects of the perovskite.

[0035] Furthermore, the grinding process in step S2 includes wet grinding and dry grinding, wherein the dry grinding is ball milling. Preferably, since the grinding balls have a better impact, the post-treatment additives can be promoted to enter the micropores of the template, thereby achieving a better grinding and diffusion effect.

[0036] Furthermore, the annealing under light in step S3 includes the following two situations:

[0037] A1: First light exposure, then annealing to form a passivation layer;

[0038] A2: Exposure of defects by light and annealing to form a passivation layer are carried out simultaneously.

[0039] A perovskite luminescent body with light stability is prepared by the above method.

[0040] The beneficial effects of the present invention are mainly reflected in:

[0041] 1. This invention provides a post-processing technology to enhance the photostability of high-temperature, solid-state synthesized perovskite luminescent materials. Compared to existing high-temperature, solid-state synthesized perovskite luminescent materials, this post-processing technology not only makes these perovskite luminescent materials resistant to water, oxygen, and heat, but also further resists the formation of light-induced defects. This post-processing technology makes perovskite luminescent materials promising for applications requiring external light excitation, such as LEDs and light-conversion coatings.

[0042] 2. This invention uses light to induce defects in perovskite nanocrystals, while post-treatment additives react with the perovskite nanocrystals to passivate the defects. During this process of defect generation and passivation, light-induced defects are eliminated, thereby improving the light stability of the perovskite. DETAILED DESCRIPTION

[0043] To make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0044] The "perovskite nanocrystals" and "perovskite luminescent materials" mentioned in the present invention both refer to the CsPbX3 perovskite structure. The perovskite luminescent material comprises a micro- / mesoporous template having pores for the embedding and growth of perovskite nanocrystals.

[0045] Example 1:

[0046] A method for improving the light stability of perovskite by post-processing, comprising the following steps:

[0047] Step 1: Cesium halide, lead halide and micro / mesoporous template (MCM-41 molecular sieve) are ball-milled for 2 h.

[0048] Step 2: Heat the mixed powder to 470°C, maintain for 120 minutes, and cool naturally.

[0049] Step 3: Weigh 2 g of the perovskite luminescent material obtained after calcination in step 2, add 0.1 g of KF, and ball mill at a speed of 230 r / min for 1 h.

[0050] Step 4: Weigh a certain amount of the perovskite light emitting body obtained after grinding in step 3 and place it on a heating table and heat it to 200 degrees Celsius. 2 The samples were irradiated with blue light (450nm) for 600 minutes and then cooled naturally.

[0051] In the above step 1, the cesium halide is cesium bromide, the lead halide is lead bromide, and the molar ratio of cesium bromide to lead bromide is 1:1.

[0052] Experimental Analysis: The sintered powder was tested for its fluorescence quantum yield (PLQY). As shown in Table 1, the PLQY for this sample was 90%. In comparison, the PLQY for the unpost-treated perovskite emitter (not subjected to Steps 3 and 4) provided in Comparative Example 1 was 55%. This improvement in PLQY demonstrates that post-treatment can passivate defects in the perovskite CsPbBr3 emitter.

[0053] The stability of the perovskite luminescent material obtained by the above post-treatment was tested under strong blue light irradiation environment. See Table 1 for details. 2After continuous irradiation with blue light (450nm) for 100 hours, the luminous intensity of the luminophore can maintain 80% of the original intensity. In comparison, the luminous intensity of the perovskite luminophore provided in Comparative Example 1, which has not undergone post-treatment, dropped to 30% of the initial intensity after 100 hours under the same blue light test conditions. The blue light stability proves that post-treatment is beneficial to improving the photostability of CsPbBr3 luminophores.

[0054] It should be noted that the methods for preparing perovskite light emitters in steps 1 and 2 above are prior art. Therefore, other details unrelated to the inventive aspects of the present invention will not be repeated here. For details, please refer to the following prior art: Our company's prior Chinese patent application, publication number CN116752116A, discloses a method for growing halide perovskite nanocrystals by in-situ chemical vapor deposition. Any modifications, supplements, or similar substitutions made by those skilled in the art within the scope of the principles of the present invention shall be included within the scope of protection of the present invention.

[0055] Example 2:

[0056] A method for improving the light stability of perovskite by post-processing, comprising the following steps:

[0057] Step 1: Cesium halide, lead halide and micro / mesoporous template (MCM-41 molecular sieve) are ball-milled for 2 h.

[0058] Step 2: Heat the mixed powder to 470°C, maintain for 120 minutes, and cool naturally.

[0059] Step 3: Weigh 2 g of the perovskite luminescent material obtained after calcination in step 2, add 2.84 g of potassium pyrophosphate, and ball mill at a speed of 230 r / min for 1 h.

[0060] Step 4: Weigh a certain amount of the perovskite light emitting body obtained after grinding in step 3 and place it on a heating table and heat it to 200 degrees Celsius. 2 The samples were irradiated with blue light (450nm) for 600 minutes and then cooled naturally.

[0061] In the above step 1, the cesium halide is cesium bromide, the lead halide is lead bromide, and the molar ratio of cesium bromide to lead bromide is 1:1.

[0062] Experimental Analysis: The sintered powder was tested for its fluorescence quantum yield (PLQY). As shown in Table 1, the PLQY for this sample was 96%. In comparison, the PLQY for the untreated perovskite emitter in Comparative Example 1 was 55%. This improvement in PLQY demonstrates that post-treatment can passivate defects in the perovskite CsPbBr3 emitter.

[0063] The stability of the perovskite luminescent material obtained by the above post-treatment was tested under strong blue light irradiation environment. See Table 1 for details. 2 After continuous irradiation with blue light (450nm) for 100 hours, the luminous intensity of the luminophore can maintain 84% of the original intensity. In comparison, the luminous intensity of the untreated perovskite luminophore provided in Comparative Example 1 dropped to 30% of the initial intensity after 100 hours under the same blue light test conditions. The blue light stability proves that post-treatment is beneficial to improving the photostability of CsPbBr3 luminophores.

[0064] Example 3:

[0065] A method for improving the light stability of perovskite by post-processing, comprising the following steps:

[0066] Step 1: Cesium halide, lead halide and micro / mesoporous template (MCM-41 molecular sieve) are ball-milled for 2 h.

[0067] Step 2: Heat the mixed powder to 470°C, maintain for 120 minutes, and cool naturally.

[0068] Step 3: Weigh 2 g of the perovskite luminescent material obtained after calcination in step 2, add 2.28 g of diammonium hydrogen phosphate, and ball mill at a speed of 230 r / min for 1 h.

[0069] Step 4: Weigh a certain amount of the perovskite light emitting body obtained after grinding in step 3 and place it on a heating table and heat it to 200 degrees Celsius. 2 The samples were irradiated with blue light (450nm) for 600 minutes and then cooled naturally.

[0070] In the above step 1, the cesium halide is cesium bromide, the lead halide is lead bromide, and the molar ratio of cesium bromide to lead bromide is 1:1.

[0071] Experimental Analysis: The sintered powder was tested for its fluorescence quantum yield (PLQY). As shown in Table 1, the PLQY for this sample was 92%. In comparison, the PLQY for the untreated perovskite emitter in Comparative Example 1 was 55%. This improvement in PLQY demonstrates that post-treatment can passivate defects in the perovskite CsPbBr3 emitter.

[0072] The stability of the perovskite luminescent material obtained by the above post-treatment was tested under strong blue light irradiation environment. See Table 1 for details. 2After 100 hours of continuous irradiation with blue light (450nm), the luminous intensity of the luminophore can maintain 83% of the original intensity. In comparison, the luminous intensity of the perovskite luminophore provided in Comparative Example 1, which has not undergone post-treatment, dropped to 30% of the initial intensity after 100 hours under the same blue light test conditions. The blue light stability proves that post-treatment is beneficial to improving the photostability of CsPbBr3 luminophores.

[0073] Example 4:

[0074] A method for improving the light stability of perovskite by post-processing, comprising the following steps:

[0075] Step 1: Cesium halide, lead halide and micro / mesoporous template (MCM-41 molecular sieve) are ball-milled for 2 h.

[0076] Step 2: Heat the mixed powder to 470°C, maintain for 120 minutes, and cool naturally.

[0077] Step 3: Weigh 2 g of the perovskite luminescent material obtained after calcination in step 2, add 2.19 g of potassium pyrosulfate, and ball mill at a speed of 230 r / min for 1 h.

[0078] Step 4: Weigh a certain amount of the perovskite light emitting body obtained after grinding in step 3 and place it on a heating table and heat it to 200 degrees Celsius. 2 The samples were irradiated with blue light (450nm) for 600 minutes and then cooled naturally.

[0079] In the above step 1, the cesium halide is cesium bromide, the lead halide is lead bromide, and the molar ratio of cesium bromide to lead bromide is 1:1.

[0080] Experimental Analysis: The sintered powder was tested for its fluorescence quantum yield (PLQY). As shown in Table 1, the PLQY for this sample was 88%. In comparison, the PLQY for the unpost-treated perovskite emitter in Comparative Example 1 was 55%. This improvement in PLQY demonstrates that post-treatment can passivate defects in the perovskite CsPbBr3 emitter.

[0081] The stability of the perovskite luminescent material obtained by the above post-treatment was tested under strong blue light irradiation environment. See Table 1 for details. 2 After 100 hours of continuous irradiation with blue light (450nm), the luminous intensity of the luminophore can maintain 76% of the original intensity. In comparison, the luminous intensity of the perovskite luminophore provided in Comparative Example 1, which has not undergone post-treatment, dropped to 30% of the initial intensity after 100 hours under the same blue light test conditions. The blue light stability proves that post-treatment is beneficial to improving the photostability of CsPbBr3 luminophores.

[0082] Example 5:

[0083] The difference from Example 1 is that the cesium bromide in step 1 is replaced with the same molar amount of cesium iodide, and the lead bromide is replaced with the same molar amount of lead iodide. This results in a CsPb I3 perovskite light emitter. Detailed experimental data is shown in Table 1.

[0084] Example 6:

[0085] The difference from Example 1 is that the cesium bromide in step 1 is replaced by a mixture A of cesium iodide and cesium bromide, and the total molar amount of the mixture A is the same as the molar amount of cesium bromide in Example 1;

[0086] Lead bromide is replaced by a mixture B of lead iodide and lead bromide, and the total molar amount of the mixture B is the same as the molar amount of lead bromide in Example 1; so that CsPbBr is prepared. y I 3-y Perovskite light emitter. Experimental data are shown in Table 1.

[0087] Comparative Example 1:

[0088] A method for improving the light stability of perovskite by post-processing, comprising the following steps:

[0089] Step 1: Grind and mix precursors such as cesium halide, lead halide, and micro / mesoporous template (MCM-41 molecular sieve).

[0090] Step 2: Heat the mixed powder to 470°C and maintain for 120 minutes, then cool naturally; allow the precursor to react in the MCM-41 molecular sieve to form a CsPbBr3 perovskite light emitter.

[0091] In the above step 1, the cesium halide is cesium bromide, the lead halide is lead bromide, and the molar ratio of cesium bromide to lead bromide is 1:1.

[0092] Experimental analysis: The powder obtained by sintering was taken to test the fluorescence quantum yield (PLQY). As shown in Table 1, the PLQY of the sample was 55%.

[0093] The stability of the perovskite luminescent material obtained above was tested under strong blue light irradiation environment. See Table 1 for details. 2 After continuous irradiation with blue light (450nm) for 100 hours, the luminous intensity of the luminophore can maintain 30% of the original intensity.

[0094] Comparative Example 2:

[0095] The difference from Comparative Example 1 is that the cesium bromide in step 1 is replaced with the same molar amount of cesium iodide, and the lead bromide is replaced with the same molar amount of lead iodide. This results in a CsPb I3 perovskite light emitter. Detailed experimental data is shown in Table 1.

[0096] Comparative Example 3:

[0097] The difference from Comparative Example 1 is that the cesium bromide in step 1 is replaced by a mixture C of cesium iodide and cesium bromide, and the total molar amount of the mixture C is the same as the molar amount of cesium bromide in Example 1;

[0098] Lead bromide is replaced by a mixture D of lead iodide and lead bromide, and the total molar amount of the mixture D is the same as the molar amount of lead bromide in Example 1; so that CsPbBr is prepared. y I 3-y Perovskite light emitter. Experimental data are shown in Table 1.

[0099] Explanation of the attached table:

[0100] Table 1 shows the PLQY test results of the samples obtained in Examples 1-6 of the present invention and Comparative Example 1, and the ratio of the luminous intensity after 100 hours of blue light aging to the initial intensity.

[0101] Table 1:

[0102]

[0103] The above-described embodiments provide a detailed description of the preparation scheme of the present invention. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the present invention. Any modifications, supplements or similar substitutions made within the scope of the principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for improving the light stability of perovskite by post-processing, characterized in that: The steps include: S1. Preparation of perovskite light emitter: Mixing a perovskite nanocrystal precursor and a micro / mesoporous template to obtain a mixture; calcining the mixture at a temperature lower than the collapse temperature of the micro / mesoporous template to generate perovskite nanocrystals in the pores of the micro / mesoporous template; S2, grinding and diffusion; The perovskite light emitting body prepared in step S1 is mixed with a post-treatment additive, and subjected to a grinding process, so that part of the post-treatment additive is accumulated in the pores of the micro / mesoporous template through grinding diffusion, thereby obtaining a post-treatment mixed powder; S3. Exposure and passivation of photoinduced defects: The post-processed mixed powder obtained in step S2 is annealed under light, wherein the photon energy of the light is greater than the energy corresponding to the band gap width of the perovskite nanocrystal, thereby causing the perovskite nanocrystal to reach an excited state to generate photoinduced defects; the annealing temperature is 100-300°C to promote the reaction between the post-processing additive and the perovskite nanocrystal to form a passivation layer to eliminate the photoinduced defects of the perovskite nanocrystal.

2. The method for improving the light stability of perovskite by post-processing according to claim 1, characterized in that: The perovskite nanocrystal precursor includes a precursor of a CsPbX3 perovskite structure, where X is at least one of Br, Cl, and I.

3. The method for improving the light stability of perovskite by post-processing according to claim 2, characterized in that: The CsPbX3 perovskite nanocrystal precursor is composed of a Cs source precursor, a Pb source precursor and a halogen source precursor; Wherein: the Cs source precursor includes one or more of cesium halide and cesium carbonate; The Pb source precursor includes one or more of lead halide and lead acetate; The halogen source precursor includes one or more of cesium halide, lead halide, zinc halide, potassium halide, sodium halide, lithium halide, ammonia halide, calcium halide, strontium halide, and barium halide.

4. The method for improving the light stability of perovskite by post-processing according to claim 1, characterized in that: The micro / mesoporous template is a microporous material and / or a mesoporous material; The microporous material is a microporous molecular sieve, microporous silica, microporous titania, microporous alumina, microporous transition metal oxide, microporous sulfide, microporous silicate, microporous aluminate or microporous transition metal nitride; The mesoporous material is mesoporous molecular sieve, mesoporous silica, mesoporous titania, mesoporous alumina, mesoporous carbon, mesoporous transition metal oxide, mesoporous sulfide, mesoporous silicate, mesoporous aluminate or mesoporous transition metal nitride.

5. The method for improving the light stability of perovskite by post-processing according to claim 4, characterized in that: The calcination temperature of the perovskite nanocrystal precursor and the micro / mesoporous template is less than 600° C., so as to prevent the pore structure of the micro / mesoporous template from collapsing.

6. The method for improving the light stability of perovskite by post-processing according to claim 1, characterized in that: The post-treatment additive includes one of fluoride, phosphate, pyrophosphate, and pyrosulfate.

7. The method for improving the light stability of perovskite by post-processing according to claim 6, characterized in that: The fluoride is selected from NH4F, NH4HF2, KF, CsF, NaF, NaAlF6, AlFK, KBF4, KAlF4, (C3F 60 )xC5F 120 、CrF3、C8F 18 , CeF3, SnF2, F4V, F4Ti, BeF2, KPF6 and combinations thereof; Phosphate selected from Bo4P, KPO3, Na5P3O 10 , Ba3(PO4)2, Ba(H2PO4)2, Ca(H2PO4)2, K3PO4, Na3PO4, (NaPO3) n , KPF6, NH4H2PO4, (NH4)2HPO4, Ca(H2PO4)2, KH2PO4, K2HPO4, K5O 10 P3, Na2HPO4, Na5P3O 10 , NaH2PO2, MgHPO4, Mg3(PO4)2, AlNa3(PO4)2, CaHPO4 and combinations thereof; The pyrophosphate is selected from the group consisting of K4P2O7, Sn2P2O7, Ca2P2O7, Na4P2O7, Fe4(P2O7)3, Na8Fe4(P2O7)5·xH2O, Mg2P2O7, Cu2P2O7, and combinations thereof; The pyrosulfate salt is selected from the group consisting of Na2S2O7, K2S2O7, H8N2O7S2 and combinations thereof.

8. The method for improving the light stability of perovskite by post-processing according to claim 1, characterized in that: The grinding process in step S2 includes wet grinding and dry grinding, and the dry grinding is ball milling.

9. The method for improving the light stability of perovskite by post-processing according to claim 1, characterized in that: Annealing under light in step S3 includes the following two situations: A1: First light exposure, then annealing to form a passivation layer; A2: Exposure of defects by light and annealing to form a passivation layer are carried out simultaneously.

10. A light-stable perovskite luminescent material, characterized in that: The perovskite light emitting body is prepared by the method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Perovskite quantum dot and preparation method and application thereof

    CN115772401A

  • Method for growing halide perovskite nanocrystals through in-situ chemical vapor deposition

    CN116752116A

Cited By

  • All-solid-state post-processing technology of perovskite quantum dots and application of all-solid-state post-processing technology

    CN118978913A

  • Full-solid post-processing technology of perovskite quantum dots and application thereof

    CN118978913B

  • Surface post-treatment process of perovskite quantum dots

    CN121628614A