Method for detecting trace chromium element in copper foil based on ICP-OES (Inductively Coupled Plasma-Optical Emission Spectrometer)

By combining mixed acid system digestion and scandium internal standard method with the dynamic background correction mode of ICP-OES, the interference problem of high-concentration copper matrix in the detection of trace chromium in lithium battery copper foil was solved, and high-precision chromium detection was achieved.

CN120741436APending Publication Date: 2025-10-03HENGTONG PRECISION COPPER FOIL TECHNOLOGY (DEYANG) CO LTD

Patent Information

Application Number
CN202510854818.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-06-25
Publication Date
2025-10-03

AI Technical Summary

Technical Problem

In the existing technology, the detection of trace chromium elements in lithium battery copper foil has problems such as interference from high-concentration copper matrix, insufficient detection limit and low detection accuracy. The traditional method is cumbersome to operate and easily introduces impurities.

Method used

A mixed acid system was used to digest the lithium battery copper foil. Concentrated nitric acid provided an acidic environment and oxidation, while hydrofluoric acid promoted dissolution. The scandium internal standard method and the dynamic background correction mode of ICP-OES were introduced to eliminate the interference of the copper matrix on the chromium element spectrum and improve the detection accuracy.

Benefits of technology

It significantly improves the detection accuracy and digestion efficiency of trace chromium elements, can effectively eliminate the interference of copper matrix, has a lower detection limit, a stable spike recovery rate, and more accurate detection results.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120741436A_ABST
    Figure CN120741436A_ABST
Patent Text Reader

Abstract

The invention discloses a method for detecting trace chromium element in copper foil based on ICP-OES (Inductively Coupled Plasma-Optical Emission Spectrometer), which comprises the following steps: soaking a lithium battery copper foil in a mixed solution of concentrated nitric acid and hydrofluoric acid for high-temperature digestion, adding a scandium internal standard solution, and fixing the volume to obtain a solution to be detected; preparing a mixed standard solution of chromium element and scandium element with a plurality of concentration gradients, and establishing a standard curve through ICP-OES; and determining the content of the chromium element in the to-be-detected solution according to the standard curve. The lithium battery copper foil is digested through a mixed acid system, concentrated nitric acid provides an acid environment and an oxidation effect, hydrofluoric acid promotes dissolution, it is ensured that the copper foil is completely dissolved, and the digestion efficiency is improved; a scandium internal standard method is introduced, a dynamic background correction mode of ICP-OES is adopted, a scandium internal standard element can correct signal fluctuation in a sample introduction process, dual guarantee is formed by the scandium internal standard element and dynamic background correction, interference of a copper matrix on a Cr spectral line is specifically eliminated, and the trace chromium element detection precision is remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of chromium element detection in lithium battery copper foil, and in particular to a method for detecting trace chromium elements in copper foil based on ICP-OES. Background Art

[0002] Lithium battery copper foil is the core material for the negative electrode current collector of lithium batteries, and its purity directly affects battery performance. To improve the oxidation resistance of lithium battery copper foil, it needs to be passivated to form a dense film. The passivation solution mainly contains chromic anhydride, and the concentration of chromium (Cr) in it directly affects the antioxidant effect of lithium battery copper foil. If the Cr content is too low, the copper foil will fail the oxidation resistance test; if the Cr content is too high, the conductivity of the copper foil will be reduced. Cr can also affect human health and cause environmental pollution. Therefore, it is necessary to accurately detect and control the Cr content on the copper foil surface.

[0003] Traditional spectrophotometry is cumbersome to operate and lacks sensitivity; atomic absorption spectrometry (AAS) has a narrow linear range and severe matrix interference; the existing ICP-OES (inductively coupled plasma optical emission spectroscopy) method is not optimized in terms of eliminating copper matrix interference and stabilizing trace Cr signals, resulting in insufficient detection limits. Patent CN109781497A uses hydrochloric acid to heat and boil the copper foil to dissolve it, filters out solid impurities after dissolution, heats and concentrates the filtrate, cools and then adjusts the volume to obtain a test solution. This method cannot determine whether the copper foil is completely dissolved, and the filtration adds a pretreatment step, which can easily introduce impurity elements that affect the test results. Patent CN111610181A uses highly concentrated hydrochloric acid and hydrogen peroxide to catalyze and accelerate the dissolution of the copper foil. After dilution, the test solution is obtained and ICP-OES is used to test the Cr content. Although this method simplifies the pretreatment process, it does not optimize the influence of the high-concentration Cu matrix, and its test accuracy is difficult to guarantee.

[0004] Therefore, there is currently no dedicated ICP-OES method for the detection of Cr in lithium battery copper foil, and technical difficulties such as interference from high-concentration copper matrix and improving the recovery rate of trace Cr need to be solved. Summary of the Invention

[0005] In response to the deficiencies in the prior art, the present invention provides a method for detecting trace chromium in copper foil based on ICP-OES. A mixed acid system is used to digest lithium battery copper foil. Concentrated nitric acid provides an acidic environment and oxidation, while hydrofluoric acid promotes dissolution, ensuring complete dissolution of the copper foil and improving digestion efficiency. A scandium (Sc) internal standard method is introduced, and the (DBC) dynamic background correction mode of the ICP-OES is adopted to specifically eliminate interference of the copper matrix on the Cr267.716nm spectral line, thereby significantly improving the detection accuracy of trace chromium.

[0006] In order to solve the above technical problems, the present invention provides a method for detecting trace chromium in copper foil based on ICP-OES, comprising the following steps:

[0007] S1. Immerse the lithium battery copper foil in a mixture of concentrated nitric acid and hydrofluoric acid and digest it at high temperature. Add the scandium internal standard solution and adjust the volume to obtain a test solution.

[0008] S2. Prepare several mixed standard solutions of chromium and scandium with different concentration gradients, and establish a standard curve by ICP-OES.

[0009] S3. Determine the content of chromium in the solution to be tested according to the standard curve.

[0010] The present invention places the lithium battery copper foil in a mixed acid system of concentrated nitric acid and hydrofluoric acid for digestion. The concentrated nitric acid provides an acidic environment and an oxidizing effect to digest the copper foil. During the process, a passivation layer such as copper oxide is generated and covers the copper surface. The hydrofluoric acid dissolves the copper oxide through the reaction of CuO+2HF→CuF2+H2O, thereby exposing a fresh copper surface and accelerating the digestion efficiency of the concentrated nitric acid. The iron impurities in the copper foil form Fe 3+ , which may catalyze side reactions or generate precipitation that interferes with digestion. The F released by hydrofluoric acid - with Fe 3+ Forming a stable complex [FeF6] 3- , inhibiting its oxidation activity; in addition, the surface of the copper foil contains silicate impurities (silicone oil or silicon dioxide), and hydrofluoric acid generates volatile silicon tetrafluoride through the reaction SiO2+4HF→SiF4↑+2H2O, which completely removes silicon contamination and prevents it from hindering the dissolution of the copper foil; in summary, hydrofluoric acid promotes dissolution, ensures the complete dissolution of the copper foil, and improves the digestion efficiency.

[0011] The present invention introduces a scandium internal standard method and adopts the (DBC) dynamic background correction mode of ICP-OES. The scandium internal standard element can correct signal fluctuations during the sample introduction process, forming a dual guarantee with the dynamic background correction, specifically eliminating the interference of the copper matrix on the Cr267.716nm spectral line, and significantly improving the detection accuracy of trace chromium elements.

[0012] Furthermore, in S1, the volume ratio of concentrated nitric acid to hydrofluoric acid is (3-5):1.

[0013] Furthermore, in S1, the high temperature digestion temperature is 180-200°C and the time is 10-15 minutes.

[0014] Furthermore, in S1, the concentration of scandium in the solution to be tested is 0-2 ppm.

[0015] Furthermore, in S2, the concentrations of chromium and scandium in the mixed standard solution are the same, and the concentrations of both are 0-10 ppm.

[0016] Furthermore, in S2, the ICP-OES parameters are: RF power 1250±50W, pump speed 45±5r / min, working pressure 0.6-0.7MPa, radial observation in dynamic background correction mode, processing time 40-60s, and exposure time 5-8s.

[0017] Furthermore, the working atmosphere of the ICP-OES is high-purity argon (purity ≥ 99.999%).

[0018] Furthermore, in S2, when the standard curve is established, the 267.716 nm spectral line is selected for chromium and the 361.384 nm spectral line is selected for scandium, and the calibration determination coefficient R of the standard curve is ≥ 0.999.

[0019] Furthermore, in S1, the ratio of the mass of the electrolytic copper foil to the volume of the solution to be tested is (0.9-1.1) g:50 mL.

[0020] Furthermore, in S1, the lithium battery copper foil is an electrolytic copper foil or a rolled copper foil with a thickness of 4.5-15 μm.

[0021] Furthermore, in S1, the lithium battery copper foil is cut into pieces and then immersed in the mixed solution.

[0022] Beneficial effects of the present invention:

[0023] The present invention uses a mixed acid system to digest lithium battery copper foil, wherein concentrated nitric acid provides an acidic environment and an oxidizing effect, and hydrofluoric acid promotes dissolution, thereby ensuring that the copper foil is completely dissolved and improving the digestion efficiency.

[0024] The present invention introduces a scandium internal standard method and adopts the dynamic background correction mode of ICP-OES. The scandium internal standard element can correct signal fluctuations during the sample introduction process, forming a dual guarantee with the dynamic background correction, specifically eliminating the interference of the copper matrix on the Cr 267.716nm spectral line, and significantly improving the detection accuracy of trace chromium elements. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the technical solution of the present invention, the following briefly introduces the drawings required for use in the embodiments. Obviously, the drawings described below are merely embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0026] Figure 1 This is a graph showing the Cr element standard curve in Example 1 of the present invention;

[0027] Figure 2 This is a standard curve diagram of the Sc element in Example 1 of the present invention;

[0028] Figure 3 This is a graph showing the standard curve of Cr element in Example 2 of the present invention;

[0029] Figure 4 It is a standard curve diagram of Sc element in Example 2 of the present invention. DETAILED DESCRIPTION

[0030] The following will provide a clear and complete description of the technical solutions of the present invention in conjunction with specific embodiments of the present invention. Obviously, the embodiments described are only some embodiments of the present invention, not all embodiments. All other embodiments obtained by ordinary technicians in this field based on the embodiments of the present invention without making any creative efforts shall fall within the scope of protection of the present invention.

[0031] This embodiment relates to a method for detecting trace chromium in copper foil based on ICP-OES, comprising the following steps:

[0032] S1. Immerse the lithium battery copper foil in a mixture of concentrated nitric acid and hydrofluoric acid and digest it at high temperature. Add the scandium internal standard solution and adjust the volume to obtain a test solution.

[0033] S2. Prepare several mixed standard solutions of chromium and scandium with different concentration gradients, and establish a standard curve by ICP-OES.

[0034] S3. Determine the content of chromium in the solution to be tested according to the standard curve.

[0035] In this embodiment, the lithium battery copper foil is placed in a mixed acid system of concentrated nitric acid and hydrofluoric acid for digestion. The concentrated nitric acid provides an acidic environment and oxidation to digest the copper foil. During the process, a passivation layer such as copper oxide is produced and covers the copper surface. The hydrofluoric acid dissolves the copper oxide through the reaction of CuO+2HF→CuF2+H2O, thereby exposing a fresh copper surface and accelerating the digestion efficiency of the concentrated nitric acid. The iron impurities in the copper foil form Fe 3+ , which may catalyze side reactions or generate precipitation that interferes with digestion. The F released by hydrofluoric acid - with Fe 3+ Forming a stable complex [FeF6] 3-, inhibiting its oxidative activity. Furthermore, the copper foil surface contains silicate impurities (silicone oil or silicon dioxide). Hydrofluoric acid generates volatile silicon tetrafluoride through the reaction of SiO2 + 4HF → SiF4↑ + 2H2O, completely removing the silicon contamination and preventing it from hindering the dissolution of the copper foil. In summary, hydrofluoric acid promotes dissolution, ensuring complete dissolution of the copper foil and improving digestion efficiency. The introduction of scandium as an internal standard and the use of the ICP-OES (DBC) dynamic background correction mode correct for signal fluctuations during sample introduction, providing dual protection alongside dynamic background correction, specifically eliminating interference from the copper matrix on the Cr 267.716nm spectral line, significantly improving the accuracy of trace chromium detection.

[0036] As a preferred embodiment, in S1, the volume ratio of concentrated nitric acid to hydrofluoric acid is (3-5):1; the temperature of the high-temperature digestion is 180-200°C, and the time is 10-15 minutes; the concentration of scandium in the solution to be tested is 0-2ppm.

[0037] As a preferred embodiment, in S1, the ratio of the mass of the electrolytic copper foil to the volume of the solution to be tested is (0.9-1.1) g:50 mL; the lithium battery copper foil is an electrolytic copper foil or a rolled copper foil with a thickness of 4.5-15 μm; the lithium battery copper foil is cut into pieces and immersed in the mixed solution.

[0038] As a preferred embodiment, in S2, the concentrations of chromium and scandium in the mixed standard solution are the same, and both concentrations are 0-10 ppm.

[0039] As a preferred embodiment, in S2, the parameters of the ICP-OES are: RF power 1250±50W, pump speed 45±5r / min, working pressure 0.6-0.7MPa, radial observation in dynamic background correction mode, processing time 40-60s, exposure time 5-8s, and working atmosphere of high-purity argon (purity ≥99.999%), wherein the carrier gas flow rate is 0.50±0.05L / min, the auxiliary gas flow rate is 0.50±0.05L / min, the cooling gas flow rate is 12.5±0.5L / min, and the nebulizing gas flow rate is 0.65±0.05L / min; when establishing the standard curve, the 267.716nm spectral line is selected for chromium element, and the 361.384nm spectral line is selected for scandium element, and the calibration determination coefficient R≥0.999 of the standard curve.

[0040] Example 1

[0041] This embodiment relates to a method for detecting trace chromium in copper foil based on ICP-OES, comprising the following steps:

[0042] (1) Select a 6μm thick lithium battery copper foil sample, wear nitrile gloves, and cut it into 1.0×1.0cm fragments. Weigh three sets of parallel samples, sample A with a mass of 1.005g, sample B with a mass of 1.008g, and sample C with a mass of 1.006g. Place them in three 50mL beakers, add 6mL of mixed acid (volume ratio HNO3:HF=5:1), and place them on a 180℃ graphite hot plate for high temperature digestion for 10min. After digestion is completed, remove them and cool them to room temperature. Then transfer the sample solutions to 50mL volumetric flasks, wash the beakers with appropriate amount of ultrapure water at least twice, and transfer the washing water to the volumetric flasks. At the same time, add 3mL, 5mL, and 8mL of Sc internal standard solution (5.0mg / L) to the A, B, and C sample volumetric flasks respectively. Finally, use ultrapure water to make up the volume and shake well. The concentrations of scandium in the samples to be tested are 0.3ppm, 0.5ppm, and 0.8ppm, respectively.

[0043] (2) Prepare five sets of mixed standard solutions of Cr and Sc. The concentrations of Cr and Sc in the standard solutions are: 0 ppm, 0.50 ppm, 1.00 ppm, 3.00 ppm, and 6.00 ppm, respectively.

[0044] (3) ICP-OES (model: PerkinElmer Avio 200) was used to test the standard solution to establish the standard defect. The test parameters were: RF power 1250W, pump speed 45r / min, working pressure 0.65MPa, radial observation in dynamic background correction mode, processing time 50s, exposure time 6s, working atmosphere was high-purity argon (purity ≥99.999%), carrier gas flow rate 0.50L / min, auxiliary gas flow rate 0.50L / min, cooling gas flow rate 12.5L / min, nebulizer gas flow rate 0.65L / min; when establishing the standard curve, the 267.716nm spectral line of chromium was selected, and the 361.384nm spectral line of scandium was selected. The calibration coefficients of the standard curve obtained by the test were Cr: R2 = 1.0000, Sc: R2 = 0.9998, reference Figure 1 and Figure 2 , the linear relationship meets the requirements and the standard curve is qualified.

[0045] (4) The chromium content in the sample to be tested in step (1) was measured according to the standard curve. The test results are shown in Table 1, where the calculation formula for the unit mass Cr content in the copper foil is:

[0046]

[0047] Wherein, C represents the measured Cr element content, in ppm; V represents the constant volume, in mL; and m represents the sample mass, in g.

[0048] Table 1

[0049]

[0050] As shown in Table 1, the inventive method has a linear zero in the range of 0-5 ppm of Cr concentration in the test solution, which meets the requirements of trace Cr testing. The spiked recovery rate is stable at 98%-102%, and the RSD is <1.5%, which proves that the method has excellent repeatability.

[0051] Example 2

[0052] This embodiment detects interference from a copper substrate, comprising the following steps:

[0053] (1) Add the Cu standard solution to a 50 mL volumetric flask, followed by the Cr standard solution and Sc standard solution (internal standard element). Finally, dilute to volume with ultrapure water and shake well to obtain a high-copper matrix solution. The solution has a Cu concentration of 1000 ppm, a Cr concentration of 5.00 ppm, and a Sc concentration of 1.00 ppm.

[0054] (2) Prepare mixed standard solutions of Cr and Sc. The concentrations of the standard solutions are: 0 ppm, 0.50 ppm, 1.00 ppm, 3.00 ppm, 6.00 ppm, and 10.00 ppm.

[0055] (3) Using ICP-OES (model: PerkinElmer Avio 200), the sample was tested according to the parameters of Example 1. The internal standard correction method was combined with dynamic background correction (DBC). The spectral interference of the Cu matrix on the Cr267.716nm was corrected in real time by Sc 361.384nm. The calibration determination coefficients of the standard curve obtained by the test were Cr: R2 = 0.9999, Sc: R2 = 0.9998, as shown in Figure 2. Figure 3 and Figure 4 , the linear relationship meets the requirements, the standard curve is qualified, and the test results are shown in Table 2.

[0056] Table 2

[0057] Interference Type Measured Cr content before correction (ppm) Measured Cr content after correction (ppm) deviation(%) Copper substrate 5.22 4.94 -1.2

[0058] As shown in Table 2, the internal standard method of the present invention combined with dynamic background correction can reduce the high copper matrix interference to <1.5%, and can effectively eliminate >99% of the copper matrix interference.

[0059] The method in Example 1 was compared with the prior art AAS and spectrophotometry methods to test the Cr content on the surface of copper foil. The detection limit, single-sample time consumption, and spiked recovery range are shown in Table 3. Compared with AAS and spectrophotometry, the ICP-OES method in Example 1 has a lower detection limit of 0.05 ppm; a single-sample time consumption of approximately 6 minutes, which is shorter; and a spiked recovery range of 98-102%, providing more accurate test results.

[0060] Table 3

[0061] Detection method Detection limit (ppm) Single sample time (min) Spike recovery range Example 1 0.05 6 98.0-102.0% AAS Law 0.20 15 95.0-107.0% Spectrophotometry 1.00 30 90.0-110.0%

[0062] In summary, the present invention uses a mixed acid system to digest lithium battery copper foil. Concentrated nitric acid provides an acidic environment and oxidation, while hydrofluoric acid promotes dissolution, ensuring complete dissolution of the copper foil and improving digestion efficiency. The present invention also introduces a scandium internal standard method and adopts the dynamic background correction mode of ICP-OES. The scandium internal standard element can correct signal fluctuations during the sample introduction process, forming a dual guarantee with the dynamic background correction, specifically eliminating the interference of the copper matrix on the Cr 267.716nm spectral line, and significantly improving the detection accuracy of trace chromium elements.

[0063] The present invention has been described in detail above with reference to specific embodiments and exemplary examples. However, these descriptions should not be construed as limiting the present invention. Those skilled in the art will appreciate that various equivalent substitutions, modifications, or improvements may be made to the technical solutions and implementations of the present invention without departing from the spirit and scope of the present invention, all of which fall within the scope of the present invention. The scope of protection of the present invention shall be determined by the appended claims.

Claims

1. A method for detecting trace chromium in copper foil based on ICP-OES, characterized in that: The steps include: S1. Immerse the lithium battery copper foil in a mixture of concentrated nitric acid and hydrofluoric acid and digest it at high temperature. Add the scandium internal standard solution and adjust the volume to obtain a test solution. S2. Prepare several mixed standard solutions of chromium and scandium with different concentration gradients, and establish a standard curve by ICP-OES. S3. Determine the content of chromium in the solution to be tested according to the standard curve.

2. The method for detecting trace chromium in copper foil based on ICP-OES according to claim 1, wherein: In S1, the volume ratio of concentrated nitric acid to hydrofluoric acid is (3-5):

1.

3. The method for detecting trace chromium in copper foil based on ICP-OES according to claim 1, wherein: In S1, the high temperature digestion temperature is 180-200°C and the time is 10-15 minutes.

4. The method for detecting trace chromium in copper foil based on ICP-OES according to claim 1, wherein: In S1, the concentration of scandium in the solution to be tested is 0-2 ppm.

5. The method for detecting trace chromium in copper foil based on ICP-OES according to claim 1, wherein: In S2, the concentrations of chromium and scandium in the mixed standard solution are the same, and both concentrations are 0-10 ppm.

6. The method for detecting trace chromium in copper foil based on ICP-OES according to claim 1, wherein: In S2, the ICP-OES parameters are: RF power 1250±50W, pump speed 45±5r / min, working pressure 0.6-0.7MPa, radial observation in dynamic background correction mode, processing time 40-60s, and exposure time 5-8s.

7. The method for detecting trace chromium in copper foil based on ICP-OES according to claim 1, wherein: In S2, when the standard curve is established, the 267.716nm spectral line is selected for chromium and the 361.384nm spectral line is selected for scandium. The calibration coefficient R of the standard curve is ≥ 0.

999.

8. The method for detecting trace chromium in copper foil based on ICP-OES according to claim 1, wherein: In S1, the ratio of the mass of the electrolytic copper foil to the volume of the solution to be tested is (0.9-1.1) g:50 mL.

9. The method for detecting trace chromium in copper foil based on ICP-OES according to claim 1, wherein: In S1, the lithium battery copper foil is an electrolytic copper foil or a rolled copper foil with a thickness of 4.5-15 μm.

10. The method for detecting trace chromium in copper foil based on ICP-OES according to claim 1, wherein: In S1, the lithium battery copper foil is cut into pieces and then immersed in the mixed solution.

Citation Information

Patent Citations

  • Quantitative detection method for surface chromium content of electrolytic copper foil

    CN109781497A

  • Quantitative detection method for chromium content of copper foil

    CN111610181A

Cited By

  • Method for detecting content of Zn element in surface treatment layer of rolled copper foil

    CN116203116A

  • Method for detecting trace elements in electrolyte by ICP-OES (Inductively Coupled Plasma Optical Emission Spectrometer) and application

    CN122084604A