Additive manufacturing high-temperature alloy product with excellent high-temperature strength plasticity and preparation method of additive manufacturing high-temperature alloy product

By controlling the proportion of high-temperature alloying elements and the heat treatment process, the metallurgical defects of high-temperature alloys in additive manufacturing have been solved, achieving high density and excellent strength and plasticity of high-temperature alloys to meet practical application requirements.

CN120843894APending Publication Date: 2025-10-28RESEARCH INSTITUTE OF ADVANCED MATERIALS (SHENZHEN) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202511019314.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-07-23
Publication Date
2025-10-28

AI Technical Summary

Technical Problem

Existing high-temperature alloys have metallurgical defects such as pores, lack of fusion, and cracks during additive manufacturing, resulting in low density, substandard mechanical properties, and poor strength-plasticity matching, making it difficult to meet actual application requirements.

Method used

By controlling the mass fraction range of elements such as Cr, Co, Mo, Al, Ti, Nb, and Ta in high-temperature alloys, and combining the volume fraction of γ' strengthening phase and TCP phase, additive manufacturing high-temperature alloy products with excellent high-temperature strength and plasticity are prepared by using a heat treatment process of hot isostatic pressing-solution heat treatment-aging heat treatment.

Benefits of technology

It improves the density and printability of high-temperature alloys, with tensile strength of 900MPa~1100MPa, yield strength of 750MPa~1000MPa, elongation of 6%~20%, and reduction of area of ​​8%~20% at 800℃, overcoming the defects of poor printability, poor high-temperature creep resistance, and poor high-temperature plasticity in existing technologies.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120843894A_ABST
    Figure CN120843894A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of high-temperature alloys, in particular to an additive manufacturing high-temperature alloy product with excellent high-temperature strength and plasticity and a preparation method thereof, and the alloy product comprises the following components in percentage by mass: 10%-18% of Cr, 23.1%-28% of Co, 3.6%-6% of Mo, 1.9%-6% of W, 1%-3% of Al, 1.5%-4.75% of Ti, 1.01%-3% of Nb, 0%-5% of Ta, 0%-8% of Fe, 0.01%-0.5% of C, 0%-0.05% of B, 0%-0.2% of Zr, 0%-0.5% of O, 0-0.2% of N and the balance of Ni. By controlling the content of main elements, the problems of poor printability, poor high-temperature creep resistance, poor high-temperature strength and plasticity and difficulty in balancing each index are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of high-temperature alloy technology, and in particular to an additive manufacturing high-temperature alloy product with excellent high-temperature strength and plasticity and its preparation method. Background Technology

[0002] High-temperature alloy products, due to the diverse types and wide variations in the content of alloying elements, often exhibit metallurgical defects such as voids, incomplete fusion, and cracks during additive manufacturing. This results in low alloy density, substandard mechanical properties, and poor strength-ductility matching. Easily printable alloys, such as GH4169, have fewer defects but low strength-ductility above 800℃, failing to meet practical application requirements. Difficult-to-print alloys, such as GH4720, have better high-temperature mechanical properties but poor printability. Current technology demands a high-temperature alloy product with good printability, high high-temperature creep resistance, and high high-temperature strength-ductility. Summary of the Invention

[0003] Based on the above analysis, the present invention aims to provide an additive manufacturing high-temperature alloy product with excellent high-temperature strength and plasticity and its preparation method, which solves at least one of the problems of poor printability, poor high-temperature creep resistance, poor high-temperature strength and plasticity, and difficulty in balancing various indicators in the prior art.

[0004] The objective of this invention is mainly achieved through the following technical solutions:

[0005] An additively manufactured high-temperature alloy product with excellent high-temperature strength and plasticity comprises the following components by mass fraction: Cr 10%–18%, Co 23.1%–28%, Mo 3.6%–6%, W 1.9%–6%, Al 1%–3%, Ti 1.5%–4.75%, Nb 1.01%–3%, Ta 0%–5%, Fe 0%–8%, C 0.01%–0.5%, B 0%–0.05%, Zr 0%–0.2%, O 0–0.5%, N 0–0.2%, with the balance being Ni.

[0006] Preferably, the volume fraction of the γ' strengthening phase in the high-temperature alloy product is 30% to 50%, and the volume fraction of the TCP phase is 0% to 1%.

[0007] Preferably, the mass fractions of Cr and Co in the high-temperature alloy product satisfy the following condition: 32 ≤ Cr + Co ≤ 45.

[0008] Preferably, the mass fractions of W and Mo in the high-temperature alloy product satisfy the following condition: 5.5 ≤ W + Mo ≤ 10.

[0009] Preferably, the mass fractions of Al, Ti, Nb, and Ta in the high-temperature alloy product satisfy the following: 5% ≤ Al + Ti + Nb + Ta ≤ 8%.

[0010] Preferably, the mass fraction of B in the high-temperature alloy product is 0.02% to 0.05%, and / or the mass fraction of Zr is 0.02% to 0.2%.

[0011] Preferably, the high-temperature alloy product contains impurity elements Mn ≤ 0.05%; impurity elements V ≤ 0.04%; and the total mass of impurity rare earth elements ≤ 0.02%.

[0012] A molding method for additive manufacturing high-temperature alloy articles, used to prepare the above-mentioned additive manufacturing high-temperature alloy articles with excellent high-temperature strength and plasticity, comprising:

[0013] S1: Metal raw materials are smelted in proportion to obtain nickel-based high-temperature alloy ingots;

[0014] S2: High-temperature alloy powder for additive manufacturing is obtained by atomization powder preparation;

[0015] S3: High-temperature alloy preforms are obtained by additive manufacturing of high-temperature alloy powder;

[0016] S4: High-temperature alloy products are obtained by heat treatment of high-temperature alloy pre-products.

[0017] Preferably, the heat treatment in step S4 includes solution heat treatment and aging heat treatment performed sequentially.

[0018] Preferably, the high-temperature alloy preform is subjected to hot isostatic pressing before solution heat treatment.

[0019] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects:

[0020] (1) This invention controls the main elements as follows: Cr 10%–18%, Co 23.1%–28%, Mo 3.6%–6%, W 1.9%–6%, Al 1%–3%, Ti 3.42%–4.75%, Nb 1.01%–3%, and Ta The mass fraction of the γ' strengthening phase is controlled at 30%–50%, preferably 30%–45%, within the range of 0%–5% by mass; the volume fraction of the TCP phase is 0–0.3%; the volume fraction of the γ' strengthening phase in the prepared high-temperature alloy products is controlled at 30%–50%, preferably 30%–45%, with a density ≥99.5% and good printability; at 800℃, the tensile strength is 900MPa–1100MPa, the yield strength is 750MPa–1000MPa, the elongation is 6%–20%, and the reduction of area is 8%–20%; it overcomes the defects of existing technologies such as poor printability, poor high-temperature creep resistance, poor high-temperature strength and plasticity, and difficulty in balancing various indicators.

[0021] (2) By controlling the sum of Cr and Co elements and the sum of W and Mo elements within a limited range, this invention improves the solid solution strengthening effect of the alloy, thereby improving its high-temperature plasticity and creep resistance; at the same time, it can improve the high-temperature oxidation resistance of the alloy, further improving its high-temperature plasticity and creep resistance.

[0022] (3) By controlling the mass fractions of Al, Ti, Nb and Ta within a limited range, this invention can not only improve the volume ratio of the γ' phase and the high-temperature stability of the alloy through coherent strain strengthening, but also ensure a sufficient volume fraction of the γ′ phase to obtain better creep strength and mechanical strength above 800℃, while achieving higher strength and plasticity / toughness; overcoming the defects of existing technologies in that it is difficult to balance high-temperature creep resistance and high-temperature plasticity.

[0023] (4) By controlling the mass fraction of B and Zr within a limited range, the present invention helps to simultaneously improve creep resistance, plasticity and reduce cracks, overcoming the defects of the prior art such as poor high-temperature creep resistance, poor high-temperature plasticity, many cracks, poor density and difficulty in balancing multiple indicators.

[0024] (5) By controlling the upper limit of the mass fraction of impurity elements Mn, V and rare earth elements, this invention helps to suppress γ' phase coarsening, reduce unfavorable phase precipitation, improve high temperature stability, reduce fatigue cracks, improve density, improve service life, mechanical properties and printability.

[0025] (6) The present invention performs heat treatment in the order of hot isostatic pressing, solution heat treatment and aging heat treatment. On the one hand, it helps to further eliminate micropores or grain boundary microcracks that may remain after aging heat treatment, and improves density and printability. On the other hand, it can further release residual stress, which helps stress relaxation and microstructure stabilization, and reduces the risk of stress cracking in subsequent service. At the same time, hot isostatic pressing is conducive to uniform precipitation of alloying elements, avoids local over-aging or insufficient precipitation, improves microstructure consistency, and thus obtains more stable mechanical properties. In addition, hot isostatic pressing can reduce the quenching sensitivity of the material and inhibit the premature precipitation of alloying elements, which is conducive to the formation of highly supersaturated solid solutions and provides a good foundation for subsequent aging strengthening.

[0026] Other features and advantages of the invention will be set forth in the following description, and some advantages may become apparent from the description or be learned by practicing the invention. The objects and other advantages of the invention may be realized and obtained from the embodiments described and the accompanying drawings. Attached Figure Description

[0027] Figure 1a , 1b This is a metallographic diagram of the alloy in Example 1. Figure 1a In the horizontal direction, Figure 1bIt is in the vertical direction.

[0028] Figure 2a , 2b This is a metallographic diagram of the internal structure of alloy in Comparative Example 1. Figure 2a In the horizontal direction, Figure 2b It is in the vertical direction.

[0029] Figure 3a , 3b The image shows the metallographic structure of alloy 2 in Comparative Example. Figure 3a In the horizontal direction, Figure 3b It is in the vertical direction.

[0030] Figure 4a , 4b This is a metallographic diagram of the internal structure of alloy 3 in Comparative Example. Figure 4a In the horizontal direction, Figure 4b It is in the vertical direction.

[0031] Figure 5a , 5b This is a metallographic diagram of the internal structure of alloy 4 in Comparative Example. Figure 5a In the horizontal direction, Figure 5b It is in the vertical direction. Detailed Implementation

[0032] The preferred embodiments of the present invention will now be described in detail with reference to the accompanying drawings, which constitute a part of the present invention and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not intended to limit the present invention.

[0033] High-temperature alloy products often exhibit metallurgical defects such as voids, incomplete fusion, and cracks during additive manufacturing due to the diverse types and wide variations in the content of alloying elements. This results in low alloy density, substandard mechanical properties, and poor strength-ductility matching. Easily printable alloys, such as GH4169, have fewer defects but exhibit low strength-ductility above 800℃, making them unsuitable for practical applications. Conversely, difficult-to-print alloys, such as GH4720, have better high-temperature mechanical properties but poor printability.

[0034] On one hand, this invention discloses an additively manufactured high-temperature alloy product with excellent high-temperature strength and plasticity, comprising the following components by mass fraction: Cr 10%–18%, Co 23.1%–28%, Mo 3.6%–6%, W 1.9%–6%, Al 1%–3%, Ti 3.42%–4.75%, Nb 1.01%–3%, Ta 0%–5%, Fe 0%–8%, C 0.01%–0.5%, B 0%–0.05%, Zr 0%–0.2%, O 0–0.5%, N 0–0.2%, with the balance being Ni.

[0035] Preferably, the volume fraction of the γ′ strengthening phase in the high-temperature alloy product is 30% to 50%, and the volume fraction of the TCP phase is 0% to 1%. These characteristics help ensure that the alloy has high high-temperature strength, microstructure stability, and good printability.

[0036] More preferably, the volume fraction of the γ' strengthening phase in the high-temperature alloy product is 30% to 45%.

[0037] It should be noted that the γ′ phase is the core reinforcing phase. The more uniform its distribution, the smaller the size of the basic phase unit, for example, reaching a nanoscale distribution. A higher proportion, generally greater than 50%, helps to improve high-temperature stability and creep resistance at high temperatures; however, an excessively high proportion of the γ′ phase will exacerbate thermal cracking (liquefaction cracking or strain aging cracking) and reduce printability.

[0038] TCP phases (topologically close-packed phases, such as σ, μ, and P phases) can lead to the depletion of matrix solid solution elements and the initiation of brittle cracks due to the precipitation of some elements at grain boundaries / dendritic spaces (such as Cr, Mo, and W), which reduces stability, mechanical properties, and printability at high temperatures.

[0039] The applicant's research found that controlling the volume fraction of the γ' strengthening phase in high-temperature alloy products to 30%–50%, preferably 30%–45%, helps to improve the high-temperature strength, microstructure stability, and printability of the alloy by controlling the volume fraction of the TCP phase to below 1%.

[0040] Compared with existing technologies, this invention controls the mass range of the main elements Cr (10%–18%), Co (23.1%–28%), Mo (3.6%–6%), W (1.9%–6%), Al (1%–3%), Ti (3.42%–4.75%), Nb (1.01%–3%), and Ta (0%–5%) to prepare high-temperature alloy products with a volume fraction of γ′ strengthening phase of 30%–50%, preferably 30%–45%, a density ≥99.5%, and good printability. At 800℃, the tensile strength is 900MPa–1100MPa, the yield strength is 750MPa–1000MPa, the elongation is 6%–20%, and the reduction of area is 8%–20%. This invention overcomes the shortcomings of existing technologies, such as poor printability, poor high-temperature creep resistance, poor high-temperature strength and plasticity, and difficulty in balancing various indicators.

[0041] It should be noted that a Co mass fraction of 23.1% to 28% helps to improve the solid solution strengthening effect, increase the high-temperature strength of the matrix, reduce stacking fault energy, improve plasticity, and inhibit TCP (topological close-packed) phase precipitation.

[0042] A Cr mass fraction of 10% to 18% helps to form a Cr2O3 oxide film, improving its antioxidant and hot corrosion resistance; however, excessive Cr may promote the precipitation of the σ phase.

[0043] Preferably, the mass fractions of Cr and Co satisfy: 32≤Cr+Co≤45. Controlling the Cr and Co elements within this range can enhance the solid solution strengthening effect of the alloy, improve its high-temperature plasticity and creep resistance, and at the same time improve the high-temperature oxidation resistance of the alloy, further enhancing its high-temperature plasticity and creep resistance.

[0044] A Mo mass fraction of 3.6%–6% and a W mass fraction of 1.9%–6% help to generate solid solution strengthening through atomic size differences and improve creep resistance; at the same time, W can also increase the melting point; excess Mo may generate the δ phase.

[0045] Preferably, the mass fractions of W and Mo satisfy: 5.5≤W+Mo≤10; controlling W and Mo elements within this range can improve the solid solution strengthening effect of the alloy, and at the same time improve the high-temperature creep resistance and plasticity of the alloy.

[0046] Compared with the prior art, the present invention improves the solid solution strengthening effect of the alloy by controlling the sum of Cr and Co elements and the sum of W and Mo elements within a limited range, thereby improving the high-temperature plasticity and creep resistance; at the same time, it can improve the high-temperature oxidation resistance of the alloy, further improving the high-temperature plasticity and creep resistance.

[0047] The Al mass fraction of 1% to 3% and the Ti mass fraction of 1.5% to 4.75% help to form the γ'-Ni3(Al,Ti) phase, which improves the volume ratio of the γ' phase and the high-temperature stability of the alloy through coherent strain strengthening.

[0048] The mass fraction of Nb is 1.01% to 3%, and the mass fraction of Ta is 0% to 5%. Nb and Ta can partially replace Al / Ti in the γ' phase, improving the high-temperature stability of the alloy. At the same time, Nb can also inhibit grain boundary slip, and Ta can enhance oxidation resistance.

[0049] Preferably, the mass fractions of Al, Ti, Nb, and Ta satisfy the following condition: 5% ≤ Al + Ti + Nb + Ta ≤ 8%.

[0050] Further research by the applicant revealed that Al, Ti, Nb, and Ta are the main forming elements of γ′-Ni3 (Al,Ti,Nb,Ta), and their total amount directly determines the volume fraction of the γ′ phase. If the total mass fraction of Al, Ti, Nb, and Ta is too low, it is difficult to ensure a sufficient volume fraction of the γ′ phase, resulting in a decrease in creep strength and mechanical strength above 800℃. If the total mass fraction of Al, Ti, Nb, and Ta is too high, it leads to excessive coarsening of the γ′ phase, resulting in a strength-plasticity inversion, that is, when the strength of the material increases, the plasticity / toughness often decreases.

[0051] Compared with the prior art, this invention, by controlling the mass fractions of Al, Ti, Nb, and Ta within a defined range, can not only improve the volume ratio of the γ' phase and the high-temperature stability of the alloy through coherent strain strengthening, but also ensure a sufficient volume fraction of the γ′ phase, thereby obtaining better creep strength and mechanical strength above 800℃, while achieving higher strength and plasticity / toughness; it overcomes the shortcomings of the prior art in balancing high-temperature creep resistance and high-temperature plasticity.

[0052] A C mass fraction of 0.01% to 0.5% indicates that C contributes to the formation of MC (such as TiC / NbC) or M. 23 C6 carbides pin grain boundaries; excessive C may lead to grain boundary embrittlement.

[0053] A B mass fraction of 0%–0.05% and a Zr mass fraction of 0%–0.2% can agglomerate grain boundaries, enhance grain boundary bonding, reduce cracks, increase density, and improve printability; B improves creep plasticity, and Zr purifies grain boundaries; excessive amounts may generate low-melting-point borides.

[0054] Preferably, the mass fraction of B is 0.02% to 0.05%, which can be 0.02%, 0.03%, 0.04%, or 0.05%, and / or the mass fraction of Zr is 0.02% to 0.2%, which can be 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.10%, 0.11%, 0.12%, 0.13%, 0.14%, 0.15%, 0.16%, 0.17%, 0.18%, 0.19%, or 0.20%.

[0055] Compared with the prior art, the present invention helps to improve creep resistance, plasticity and reduce cracks by controlling the mass fraction of B and Zr within a limited range, thus overcoming the defects of the prior art such as poor high-temperature creep resistance, poor high-temperature plasticity, many cracks, poor density and difficulty in balancing multiple indicators.

[0056] A Fe mass fraction of 0% to 8% reduces costs and improves hot workability, but excessive amounts reduce high-temperature strength and oxidation resistance.

[0057] Preferably, the Fe mass fraction is 3% to 8%, which can be 3%, 4%, 5%, 6%, 7% or 8%.

[0058] The mass fraction of O is ≤0.5%, and the mass fraction of N is ≤0.2%. O and N are impurity elements. Controlling their content can prevent a decrease in overall mechanical properties, especially brittle fracture.

[0059] Preferably, the composition of high-temperature alloy products needs to control the following impurity components: Mn≤0.05%; V≤0.04%; total mass of rare earth elements (La, Ce, Y, etc.)≤0.02%.

[0060] It should be noted that controlling the upper limit of the impurity element Mn within the above range has the following advantages:

[0061] It can completely eliminate the risk of low-melting-point phases in the Mn system, such as the possibility that Mn may form a Ni-Mn eutectic (melting point 1140℃), which can trigger micro-region liquefaction cracks during rapid solidification.

[0062] It can reduce oxide film adhesion and powder spreading defects. For example, the composite oxide film of MnO and Al2O3 will reduce melt wettability, leading to powder spreading spheroidization during additive manufacturing and increasing density.

[0063] It can prevent the coarsening of the γ' phase. For example, Mn will segregate at the γ′ / γ interface during aging, which will accelerate the Ostwald ripening of the γ' phase and reduce the size stability of the γ' phase.

[0064] It should be noted that controlling the upper limit of impurity element V within the above range has the following advantages:

[0065] It can suppress the independent precipitation of the η phase (Ni3V). For example, V may form the η phase (lamellar brittle phase) through the Ni-Al-V ternary reaction.

[0066] It can reduce the fluctuation of laser reflectivity. For example, the reflectivity of the oxide of V (V2O5) is as high as 65% at AM laser wavelength (1064nm). Without V, the laser energy absorption is more stable (melting depth fluctuation <±5%).

[0067] Reduce the tendency of TCP phase formation; for example, V can promote σ phase precipitation, and the absence of V can extend the service life.

[0068] It should be noted that controlling the upper limit of rare earth elements as impurities within the above range has the following advantages:

[0069] It can avoid the "double contamination" of rare earth oxides. For example, rare earths (such as Ce) can combine with Al / Ti oxides to form REAlO3 composite inclusions (size > 2 μm), which become fatigue crack initiation sites. Without rare earths, the inclusion density is significantly reduced and the compaction density is significantly increased.

[0070] It can eliminate liquid metal embrittlement (LME). For example, rare earth eutectic with Ni (such as Ce-Ni, melting point 875℃) can induce HAZ liquefaction cracks, improving mechanical properties and printability.

[0071] Compared with existing technologies, this invention helps to suppress γ′ phase coarsening, reduce undesirable phase precipitation, improve high-temperature stability, reduce fatigue cracks, increase density, improve service life, mechanical properties, and printability by controlling the upper limit of the mass fraction of Mn, V, and rare earth elements.

[0072] On the other hand, this invention discloses a molding method for additive manufacturing high-temperature alloy articles, used to prepare the above-mentioned additive manufacturing high-temperature alloy articles with excellent high-temperature strength and plasticity, comprising:

[0073] S1: Metal raw materials are smelted in proportion to obtain nickel-based high-temperature alloy ingots;

[0074] S2: High-temperature alloy powder for additive manufacturing is obtained by methods such as atomization powder preparation;

[0075] S3: High-temperature alloy preforms are obtained by additive manufacturing of high-temperature alloy powder;

[0076] S4: High-temperature alloy products are obtained by heat treatment of high-temperature alloy pre-products.

[0077] Specifically, in steps S1 and S2, ingot casting and atomization powder production can be implemented using existing technical solutions.

[0078] Specifically, in step S3 of additive manufacturing, the laser power is 150W to 250W, which can be 150W, 160W, 170W, 180W, 190W, 200W, 210W, 220W, 230W, 240W or 250W.

[0079] Specifically, in step S3 of additive manufacturing, the scanning speed is 500mm / s to 1500mm / s, which can be 500mm / s, 600mm / s, 700mm / s, 800mm / s, 900mm / s, 1000mm / s, 1200mm / s, 1300mm / s, 1400mm / s or 1500mm / s.

[0080] Specifically, the heat treatment in step S4 includes solution heat treatment and aging heat treatment performed sequentially.

[0081] Specifically, step S4 includes:

[0082] Step S401 Solution heat treatment: 1050℃~1130℃, which can be 1050℃, 1060℃, 1080℃, 1090℃, 1100℃, 1120℃ or 1130℃; hold for 2h~10h and then air cool; the holding time can be 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h or 10h.

[0083] Step S402 Aging heat treatment: Hold at 700℃~850℃ for 4h~48h and then air cool.

[0084] It should be noted that solution heat treatment can eliminate segregation and some coarse strengthening phases, dissolve coarse γ′ phases, carbides / nitrides, TCP phases / η phases in the cast or printed state; homogenize dendritic segregation (Nb and Ti element enrichment commonly seen in additive manufacturing); and control grain size (through temperature / cooling rate).

[0085] It should be noted that aging heat treatment can precisely precipitate nanoscale γ' (Ni3Al / Ti / Nb) phase or (Ni3Nb) reinforcing phase; optimize size / distribution, exhibiting bimodal or unimodal distribution; and release residual stress (especially critical after additive manufacturing).

[0086] Preferably, the high-temperature alloy preform is subjected to hot isostatic pressing before solution heat treatment.

[0087] Specifically, the hot isostatic pressing conditions are 1100℃~1200℃, which can be 1100℃, 1120℃, 1130℃, 1140℃, 1150℃, 1160℃, 1170℃, 1180℃, 1190℃, or 1200℃.

[0088] It should be noted that the hot isostatic pressing temperature should be close to but lower than the alloy solution temperature to avoid complete re-dissolution of γ′. Excessive temperature can lead to coarsening / dissolution of the γ′ phase: the nano γ′ precipitated during aging may coarsen or partially dissolve at the high temperature of hot isostatic pressing (HIP), resulting in a decrease in strength. At the same time, excessive temperature carries the risk of recrystallization. If the HIP temperature exceeds the alloy recrystallization threshold (e.g., for single crystal alloys >1300℃), it may damage the oriented grains.

[0089] Specifically, the hot isostatic pressure is 100MPa to 200MPa, and can be 100MPa, 110MPa, 120MPa, 130MPa, 140MPa, 150MPa, 160MPa, 170MPa, 180MPa, 190MPa or 200MPa.

[0090] It should be noted that 100MPa can close >99% of <10μm pores; 200MPa can be used for large-size or high-crack-density parts.

[0091] Specifically, the hot isostatic pressing time is 2h to 4h; it can be 2h, 2.1h, 2.2h, 2.3h, 2.4h, 2.5h, 2.6h, 2.7h, 2.8h, 2.9h, 3.0h, 3.1h, 3.2h, 3.3h, 3.4h, 3.5h, 3.6h, 3.7h, 3.8h, 3.9h or 4h.

[0092] It should be noted that a hot isostatic pressing time of 2 hours is sufficient to achieve pore closure and diffusion healing; a time of more than 4 hours can easily lead to abnormal grain growth.

[0093] It should be noted that the hot isostatic pressing performed before aging treatment in this invention has the following advantages:

[0094] (1) Further eliminate micro-defects

[0095] Through the action of high temperature and high pressure inert gas, defects such as porosity, shrinkage porosity, and microcracks inside the casting are effectively closed, making the material close to the theoretical density; after the defects are reduced, stress concentration and crack initiation points are eliminated, significantly improving fatigue life, tensile strength and yield strength.

[0096] (2) The material after hot isostatic pressing is dense and uniform, and the alloying elements are more likely to precipitate uniformly during the subsequent solid solution and aging process; avoiding local over-aging or insufficient precipitation; improving the consistency of the structure, thereby obtaining more stable mechanical properties;

[0097] (3) Hot isostatic pressing achieves slow cooling under high pressure without producing quenching cracks, reducing the quenching sensitivity of the material; at the same time, it inhibits the premature precipitation of alloying elements, which is conducive to the formation of highly supersaturated solid solutions and provides a good foundation for subsequent age strengthening.

[0098] Compared with existing technologies, this invention performs heat treatment in the order of hot isostatic pressing (HIP), solution heat treatment, and aging heat treatment. On the one hand, this helps to further eliminate micropores or grain boundary microcracks that may remain after aging heat treatment, improving density and printability. On the other hand, it can further release residual stress, which helps stress relaxation and microstructure stabilization, reducing the risk of stress cracking during subsequent service. At the same time, HIP facilitates the uniform precipitation of alloying elements, avoids local over-aging or insufficient precipitation, and improves microstructure consistency, thereby obtaining more stable mechanical properties. In addition, HIP can reduce the quenching sensitivity of the material and inhibit the premature precipitation of alloying elements, which is conducive to the formation of highly supersaturated solid solutions, providing a good foundation for subsequent age hardening.

[0099] The above-mentioned additively manufactured high-temperature alloy products have a γ′ strengthening phase volume fraction controlled at 30%–50%, preferably 30%–45%; a TCP phase volume fraction of 0–0.3%; a density ≥99.5%, preferably ≥99.67%; good printability; and at 800℃, a tensile strength of 900 MPa–1100 MPa, a yield strength of 750 MPa–1000 MPa, an elongation of 6%–20%, and a reduction of area of ​​8%–20%.

[0100] To further illustrate the technical solution of the present invention, the following embodiments and comparative examples are provided:

[0101] Example 1

[0102] This embodiment discloses a forming method for additive manufacturing high-temperature alloy products, including the following steps:

[0103] S1: According to the given alloy element ratio, weigh a certain amount of raw materials such as Ni, Co, Cr, Al, Ti, W, Ta, Mo, Nb, Fe, C, B, Zr, etc., put the raw materials into a vacuum induction furnace, evacuate the equipment to a vacuum and start melting; after melting is completed, nickel-based high-temperature alloy ingots are obtained.

[0104] S2: The alloy ingot is placed in the gas atomization powder making furnace. After the equipment is evacuated to a vacuum, the alloy is remelted into a liquid state. The liquid metal flow is impacted by high-pressure inert gas, which breaks it into tiny droplets and solidifies it into powder. The alloy powder is then sieved to obtain high-temperature alloy powder (particle size 15–53 μm) suitable for additive manufacturing.

[0105] S3: Place the powder in the additive manufacturing equipment, and print when the equipment is evacuated and protected by inert gas. The laser power is 150W and the scanning speed is 500mm / s to obtain the additive manufacturing high temperature alloy.

[0106] S4: Hot isostatic pressing is applied to the alloy, wherein the hot isostatic pressing temperature is 1200℃, the pressure is 170MPa, and the time is 4 hours.

[0107] S5: The alloy was subjected to heat treatment. The solution heat treatment was carried out at 1070℃ for 4 hours and then air-cooled. The aging heat treatment was carried out at 760℃ for 16 hours and then air-cooled. The composition results of the high-temperature alloy products are shown in Table 1, and the test results of the mechanical properties of the high-temperature alloys are shown in Table 2.

[0108] Example 2

[0109] This embodiment discloses a forming method for additive manufacturing high-temperature alloy products, including the following steps:

[0110] S1: According to the given alloy element ratio, weigh a certain amount of raw materials such as Ni, Co, Cr, Al, Ti, W, Ta, Mo, Nb, Fe, C, B, Zr, etc., put the raw materials into a vacuum induction furnace, evacuate the equipment to a vacuum and start melting; after melting is completed, nickel-based high-temperature alloy ingots are obtained.

[0111] S2: The alloy ingot is placed in the gas atomization powder making furnace. After the equipment is evacuated to a vacuum, the alloy is remelted into a liquid state. The liquid metal flow is impacted by high-pressure inert gas, which breaks it into tiny droplets and solidifies it into powder. The alloy powder is then sieved to obtain high-temperature alloy powder (particle size 15–53 μm) suitable for additive manufacturing.

[0112] S3: Place the powder in the additive manufacturing equipment, and print when the equipment is evacuated and protected by inert gas. The laser power is 200W and the scanning speed is 1000mm / s to obtain the additive manufacturing high temperature alloy.

[0113] S4: Hot isostatic pressing is applied to the alloy, wherein the hot isostatic pressing temperature is 1100℃, the pressure is 200MPa, and the time is 3 hours.

[0114] S5: The alloy is subjected to heat treatment. The solution heat treatment is held at 1100℃ for 4 hours and then air-cooled. The aging heat treatment is held at 820℃ for 24 hours and then air-cooled. The composition results of the high-temperature alloy products are shown in Table 1, and the test results of the mechanical properties of the high-temperature alloys are shown in Table 2.

[0115] It should be noted that Examples 3-10 and Comparative Examples 1-9 have the same process conditions as Example 1, but the alloy element compositions are different.

[0116] Example 6 does not contain B compared to Example 1, Example 7 does not contain Zr compared to Example 1, and Example 10 does not contain Fe compared to Example 1. The corresponding changes are made up by Ni.

[0117] In Comparative Example 1, the sum of the mass fractions of Al, Ti, Nb, and Ta is 9.1%, which does not satisfy the condition: 5% ≤ Al + Ti + Nb + Ta ≤ 8%.

[0118] In Comparative Example 2, the sum of the mass fractions of W and Mo is 10.3%, which does not satisfy the condition: 5.5 ≤ W + Mo ≤ 10.

[0119] The combined mass fractions of Cr and Co in Comparative Example 3 are 27.4%, which does not satisfy the condition: 32 ≤ Cr + Co ≤ 45.

[0120] The combined mass fractions of W and Mo in Comparative Example 4 are 2%, which does not satisfy the condition: 5.5 ≤ W + Mo ≤ 10.

[0121] The mass fractions of O and N in Comparative Examples 5-7 do not meet the range defined by this invention.

[0122] Comparative Examples 8, 9, and 10 contain metals V, Mn, or rare earth Ce that are not within the scope of this invention.

[0123] Table 1. Composition (wt.%) of different additively manufactured nickel-based superalloys

[0124]

[0125]

[0126] Table 2 shows the test results of the mechanical properties of the nickel-based superalloys in the examples.

[0127]

[0128] It should be noted that the mechanical properties of nickel-based superalloys were tested in accordance with GB / T 228.2-2015 and GB / T 2039-2024 standards.

[0129] Density is represented by the area ratio of defect-free tissues using metallographic analysis; the volume ratio of γ′ phase and TCP phase is also obtained by the area ratio of different phases using metallographic analysis.

[0130] The results show:

[0131] In the high-temperature alloy products prepared in Examples 1-9, the volume fraction of the γ' strengthening phase is controlled at 30% to 50%, preferably 30% to 45%; the volume fraction of the TCP phase is 0% to 0.3%; the density is ≥99.5%, preferably ≥99.67%; and the printability is good. At 800°C, the tensile strength is 900 MPa to 1100 MPa, the yield strength is 750 MPa to 1000 MPa, the elongation is 6% to 20%, preferably 8% to 20%, and the reduction of area is 8% to 20%.

[0132] A comparison of Examples 6 / 7 / 10 and Example 1 shows that the addition of trace amounts of B and Zr can improve density, reduce crack formation, and improve printability; the addition of appropriate amounts of Fe can also improve density, reduce crack formation, and improve printability.

[0133] Comparing Example 1 and Comparative Examples 1-10, it can be seen that when the proportions of each element exceed the limits defined by the present invention, the mechanical properties and the volume ratio of the γ′ phase are significantly lower than those in Example 1 of the present invention.

[0134] Figures 1a-5b Metallographic images of Example 1 and Comparative Examples 1-4 are shown. The results are as follows:

[0135] The proportion of cracks in the metallographic images of Comparative Examples 1-4 is significantly higher than that in Example 1. Example 1 has no obvious cracks, higher density, and better printability.

[0136] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention.

Claims

1. An additively manufactured high-temperature alloy product with excellent high-temperature strength and plasticity, characterized in that, The composition by mass fraction is as follows: Cr 10%–18%, Co 23.1%–28%, Mo 3.6%–6%, W 1.9%–6%, Al 1%–3%, Ti 1.5%–4.75%, Nb 1.01%–3%, Ta 0%–5%, Fe 0%–8%, C 0.01%–0.5%, B 0%–0.05%, Zr 0%–0.2%, O 0–0.5%, N 0–0.2%, with the balance being Ni.

2. The additively manufactured high-temperature alloy product with excellent high-temperature strength and plasticity according to claim 1, characterized in that, The volume fraction of the γ' strengthening phase in the high-temperature alloy product is 30%–50%, and the volume fraction of the TCP phase is 0%–1%.

3. The additively manufactured high-temperature alloy product with excellent high-temperature strength and plasticity according to claim 1, characterized in that, The mass fractions of Cr and Co in the high-temperature alloy product satisfy the following condition: 32 ≤ Cr + Co ≤ 45.

4. The additively manufactured high-temperature alloy product with excellent high-temperature strength and plasticity according to claim 1, characterized in that, The mass fractions of W and Mo in the high-temperature alloy product satisfy the following condition: 5.5 ≤ W + Mo ≤ 10.

5. The additively manufactured high-temperature alloy product with excellent high-temperature strength and plasticity according to claim 1, characterized in that, The mass fractions of Al, Ti, Nb, and Ta in the high-temperature alloy product satisfy the following: 5% ≤ Al + Ti + Nb + Ta ≤ 8%.

6. The additively manufactured high-temperature alloy product with excellent high-temperature strength and plasticity according to claim 1, characterized in that, The high-temperature alloy product contains B with a mass fraction of 0.02% to 0.05%, and / or Zr with a mass fraction of 0.02% to 0.2%.

7. The additively manufactured high-temperature alloy product with excellent high-temperature strength and plasticity according to any one of claims 1-6, characterized in that, The high-temperature alloy product contains impurity elements Mn ≤ 0.05%; V ≤ 0.04%; and the total mass of rare earth impurities ≤ 0.02%.

8. A method for forming additively manufactured high-temperature alloy articles, used to prepare additively manufactured high-temperature alloy articles with excellent high-temperature strength and plasticity as described in any one of claims 1-7, characterized in that, include: S1: Metal raw materials are smelted in proportion to obtain nickel-based high-temperature alloy ingots; S2: High-temperature alloy powder for additive manufacturing is obtained by atomization powder preparation; S3: High-temperature alloy powder is additively manufactured to obtain high-temperature alloy preforms; S4: High-temperature alloy products are obtained by heat treatment of high-temperature alloy pre-products.

9. The forming method for additive manufacturing high-temperature alloy articles according to claim 8, characterized in that, The heat treatment in step S4 includes solution heat treatment and aging heat treatment performed sequentially.

10. The forming method for additive manufacturing high-temperature alloy articles according to claim 9, characterized in that, High-temperature alloy preforms undergo hot isostatic pressing before solution heat treatment.