A silver electroplating solution containing thiodiethylene glycol and its preparation method
By regulating silver grain growth through complexes of thiodiethylene glycol with nitrogen-containing heterocyclic compounds and thiourea derivatives, the problems of coating quality and operational complexity in cyanide-free silver plating technology have been solved, achieving efficient and environmentally friendly silver plating results.
Patent Information
- Application Number
- CN202511248262.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-09-03
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2045-09-03
AI Technical Summary
Existing cyanide-free silver plating technology suffers from inferior plating quality compared to cyanide solutions, insufficient gloss and durability, and higher operational complexity, increasing production costs and environmental risks.
A silver electroplating solution containing thiodiethylene glycol is used. Thiodiethylene glycol forms a highly stable complex with nitrogen-containing heterocyclic compounds. The growth of silver grains is regulated by combining thiourea derivatives. A cyanide-free system is used to reduce environmental pollution. The adhesion of the coating is improved by using corrosion inhibitors and anti-displacement treatment solutions.
It improves the hardness and wear resistance of the coating, reduces the risk of environmental pollution, simplifies the operation process, and provides coating quality comparable to traditional cyanide silver plating.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention belongs to the field of silver plating technology and relates to a silver electroplating solution containing thiodiethylene glycol and its preparation method. Background Technology
[0002] Traditional silver plating technology primarily relies on cyanide as a complexing agent. Cyanide solutions possess excellent stability and coating gloss, thus they have long been widely used in various industrial silver plating processes. However, the toxicity of cyanide and its potential environmental hazards have prompted the search for safer alternatives. Traditional silver plating processes typically require stringent operating conditions and wastewater treatment measures to mitigate environmental pollution risks, which significantly increases production costs and operational complexity. Furthermore, the management and disposal of cyanide solutions must adhere to strict regulations and standards to ensure operator safety and environmental protection.
[0003] In recent years, to reduce the environmental and safety problems caused by cyanide use, cyanide-free silver plating technology has been gradually developed and applied. These technologies typically use non-cyanide complexing agents, such as thiosulfates, aminosulfonates, or other organic complexing agents, to replace cyanide. In cyanide-free silver plating processes, the use of more environmentally friendly chemicals can significantly reduce the toxicity and environmental risks of the process, while also reducing the complexity of wastewater treatment. These alternative technologies can generally provide coating quality comparable to traditional cyanide silver plating, with lower production costs and operational complexity. However, the widespread adoption of cyanide-free silver plating technology is still limited by some technical challenges.
[0004] While cyanide-free silver plating technology offers significant advantages in terms of environmental friendliness and safety, existing technologies still have some shortcomings. Firstly, the stability and coating quality of cyanide-free silver plating solutions may be inferior to cyanide solutions under certain conditions, resulting in slightly lower gloss and durability compared to traditional processes. Furthermore, some cyanide-free silver plating technologies may require more complex chemical formulations or more demanding operating conditions, increasing process complexity. Therefore, further optimizing cyanide-free silver plating technology to improve coating quality and reduce operational difficulty is a pressing issue that needs to be addressed. Summary of the Invention
[0005] The purpose of this invention is to provide a silver electroplating solution containing thiodiethylene glycol and its preparation method, which is a cyanide-free system that reduces environmental pollution.
[0006] The objective of this invention can be achieved through the following technical solutions: A silver electroplating solution containing thiodiethylene glycol, comprising: Pre-plating solution: contains Ag + 1.0-3.0 g / L; Thiodiethylene glycol: 20-35 vol%; Nitrogen-containing heterocyclic compound auxiliary complexing agent: 25-60 g / L; Methylsulfonic acid: 25-45 mL / L; Main plating bath starter: Contains Ag + 30-50 g / L; Thiodiethylene glycol: 20-35 vol%; Nitrogen-containing heterocyclic compound auxiliary complexing agent: 70-130 g / L; Methylsulfonic acid: 25-45 mL / L; Thiourea derivative additive: 5-20 g / L; Supplements: Contains thiodiethylene glycol: 0.05-0.5 vol%, silver sulfamate: 350-550 g / L, and corrosion inhibitor: 5-20 g / L.
[0007] In this application, the thioether group (-S-) of thiodiethylene glycol provides a lone pair of electrons with Ag. + Tetrahedral complexes are formed, exhibiting higher stability constants than silver cyanide; nitrogen-containing heterocyclic compounds (such as 2-mercaptobenzimidazole) coordinate with nitrogen heterocycles via thiol groups (-SH) to form mixed ligand complexes, shifting the deposition potential negatively and inhibiting substitution reactions; thiourea derivatives adsorb onto the cathode surface to form a steric hindrance layer, inhibiting disordered silver ion deposition, and the C=S bond in the molecule breaks to produce S... 2- , with Ag + Nano-Ag2S crystal nuclei are generated, leading to the growth of dense coating.
[0008] Furthermore, the preparation method of the thiodiethylene glycol-containing silver electroplating solution includes the following steps: Preparation of pre-plating solution: Dissolve thiodiethylene glycol and nitrogen-containing heterocyclic compound auxiliary complexing agent in water and stir until dissolved; add methanesulfonic acid dropwise and stir until homogeneous; then add AgNO3 solution dropwise and mix thoroughly; adjust pH to 3.5-5.5; Preparation of the main plating bath starter: Dissolve thiodiethylene glycol and auxiliary complexing agent in water and stir until dissolved; add methanesulfonic acid dropwise and stir until homogeneous; then add AgNO3 solution dropwise and mix thoroughly; add thiourea derivative additive and stir until dissolved; adjust the pH to 4.0-6.0. Preparation of the supplement: Dissolve silver sulfamate in water and stir until dissolved; add thiodiethylene glycol and corrosion inhibitor dropwise and mix thoroughly until dissolved.
[0009] As a preferred embodiment of the present invention, the nitrogen-containing heterocyclic compound auxiliary complexing agent is at least one selected from 2-mercaptobenzimidazole, benzotriazole, nicotinic acid, isonicotinic acid, 2-aminopyrimidine, and 2,2'-bipyridine.
[0010] As a preferred embodiment of the present invention, the thiourea derivative additive is at least one of thiourea, diphenylthiourea, N,N'-diethylthiourea, and propenylthiourea.
[0011] As a preferred embodiment of the present invention, the corrosion inhibitor is at least one of benzotriazole, methylbenzotriazole, and mercaptobenzothiazole.
[0012] Furthermore, a method for silver plating, using the aforementioned thiodiethylene glycol-containing silver plating solution, includes the steps of: (1) Pretreatment of the matrix; (2) Immerse the pre-treated substrate in the pre-plating solution at 20-30℃ and a cathode current density of 0.5-1.5 A / dm. 2 Perform pre-plating for 1-5 minutes; (3) Immerse the pre-plated substrate in the main plating solution's starter agent at 25-35°C and a cathode current density of 1-3 A / dm. 2 It is then silver-plated and supplemented.
[0013] As a preferred technical solution of the present invention, the pretreatment in step (1) is to immerse the substrate in an alkaline cleaning solution at 60-70°C for 5-10 minutes and then immerse it in 10% H2SO4 for 30-60 seconds for activation. After acid washing and activation, the substrate is immersed in an anti-displacement treatment solution for 20-30 seconds.
[0014] As a preferred embodiment of the present invention, the alkaline cleaning solution contains: 40-60 g / L NaOH, 20-30 g / L Na2CO3, 4-6 g / L fatty acid methyl ester ethoxylate, and the remainder is deionized water.
[0015] As a preferred embodiment of the present invention, the anti-displacement treatment solution contains: 4-6% aminosulfonic acid and 0.02-0.2% thiourea derivative.
[0016] As a preferred technical solution of the present invention, in step (3), the supplement is added to the main plating solution during the electroplating process, and the amount of supplement added is V=K×Q / (C×η); Where K = 0.85-0.95, Q = cumulative ampere-hours (Ah / L) of the main plating solution; C = silver sulfamate concentration in the supplement, ranging from 350-550 g / L; η = cathode current efficiency, ranging from 92%-95%.
[0017] The beneficial effects of this invention are: (1) The silver plating solution and silver plating process of this invention adopt a cyanide-free system, which completely avoids the risk of cyanide toxicity. Through the synergistic complexation of thiodiethylene glycol and nitrogen-containing heterocyclic compounds, the silver ion complexation is improved and the free Ag is reduced. + Concentration, further reducing environmental pollution.
[0018] (2) The present invention uses the selective adsorption effect of thiourea derivatives on the crystal surface of the coating to regulate the orientation of silver grains to preferential growth of the crystal surface, thereby improving the hardness and wear resistance of the coating and reducing the coefficient of friction. Through the anti-displacement treatment solution, which contains 5% aminosulfonic acid and 0.1% thiourea derivatives, a transition layer is formed in the pre-plating pretreatment to improve the adhesion. Detailed Implementation
[0019] To further illustrate the technical means and effects of the present invention in achieving its intended purpose, the following detailed description of the specific implementation methods, structures, features, and effects of the present invention, in conjunction with embodiments, is provided below.
[0020] Example 1 A silver electroplating solution containing thiodiethylene glycol, comprising: Pre-plating solution, which contains 2 g / LAg + 28 vol% thiodiethylene glycol, 42 g / L nitrogen-containing heterocyclic compound auxiliary complexing agent, 35 mL / L methanesulfonic acid; Main plating bath starter, containing 40 g / LAg + 27 vol% thiodiethylene glycol, 100 g / L nitrogen-containing heterocyclic compound auxiliary complexing agent, 35 mL / L methanesulfonic acid, 13 g / L thiourea derivative additive; The supplement contains 0.3 vol% thiodiethylene glycol, 450 g / L silver sulfamate, and 12 g / L corrosion inhibitor.
[0021] The method for preparing a thiodiethylene glycol-containing silver electroplating solution includes the following steps: Preparation of pre-plating solution: Dissolve thiodiethylene glycol and nitrogen-containing heterocyclic compound auxiliary complexing agent in water and stir until dissolved; add methanesulfonic acid dropwise and stir until homogeneous; then add AgNO3 solution dropwise and mix thoroughly; adjust pH to 4.5; Preparation of the main plating bath starter: Dissolve thiodiethylene glycol and auxiliary complexing agent in water and stir until dissolved; add methanesulfonic acid dropwise and stir until homogeneous; then add AgNO3 solution dropwise and mix thoroughly; add thiourea derivative additive and stir until dissolved; adjust pH to 5.0. Preparation of the supplement: Dissolve silver sulfamate in water and stir until dissolved; add thiodiethylene glycol and corrosion inhibitor dropwise and mix thoroughly until dissolved.
[0022] The nitrogen-containing heterocyclic compound auxiliary complexing agent is 2-mercaptobenzimidazole.
[0023] The thiourea derivative additive is thiourea.
[0024] The corrosion inhibitor is benzotriazole.
[0025] A method for silver plating, using the aforementioned thiodiethylene glycol-containing silver plating solution, includes the following steps: (1) Pretreatment of the matrix; (2) Immerse the pre-treated substrate in the pre-plating solution at 25°C and a cathode current density of 1 A / dm. 2 Perform pre-plating for 3 minutes; (3) Immerse the pre-plated substrate in the main plating solution's starter agent at 30°C and a cathode current density of 2A / dm³. 2 It is then silver-plated and supplemented.
[0026] The pretreatment in step (1) involves immersing the substrate in an alkaline cleaning solution at 65°C for 8 minutes, followed by immersion in 10% H2SO4 for 45 seconds for activation, and then immersion in an anti-displacement treatment solution for 25 seconds after acid washing and activation.
[0027] The alkaline cleaning solution contains: 50 g / L NaOH, 25 g / L Na2CO3, 5 g / L fatty acid methyl ester ethoxylate, and the remainder is deionized water.
[0028] The anti-displacement treatment solution contains: 5% aminosulfonic acid and 0.1% thiourea derivative.
[0029] In step (3), the supplement is added to the main plating solution during the electroplating process. The amount of supplement added is V = K × Q / (C × η). Where K=0.9, Q=cumulative ampere-hours (Ah / L) of the main plating solution; C=silver sulfamate concentration in the supplement, taken as 450 g / L; η=cathode current efficiency, taken as 93%.
[0030] Based on Example 1, the compound complexing agent was adjusted as follows: Example 2 Pre-plating solution, which contains 2 g / LAg + 28 vol% thiodiethylene glycol, 42 g / L nitrogen-containing heterocyclic compound auxiliary complexing agent, 35 mL / L methanesulfonic acid; Main plating bath starter, containing 40 g / LAg + 27 vol% thiodiethylene glycol, 100 g / L nitrogen-containing heterocyclic compound auxiliary complexing agent, 35 mL / L methanesulfonic acid, 13 g / L thiourea derivative additive; The supplement contains 0.3 vol% thiodiethylene glycol, 450 g / L silver sulfamate, and 12 g / L corrosion inhibitor.
[0031] The method for preparing a thiodiethylene glycol-containing silver electroplating solution includes the following steps: Preparation of pre-plating solution: Dissolve thiodiethylene glycol and nitrogen-containing heterocyclic compound auxiliary complexing agent in water and stir until dissolved; add methanesulfonic acid dropwise and stir until homogeneous; then add AgNO3 solution dropwise and mix thoroughly; adjust pH to 4.5; Preparation of the main plating bath starter: Dissolve thiodiethylene glycol and auxiliary complexing agent in water and stir until dissolved; add methanesulfonic acid dropwise and stir until homogeneous; then add AgNO3 solution dropwise and mix thoroughly; add thiourea derivative additive and stir until dissolved; adjust pH to 5.0. Preparation of the supplement: Dissolve silver sulfamate in water and stir until dissolved; add thiodiethylene glycol and corrosion inhibitor dropwise and mix thoroughly until dissolved.
[0032] The pre-plating solution contains nitrogen-containing heterocyclic compound auxiliary complexing agent containing nicotinic acid 30 g / L and benzotriazole 10 g / L; the main plating solution starter contains nitrogen-containing heterocyclic compound auxiliary complexing agent containing nicotinic acid 80 g / L and benzotriazole 20 g / L.
[0033] The thiourea derivative additive is thiourea.
[0034] The corrosion inhibitor is benzotriazole.
[0035] A method for silver plating, using the aforementioned thiodiethylene glycol-containing silver plating solution, includes the following steps: (1) Pretreatment of the matrix; (2) Immerse the pre-treated substrate in the pre-plating solution at 25°C and a cathode current density of 1 A / dm. 2 Perform pre-plating for 3 minutes; (3) Immerse the pre-plated substrate in the main plating solution's starter agent at 30°C and a cathode current density of 2A / dm³. 2 It is then silver-plated and supplemented.
[0036] The pretreatment in step (1) involves immersing the substrate in an alkaline cleaning solution at 65°C for 8 minutes, followed by immersion in 10% H2SO4 for 45 seconds for activation, and then immersion in an anti-displacement treatment solution for 25 seconds after acid washing and activation.
[0037] The alkaline cleaning solution contains: 50 g / L NaOH, 25 g / L Na2CO3, 5 g / L fatty acid methyl ester ethoxylate, and the remainder is deionized water.
[0038] The anti-displacement treatment solution contains: 5% aminosulfonic acid and 0.1% thiourea derivative.
[0039] In step (3), the supplement is added to the main plating solution during the electroplating process. The amount of supplement added is V = K × Q / (C × η). Where K=0.9, Q=cumulative ampere-hours (Ah / L) of the main plating solution; C=silver sulfamate concentration in the supplement, taken as 450 g / L; η=cathode current efficiency, taken as 93%.
[0040] Set extreme parameter boundary tests: Example 3 A silver electroplating solution containing thiodiethylene glycol, comprising: The pre-plating solution contains 1.0 g / LAg. + 20 vol% thiodiethylene glycol, 25 g / L nitrogen-containing heterocyclic compound auxiliary complexing agent, 25 mL / L methanesulfonic acid; Main plating bath starter, containing 30 g / LAg + 20 vol% thiodiethylene glycol, 70 g / L nitrogen-containing heterocyclic compound auxiliary complexing agent, 25 mL / L methanesulfonic acid, 5 g / L thiourea derivative additive; The supplement contains 0.05 vol% thiodiethylene glycol, 350 g / L silver sulfamate, and 5 g / L corrosion inhibitor.
[0041] The method for preparing a thiodiethylene glycol-containing silver electroplating solution includes the following steps: Preparation of pre-plating solution: Dissolve thiodiethylene glycol and nitrogen-containing heterocyclic compound auxiliary complexing agent in water and stir until dissolved; add methanesulfonic acid dropwise and stir until homogeneous; then add AgNO3 solution dropwise and mix thoroughly; adjust pH to 3.5; Preparation of the main plating bath starter: Dissolve thiodiethylene glycol and auxiliary complexing agent in water and stir until dissolved; add methanesulfonic acid dropwise and stir until homogeneous; then add AgNO3 solution dropwise and mix thoroughly; add thiourea derivative additive and stir until dissolved; adjust pH to 4.0. Preparation of the supplement: Dissolve silver sulfamate in water and stir until dissolved; add thiodiethylene glycol and corrosion inhibitor dropwise and mix thoroughly until dissolved.
[0042] The nitrogen-containing heterocyclic compound auxiliary complexing agent is 2-aminopyrimidine.
[0043] The thiourea derivative additive is N,N'-diethylthiourea.
[0044] The corrosion inhibitor is methylbenzotriazole.
[0045] A method for silver plating, using the aforementioned thiodiethylene glycol-containing silver plating solution, includes the following steps: (1) Pretreatment of the matrix; (2) Immerse the pre-treated substrate in the pre-plating solution at 20°C and a cathode current density of 0.5 A / dm. 2 Perform pre-plating for 1 minute; (3) Immerse the pre-plated substrate in the main plating solution's starter agent at 25°C and a cathode current density of 1 A / dm³. 2 It is then silver-plated and supplemented.
[0046] The pretreatment in step (1) involves immersing the substrate in an alkaline cleaning solution at 60°C for 5 minutes, followed by immersion in 10% H2SO4 for 30 seconds for activation, and then immersion in an anti-displacement treatment solution for 20 seconds after acid washing and activation.
[0047] The alkaline cleaning solution contains: 40 g / L NaOH, 20 g / L Na2CO3, 4 g / L fatty acid methyl ester ethoxylate, and the remainder is deionized water.
[0048] The anti-displacement treatment solution contains: 5% aminosulfonic acid and 0.1% thiourea derivative.
[0049] In step (3), the supplement is added to the main plating solution during the electroplating process. The amount of supplement added is V = K × Q / (C × η). Where K=0.85, Q=cumulative ampere-hours (Ah / L) of the main plating solution; C=silver sulfamate concentration in the supplement, taken as 350 g / L; η=cathode current efficiency, taken as 92%.
[0050] Set extreme parameter boundary tests: Example 4 A silver electroplating solution containing thiodiethylene glycol, comprising: The pre-plating solution contains 3.0 g / LAg. + 35 vol% thiodiethylene glycol, 60 g / L nitrogen-containing heterocyclic compound auxiliary complexing agent, 45 mL / L methanesulfonic acid; Main plating bath starter, containing 50 g / LAg + 35 vol% thiodiethylene glycol, 130 g / L nitrogen-containing heterocyclic compound auxiliary complexing agent, 45 mL / L methanesulfonic acid, 20 g / L thiourea derivative additive; The supplement contains 0.5 vol% thiodiethylene glycol, 550 g / L silver sulfamate, and 20 g / L corrosion inhibitor.
[0051] The method for preparing a thiodiethylene glycol-containing silver electroplating solution includes the following steps: Preparation of pre-plating solution: Dissolve thiodiethylene glycol and nitrogen-containing heterocyclic compound auxiliary complexing agent in water and stir until dissolved; add methanesulfonic acid dropwise and stir until homogeneous; then add AgNO3 solution dropwise and mix thoroughly; adjust pH to 5.5; Preparation of the main plating bath starter: Dissolve thiodiethylene glycol and auxiliary complexing agent in water and stir until dissolved; add methanesulfonic acid dropwise and stir until homogeneous; then add AgNO3 solution dropwise and mix thoroughly; add thiourea derivative additive and stir until dissolved; adjust pH to 6.0. Preparation of the supplement: Dissolve silver sulfamate in water and stir until dissolved; add thiodiethylene glycol and corrosion inhibitor dropwise and mix thoroughly until dissolved.
[0052] The nitrogen-containing heterocyclic compound auxiliary complexing agent is isonicotinic acid.
[0053] The thiourea derivative additive is propylene thiourea.
[0054] The corrosion inhibitor is mercaptobenzothiazole.
[0055] A method for silver plating, using the aforementioned thiodiethylene glycol-containing silver plating solution, includes the following steps: (1) Pretreatment of the matrix; (2) Immerse the pre-treated substrate in the pre-plating solution at 30°C and a cathode current density of 1.5 A / dm. 2 Perform pre-plating for 5 minutes; (3) Immerse the pre-plated substrate in the main plating solution's starter agent at 35°C and a cathode current density of 3 A / dm³. 2 It is then silver-plated and supplemented.
[0056] The pretreatment in step (1) involves immersing the substrate in an alkaline cleaning solution at 70°C for 10 minutes, followed by immersion in 10% H2SO4 for 60 seconds for activation, and then immersion in an anti-displacement treatment solution for 30 seconds after acid washing and activation.
[0057] The alkaline cleaning solution contains: 40-60 g / L NaOH, 20-30 g / L Na2CO3, 4-6 g / L fatty acid methyl ester ethoxylate, and the balance is deionized water.
[0058] The anti-displacement treatment solution contains: 5% aminosulfonic acid and 0.1% thiourea derivative.
[0059] In step (3), the supplement is added to the main plating solution during the electroplating process. The amount of supplement added is V = K × Q / (C × η). Where K=0.95, Q=cumulative ampere-hours (Ah / L) of the main plating solution; C=silver sulfamate concentration in the supplement, taken as 550 g / L; η=cathode current efficiency, taken as 95%.
[0060] Comparative Example 1 Based on Example 1, the thiodiethylene glycol in the pre-plating solution and the main plating solution starter was replaced with 250 g / L sodium thiosulfate and 50 g / L EDTA, while the rest remained the same as in Example 1.
[0061] Comparative Example 2 Based on Example 1, the concentration of silver sulfamate supplement was changed to 150 g / L, and the supplement volume was increased by 3 times under the same power supply; the rest remained the same as in Example 1.
[0062] Comparative Example 3 Based on Comparative Example 1, the pretreatment step of immersion in anti-displacement treatment solution was omitted, while the rest remained the same as in Example 1.
[0063] Comparative Example 4 Based on Example 1, the main plating bath starter does not contain thiourea derivative additives, while the rest remains the same as in Example 1.
[0064] Performance testing: Tests were conducted on copper sheets after silver plating according to the above embodiments and comparative examples; Sedimentation rate: After 2000Ah of continuous electroplating, 100mL of plating solution was filtered through a 0.45μm filter membrane, dried at 105℃ and weighed. Sedimentation rate = sediment mass / plating solution mass; Bond strength: Tested according to ASTM B571 thermal shock test, and observed for peeling. Porosity: The porosity of the coating was tested according to ASTM B765-03(2023) standard; Abrasion resistance: Abrasion resistance is tested according to ISO 4527 standard.
[0065]
[0066] The test results show that the precipitation rates in Examples 1-4 are all within 0.01%, indicating that the thiodiethylene glycol-nitrogen-containing heterocyclic complexing agent effectively inhibits Ag2S precipitation. Comparative Example 1 uses a traditional cyanide-free silver plating system with sodium thiosulfate and EDTA, which results in unstable complexation and easy oxidation of EDTA. Comparative Example 2 has a low concentration of silver sulfamate as a supplement, and the addition of the supplement has a significant impact on the concentration of the complex, resulting in a significant increase in the porosity and wear weight loss of the coating. Comparative Example 3 omits the anti-displacement treatment solution immersion, and the significantly increased peeling rate may be due to a displacement reaction in the copper substrate. Comparative Example 4 lacks a thiourea derivative, resulting in coarse grains and many defects.
[0067] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the present invention. Any indirect modifications, equivalent changes, and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.
Claims
1. A silver electroplating solution containing thiodiethylene glycol, characterized in that: include: The pre-plating solution contains 1.0-3.0 g / LAg. + 20-35 vol% thiodiethylene glycol, 25-60 g / L nitrogen-containing heterocyclic compound auxiliary complexing agent, 25-45 mL / L methanesulfonic acid; Main plating bath starter, containing 30-50 g / LAg + 20-35 vol% thiodiethylene glycol, 70-130 g / L nitrogen-containing heterocyclic compound auxiliary complexing agent, 25-45 mL / L methanesulfonic acid, 5-20 g / L thiourea derivative additive; The supplement contains 0.05-0.5 vol% thiodiethylene glycol, 350-550 g / L silver sulfamate, and 5-20 g / L corrosion inhibitor.
2. A method for preparing the thiodiethylene glycol-containing silver electroplating solution as described in claim 1, characterized in that: Includes the following steps: Preparation of pre-plating solution: Dissolve thiodiethylene glycol and nitrogen-containing heterocyclic compound auxiliary complexing agent in water and stir until dissolved; add methanesulfonic acid dropwise and stir until homogeneous; then add AgNO3 solution dropwise and mix thoroughly; adjust pH to 3.5-5.5; Preparation of the main plating bath starter: Dissolve thiodiethylene glycol and auxiliary complexing agent in water and stir until dissolved; add methanesulfonic acid dropwise and stir until homogeneous; then add AgNO3 solution dropwise and mix thoroughly; add thiourea derivative additive and stir until dissolved; adjust the pH to 4.0-6.
0. Preparation of the supplement: Dissolve silver sulfamate in water and stir until dissolved; add thiodiethylene glycol and corrosion inhibitor dropwise and mix thoroughly until dissolved.
3. The silver electroplating solution containing thiodiethylene glycol according to claim 1, characterized in that: The nitrogen-containing heterocyclic compound auxiliary complexing agent is at least one selected from 2-mercaptobenzimidazole, benzotriazole, nicotinic acid, isonicotinic acid, 2-aminopyrimidine, and 2,2'-bipyridine.
4. The silver electroplating solution containing thiodiethylene glycol according to claim 1, characterized in that: The thiourea derivative additive is at least one of thiourea, diphenylthiourea, N,N'-diethylthiourea, and propenylthiourea.
5. The silver electroplating solution containing thiodiethylene glycol according to claim 1, characterized in that: The corrosion inhibitor is at least one of benzotriazole, methylbenzotriazole, and mercaptobenzothiazole.
6. A method for silver plating, characterized in that, Using the thiodiethylene glycol-containing silver electroplating solution as described in any one of claims 1-5, the steps include: (1) Pretreatment of the substrate; the pretreatment is to immerse the substrate in an alkaline cleaning solution at 60-70℃ for 5-10 min, then activate it by immersing it in 10% H2SO4 for 30-60 s, and after acid washing activation, immerse it in an anti-displacement treatment solution for 20-30 s; the anti-displacement treatment solution contains: 4-6% aminosulfonic acid and 0.02-0.2% thiourea derivative; (2) Immerse the pre-treated substrate in the pre-plating solution at 20-30℃ and a cathode current density of 0.5-1.5 A / dm. 2 Perform pre-plating for 1-5 minutes; (3) Immerse the pre-plated substrate in the main plating solution's starter agent at 25-35°C and a cathode current density of 1-3 A / dm. 2 It is then silver-plated and supplemented.
7. The silver plating method according to claim 6, characterized in that: The alkaline cleaning solution contains: 40-60 g / L NaOH, 20-30 g / L Na2CO3, 4-6 g / L fatty acid methyl ester ethoxylate, and the balance is deionized water.
8. A silver plating method according to claim 6, characterized in that: In step (3), the supplement is added to the main plating solution during the electroplating process. The amount of supplement added is V = K × Q / (C × η). Where K = 0.85-0.95, Q = cumulative ampere-hours (Ah / L) of the main plating solution; C = silver sulfamate concentration in the supplement, ranging from 350-550 g / L; η = cathode current efficiency, ranging from 92%-95%.
Citation Information
Patent Citations
Non-cyanogen plate silver plating solution
CN101298689A
Alloy plating
CN1351678A