Low-carbon green environment-friendly calcium siliceous material for aerated concrete as well as preparation method and application of low-carbon green environment-friendly calcium siliceous material

By preparing calcium-silica materials through low-temperature calcination of low-grade limestone and waste soil, and combining them with phosphogypsum, the problems of quality fluctuation of calcium materials and resource dependence of silica materials in the production of aerated concrete have been solved. This has enabled low-carbon and environmentally friendly aerated concrete production, reducing carbon emissions and improving product stability and strength.

CN120864811APending Publication Date: 2025-10-31JIAHUA SPECIAL CEMENT
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510876972.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-06-27
Publication Date
2025-10-31

AI Technical Summary

Technical Problem

In traditional aerated concrete production, the quality fluctuations and high carbon emissions of calcareous materials, as well as the resource dependence and supply limitations of siliceous materials, restrict the industry's green and low-carbon transformation and sustainable development. In particular, the utilization problems of low-grade limestone and silica sand/fly ash have not been effectively solved.

Method used

Calcium-silica materials are prepared by low-grade limestone and waste soil through low-temperature calcination. Combined with phosphogypsum to provide sulfate components, these materials replace traditional calcium-based materials, reducing the amount of silica materials used and forming a stable cementitious system.

Benefits of technology

This has enabled low-carbon and environmentally friendly production of aerated concrete, reducing carbon emissions, simplifying raw material costs, shortening the slurry thickening and hardening time, and improving product stability and strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120864811A_ABST
    Figure CN120864811A_ABST
Patent Text Reader

Abstract

The invention discloses a low-carbon green environment-friendly calcium siliceous material for aerated concrete as well as a preparation method and application thereof, and belongs to the technical field of building materials. The calcium-silicon material disclosed by the invention comprises the following mineral components in percentage by weight: 44 to 57 percent of C2S, 5 to 9 percent of C4AF, 12 to 15 percent of f-CaO and 1 to 2 percent of f-CaSO4. The preparation method comprises the following steps: analyzing the chemical components of the raw materials of low-grade limestone, limestone mining waste soil and phosphogypsum; calculating a burdening scheme according to formulas (1)-(6), and then burdening; and calcining the raw material at low temperature, cooling and grinding. The invention also discloses the calcium-silicon material prepared by adopting the method and application of the calcium-silicon material. The low-grade limestone and the mine waste soil are used for preparing the cementing material, the phosphogypsum is used for providing a sulfate component, synergistic recycling of the three kinds of solid waste is achieved, and the raw material cost of a traditional calcium material is reduced. The calcium-silicon material disclosed by the invention is low in calcination temperature and low in carbon emission; when the calcium-silicon material is used for preparing aerated concrete, the thickening and hardening of slurry can be accelerated, and the standing time can be shortened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of building materials technology, specifically relating to low-carbon, green and environmentally friendly calcium silicate materials for aerated concrete, their preparation methods and applications. Background Technology

[0002] Autoclaved aerated concrete (AAC) is valued for its low thermal conductivity (0.07–0.21 W / m·K) and low density (400–800 kg / m³). 3 With its excellent sound insulation and fire resistance properties, it has become an advanced material in the field of civil engineering. In the context of the global construction industry's active promotion of energy conservation and emission reduction, it is widely used in non-load-bearing walls, roofs, and exterior wall cladding in buildings in cold regions. With the deepening implementation of my country's "dual-carbon" strategy and the rapid development of prefabricated buildings, green buildings, and low-energy buildings, the aerated concrete industry urgently needs to transform towards low-energy consumption, green and low-carbon practices, and high quality.

[0003] In the production system of aerated concrete, ordinary silicate cement and quicklime are the main calcium sources, and their quality stability has a profound impact on product performance. Currently, commonly used building lime suffers from quality issues of under-burning and under-burning. Under-burned lime slakes too quickly, causing the slurry to thicken prematurely and leading to "air trapping"; under-burned lime slakes slowly and cannot fully react during the static resting phase, resulting in cracks after cutting or dimensional changes during autoclaving. Furthermore, the cement hydration process is difficult to precisely control due to variations in the types, amounts, and particle sizes of admixtures added by different manufacturers and production batches, also causing fluctuations in aerated concrete quality. More importantly, calcareous cementitious materials (quicklime and cement) account for as much as 71% of carbon emissions in the aerated concrete production process. Therefore, exploring the use of industrial waste and low-grade resources to calcine calcareous materials has become a key path to achieving green and low-carbon production.

[0004] Siliceous materials, as the core component of aerated concrete, directly determine the strength and stability of the product. Currently, silica sand and fly ash are the main siliceous raw materials used in factories, but both have significant drawbacks. Siliceous sand, as a natural mineral, can lead to resource depletion and ecological damage if over-exploited; while fly ash is a type of industrial solid waste that can be reused, its supply depends on the regional distribution of thermal power plants, resulting in raw material shortages and soaring transportation costs in areas far from power plants. This not only limits the balanced development and large-scale promotion of the aerated concrete industry, but also, in economically underdeveloped regions or areas undergoing energy structure transformation, the fragility of the raw material supply chain becomes a bottleneck for industry adoption. Given that siliceous materials account for as much as 60-70% of aerated concrete production, reducing their usage is of great significance for the sustainable development of the industry.

[0005] At the same time, the utilization of limestone resources in my country also faces severe challenges. Low-grade limestone has a CaO content of less than 50% and contains impurities such as SiO2, Al2O3, and MgO, making it difficult to meet the requirements for cement raw material proportioning and resulting in resource waste. The waste soil generated from limestone mining has a SiO2 content of less than 50% and is accompanied by components such as Al2O3, Fe2O3, and MgO. Its complex chemical composition makes it difficult to utilize effectively.

[0006] Therefore, overcoming the quality fluctuations and high carbon emissions of traditional calcium sources (quicklime / cement), as well as the resource dependence and supply limitations of traditional silicon sources (silica sand / fly ash), and constructing a new calcium / silica material system with stability, low carbon emissions, and high resource efficiency (especially utilizing low-grade materials and solid waste) as its core characteristics, is a key technological bottleneck for achieving the green and low-carbon transformation and sustainable development of the aerated concrete industry. Summary of the Invention

[0007] One objective of this invention is to provide a low-carbon, green, and environmentally friendly calcium-silica material for aerated concrete. This material is prepared using low-grade limestone and waste soil through low-temperature calcination, resulting in a calcium-silica material with a special mineral composition for aerated concrete. This material can completely replace traditional calcium-based materials such as cement and quicklime, while simultaneously reducing the amount of silica materials used, thus exhibiting significant low-carbon and environmental advantages.

[0008] The second objective of this invention is to provide a method for preparing the low-carbon, green, and environmentally friendly calcium silicate material for aerated concrete.

[0009] The third objective of this invention is to provide the application of this low-carbon, green, and environmentally friendly calcium silicate material for aerated concrete.

[0010] To achieve the above objectives, the technical solution adopted by the present invention is as follows:

[0011] The first aspect of this invention discloses a method for preparing a low-carbon, green, and environmentally friendly calcium silicate material for aerated concrete. This calcium silicate material comprises the following mineral components by weight percentage: C2S: 44-57%. C4AF: 5~9%, f-CaO: 12~15%, f-CaSO4: 1%~2%;

[0012] Its preparation method includes the following steps:

[0013] S1. Analyze the chemical composition of the raw materials: low-grade limestone, limestone mining waste soil, and phosphogypsum;

[0014] S2. Based on the mineral composition of the calcium silicate material and the chemical composition content of the raw materials, calculate the batching scheme according to the following relationship between mineral composition and chemical composition:

[0015]

[0016] w(Fe2 O 3) = 0.329w(C4) A F) Formula (4);

[0017]

[0018] In the above formula, w represents the mass of each substance, such as w(CaO) representing the mass of CaO;

[0019] S3. According to the batching scheme, weigh dry low-grade limestone, limestone mining waste soil and phosphogypsum to form raw meal;

[0020] S4. The raw material is calcined at low temperature, cooled, and ground to obtain the calcium-silica material.

[0021] In some embodiments of the present invention, the chemical composition of the low-grade limestone is as follows: CaO: 47-50 wt.%, SiO2: 4-8 wt.%, Al2O3: 1-2 wt.%, Fe2O3: 0.5-1 wt.%, MgO: 1-2 wt.%, and loss on ignition is 39-41 wt.%.

[0022] In some embodiments of the present invention, the chemical composition of limestone mining waste soil is as follows: CaO: 1-2 wt.%, SiO2: 42-45 wt.%, Al2O3: 12-14 wt.%, Fe2O3: 20-22 wt.%, MgO: 2-3 wt.%, and loss on ignition is 16-18 wt.%.

[0023] In some embodiments of the present invention, in step S3, the raw material is ground to a residue of less than 15% on an 80μm sieve;

[0024] In some embodiments of the present invention, in step S4, the raw material is calcined at 1180-1220°C for 0.5-2 hours; preferably, it is calcined at 1200°C for 1 hour.

[0025] In some embodiments of the present invention, the clinker obtained from calcination is ground using a ball mill until the residue on a 45μm square-hole sieve is 23%–25% and the specific surface area is 400±20 kg / m². 2 .

[0026] The second aspect of this invention discloses a low-carbon, green, and environmentally friendly calcium silicate material for aerated concrete, which is made by the above-described method.

[0027] The third aspect of this invention discloses the application of this calcium silicate material in the preparation of aerated concrete.

[0028] The fourth aspect of this invention discloses a method for preparing aerated concrete using the above-mentioned calcium silicate material, comprising the following steps:

[0029] Step 1. Calculate the calcium-silicon ratio of the calcium-silicon material based on its chemical composition.

[0030] Step 2. Control the CaO / SiO2 molar ratio in the system to be 0.5-0.8, and calculate the amount of additional silicon material to be added based on the calcium-silicon ratio calculated in Step 1;

[0031] Step 3. Weigh the calcium silicate material and silicate material according to the proportion, stir evenly, control the slurry consistency to 180 mm, and determine the amount of water; add 80% water and stir to obtain the initial slurry; determine the amount of aluminum powder paste according to the density of aerated concrete, add the remaining 20% ​​water and mix evenly, then add it to the initial slurry and stir to obtain the slurry.

[0032] Step 4. After injecting the slurry obtained in step 3 into the mold, pre-cur it at 42-47℃, and then demold it; then autoclave the green body to obtain autoclaved aerated concrete.

[0033] In some embodiments of the present invention, during autoclaving, the temperature and pressure are gradually increased to 180°C and 1.0 MPa saturated steam pressure over 2 hours, and the constant pressure is maintained for 8 hours. Then, the pressure is gradually released over 0.5 hours to finally obtain autoclaved aerated concrete.

[0034] The mechanism by which the calcium silicate material prepared in this invention is used in the preparation of aerated concrete is as follows:

[0035] The calcium-silica material of the present invention is calcined at 1200℃, and the resulting CaO crystals are small in size and have high hydration activity. When they come into contact with water, they can quickly hydrate to form Ca(OH)2, providing an alkaline environment for the gas production of aluminum powder.

[0036] In the initial hydration stage after mixing aerated concrete slurry (with sufficient water and relatively insufficient gypsum), calcium sulfoaluminate... The rapid reaction initially produces needle-like ettringite crystals (AFt) and alumina gel; once the gypsum is consumed, platy calcium monosulfoaluminate crystals (AFm) and alumina gel are subsequently formed. These early-formed large quantities of crystals (AFt and AFm) and gel-like alumina gel interweave, fill, and coagulate, rapidly thickening the slurry and causing it to initially solidify.

[0037] Furthermore, the applicant unexpectedly discovered that the calcium thioaluminate of the present invention... The hydration products can promote the hydration of C2S, resulting in the following reaction:

[0038] 6C2S+2AH3+10H2O+AFt→nC-S-H+3AFm

[0039] Within 4 hours of reaction, the hydration rate of C2S reached 16%, which is much higher than the hydration rate of C2S in ordinary Portland cement at the same hydration age, thus promoting the thickening and hardening of the slurry.

[0040] Compared with the prior art, the present invention has the following beneficial effects:

[0041] This invention is scientifically designed and ingeniously conceived. It creatively uses low-grade limestone (CaO<50wt%) and mine waste soil (SiO2<50wt%) to replace traditional limestone and siliceous materials to prepare cementitious materials. In addition, it uses phosphogypsum (an industrial by-product) to provide sulfate components, thereby achieving the synergistic resource utilization of the three solid wastes and reducing the raw material cost of traditional calcareous materials.

[0042] The calcium silicate material of this invention has a low calcination temperature, resulting in 30% energy savings in its preparation compared to ordinary silicate cement, thus significantly reducing carbon emissions. Furthermore, it reduces the amount of silicate material used to some extent.

[0043] Compared with ordinary silicate cement and calcium oxide as calcareous materials, the use of the calcium silicate material of this invention to prepare aerated concrete can accelerate the thickening and hardening of the slurry and shorten the static settling time. Attached Figure Description

[0044] Appendix Figure 1 This is an electron microscope image of the calcium-silicon material prepared in Example 1 of the present invention. Detailed Implementation

[0045] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially.

[0046] Example 1

[0047] As a preferred embodiment of the present invention, this embodiment discloses the low-carbon, green, and environmentally friendly refueling mixture of the present invention.

[0048] The concrete uses calcium silicate materials, and its mineral composition is: C2S: 50%. C4AF: 7%, f-CaO: 14%, f-CaSO4 2%.

[0049] The method for preparing low-carbon, green, and environmentally friendly calcium silicate materials for aerated concrete in this embodiment is as follows:

[0050] S1. The chemical composition of low-grade limestone, limestone mining waste soil and phosphogypsum was analyzed and calculated. The results are shown in Table 1.

[0051] Table 1 Chemical composition of raw materials (wt.%)

[0052] raw materials LOI <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> CaO MgO <![CDATA[SO3]]> low-grade limestone 40.13 6.04 1.77 0.73 49.00 1.10 / limestone mining waste 17.00 43.60 13.67 21.51 1.85 2.29 / phosphogypsum 28.84 / 0.32 0.15 29.30 / 41.00

[0053] S2. Based on the mineral composition of calcium silicate materials and the chemical composition of raw materials, the batching scheme is calculated according to formulas (1) to (6), and the following results are obtained: the amount of low-grade limestone is 54 wt.%, limestone mining waste is 40 wt.%, and phosphogypsum is 6 wt.%.

[0054] S3. According to the batching scheme, weigh dry low-grade limestone, limestone mining waste soil and phosphogypsum to form raw meal, and grind the raw meal through an 80μm sieve with a residue of 10.5%.

[0055] S4. Calcine the raw materials at 1200℃ and keep them at that temperature for 1 hour.

[0056] S5. Cool the calcined clinker and grind it in a ball mill until the residue on a 45μm square-hole sieve is 23% and the specific surface area is 380kg / m². 2 .

[0057] The electron micrograph of the calcium-silicon material prepared in this embodiment is attached. Figure 1 As shown in the figure. It can be seen from this figure that the calcium-silica material prepared by calcination consists of C2S, Composed of f-CaO. Wherein C2S and The particle size is approximately 1 μm, exhibiting high hydration activity; f-CaO is granular and also possesses high hydration activity. Accompanied by Growth.

[0058] Example 2

[0059] As a preferred embodiment of the present invention, this embodiment discloses the low-carbon, green, and environmentally friendly refueling mixture of the present invention.

[0060] The concrete uses calcium silicate materials, and its mineral composition is: C2S: 44%. C4AF: 9%, f-CaO: 15%, f-CaSO4 1%.

[0061] The method for preparing low-carbon, green, and environmentally friendly calcium silicate materials for aerated concrete in this embodiment is as follows:

[0062] S1. Analyze and calculate the chemical composition of low-grade limestone, limestone mining waste soil and phosphogypsum. The chemical composition of the low-grade limestone, limestone mining waste soil and phosphogypsum used in this embodiment is the same as in Example 1.

[0063] S2. Based on the mineral composition of calcium silicate materials and the chemical composition of raw materials, the batching scheme is calculated according to formulas (1) to (6), and the following results are obtained: the amount of low-grade limestone is 48 wt.%, limestone mining waste is 46 wt.%, and phosphogypsum is 6 wt.%.

[0064] S3. According to the batching scheme, weigh dry low-grade limestone, limestone mining waste soil and phosphogypsum to form raw meal, and grind the raw meal through an 80μm sieve with a residue of 12.8%.

[0065] S4. Calcine the raw materials at 1250℃ and keep them at that temperature for 1 hour.

[0066] S5. Cool the calcined clinker and grind it in a ball mill until the residue on a 45μm square-hole sieve is 20% and the specific surface area is 390kg / m². 2 .

[0067] Example 3

[0068] This embodiment discloses a method for preparing autoclaved aerated concrete, using the low-carbon, green, and environmentally friendly calcium silicate material for autoclaved aerated concrete from Example 1 as a raw material. The specific preparation method is as follows:

[0069] (1) Calculate the content of CaO and SiO2 in calcium-silica materials.

[0070] Based on the chemical composition of the calcium-silicon material in Example 1, the CaO content in the calcium-silicon material of Example 1 was calculated to be 64.4 wt.%, the SiO2 content was 22.5 wt.%, and the calcium-silicon molar ratio was 3.06.

[0071] (2) Calculate the amount of silica sand used.

[0072] In this embodiment, the silica sand used has an SiO2 content of 95 wt.%. Based on the calcium-silicon ratio of the calcium silicate material itself, the CaO / SiO2 molar ratio in the system is controlled at 0.7, and the calculated mass ratio of calcium silicate material to silica sand is 56:44. That is, adding an additional 44% silica sand is sufficient to meet the production process requirements and save on the amount of silicate material used.

[0073] (3) Preparation of slurry

[0074] Weigh out the calcium silicate material and silica sand according to the proportions, and stir them in a mixer for 1 minute. The amount of water used is 0.58% of the dry powder mass, and the amount of aluminum powder paste used is 0.12% of the dry powder mass. After adding 80% of the water, stir rapidly for 1 minute. Use the remaining water to mix the aluminum powder paste into the initial slurry, and then stir for another 30 seconds to obtain the slurry.

[0075] (4) Molding and curing

[0076] After injecting the slurry obtained in step (3) into the mold, it is first pre-cured at 45°C and then demolded. Finally, the green body is placed in an autoclave for curing: the temperature and pressure are gradually increased to 180°C and 1.0MPa saturated steam pressure over 2 hours, and the constant pressure is maintained for 8 hours. Then, the pressure is gradually released over 0.5 hours to finally obtain the autoclaved aerated concrete specimen.

[0077] Example 4

[0078] This embodiment discloses a method for preparing autoclaved aerated concrete, using the low-carbon, green, and environmentally friendly calcium silicate material for autoclaved aerated concrete from Example 2 as a raw material. The specific preparation method is as follows:

[0079] (1) Calculate the content of CaO and SiO2 in calcium-silica materials.

[0080] Based on the chemical composition of the calcium-silica material in Example 2, the CaO content in the calcium-silica material of Example 2 was calculated to be 64.1 wt.% and the SiO2 content was 15.25 wt.%.

[0081] (2) Calculate the amount of silica sand used.

[0082] In this embodiment, the silica sand used has an SiO2 content of 95 wt.%. Based on the calcium-silicon ratio of the calcium silicate material itself, the CaO / SiO2 molar ratio in the system is controlled at 0.7. The calculated mass ratio of calcium silicate material to silica sand is 53.5:46.5, meaning that adding an additional 46.5% silica sand is sufficient to meet the production requirements and save on the amount of silicate material used.

[0083] (3) Preparation of slurry

[0084] Weigh out the calcium silicate material and silica sand according to the specified proportions, and stir them in a mixer for 1 minute. The amount of water used is 0.58% of the dry powder mass, and the amount of aluminum powder paste used is 0.12% of the dry powder mass. After adding 80% of the water, stir rapidly for 1 minute. Use the remaining water to incorporate the aluminum powder paste into the initial slurry, and then stir for another 30 seconds to obtain the slurry.

[0085] (4) Molding and curing

[0086] After injecting the slurry obtained in step (3) into the mold, it is first pre-cured at 45°C and then demolded. Finally, the green body is placed in an autoclave for curing: the temperature and pressure are gradually increased to 180°C and 1.0MPa saturated steam pressure over 2 hours, and the constant pressure is maintained for 8 hours. Then, the pressure is gradually released over 0.5 hours to finally obtain the autoclaved aerated concrete specimen.

[0087] Comparative Example 1

[0088] This comparative example uses quicklime and P.O42.5R cement as calcareous materials. The CaO content in quicklime is 98 wt.%; the CaO content in P.O42.5R is 60 wt.% and the SiO2 content is 21 wt.%.

[0089] In the prior art, the mass ratio of quicklime to P.O42.5R cement in the calcareous material for preparing aerated concrete is 1:2. Based on this, the mass ratios of quicklime, P.O42.5R, and silica sand in the aerated concrete of this comparative example are calculated to be 16%, 32%, and 52%, respectively.

[0090] Prepare quicklime, P.O42.5R cement, and silica sand according to the above proportions, and prepare aerated concrete according to the method of Example 3.

[0091] Experimental Example 1

[0092] The aerated concrete prepared in Examples 3, 4, and Comparative Example 1 were subjected to performance tests. The test methods were as described above. The results are shown in Table 2.

[0093] Table 2. Bulk density and strength of aerated concrete

[0094] serial number Static time / h <![CDATA[Unit weight (kg / m 3 )]]> Strength / MPa Example 3 2~3h 615 5.3 Example 4 2~3h 618 5.5 Comparative Example 1 4h 608 5.6

[0095] As shown in Table 2, the calcium silicate cementitious material prepared by this invention can replace P.O42.5R and quicklime in the preparation of aerated concrete, which can shorten the static settling time and improve the demolding efficiency. The above-mentioned indicators were tested in accordance with GB / T11968-2020 "Autoclaved Aerated Concrete Blocks". The test results show that the density and strength of the aerated concrete meet the requirements of GB / T 11968-2020 "Autoclaved Aerated Concrete Blocks". This invention simplifies raw materials and saves some silicate materials, exhibiting significant energy-saving and environmental protection benefits.

[0096] The above description is merely a preferred embodiment of the invention and does not constitute any limitation on the invention. Any simple modifications, equivalent substitutions, and improvements made to the above embodiments based on the technical essence of the invention and within the spirit and principles of the invention shall still fall within the protection scope of the invention's technical solution.

Claims

1. A method for preparing a low-carbon, green, and environmentally friendly calcium silicate material for aerated concrete, characterized in that, The calcium-silica material comprises the following mineral components by weight percentage: C2S: 44-57%, C4AF: 5~9%, f-CaO: 12~15%, f-CaSO4: 1~2%; Its preparation method includes the following steps: S1. Analyze the chemical composition of the raw materials: low-grade limestone, limestone mining waste soil, and phosphogypsum; S2. Based on the mineral composition of the calcium silicate material and the chemical composition of the raw materials, the batching scheme is calculated according to formulas (1) to (6): w(Fe2O3)=0.329w(C4AF) formula (4); In the above formula, w represents the mass of each substance; S3. According to the batching scheme, weigh dry low-grade limestone, limestone mining waste soil and phosphogypsum to form raw meal; S4. The raw material is calcined at low temperature, cooled, and ground to obtain the calcium-silica material.

2. The method for preparing a low-carbon, green, and environmentally friendly calcium silicate material for aerated concrete according to claim 1, characterized in that, The chemical composition of low-grade limestone is as follows: CaO: 47-50 wt.%, SiO2: 4-8 wt.%, Al2O3: 1-2 wt.%, Fe2O3: 0.5-1 wt.%, MgO: 1-2 wt.%, and loss on ignition is 39-41 wt.%.

3. The method for preparing a low-carbon, green, and environmentally friendly calcium silicate material for aerated concrete according to claim 1, characterized in that, The chemical composition of limestone mining waste soil is as follows: CaO: 1-2 wt.%, SiO2: 42-45 wt.%, Al2O3: 12-14 wt.%, Fe2O3: 20-22 wt.%, MgO: 2-3 wt.%, and loss on ignition is 16-18 wt.%.

4. The method for preparing a low-carbon, green, and environmentally friendly calcium silicate material for aerated concrete according to claim 1, characterized in that, In step S3, the raw material is ground to a residue of less than 15% on an 80μm sieve.

5. The method for preparing a low-carbon, green, and environmentally friendly calcium silicate material for aerated concrete according to claim 1, characterized in that, In step S4, the raw materials are calcined at 1180–1220°C for 0.5–2 hours; preferably, they are calcined at 1200°C for 1 hour. The calcined clinker was ground in a ball mill until the residue on a 45μm square-hole sieve was 23%–25% and the specific surface area was 400±20 kg / m². 2 .

6. A low-carbon, green, and environmentally friendly calcium silicate material for aerated concrete, characterized in that, It is made by the method described in any one of claims 1-5.

7. The application of the calcium silicate material according to claim 6 in the preparation of aerated concrete.

8. A method for preparing aerated concrete using the calcium silicate material as described in claim 6, characterized in that, Includes the following steps: Step 1. Calculate the calcium-silicon ratio of the calcium-silicon material according to claim 6; Step 2. Control the CaO / SiO2 molar ratio in the system to be 0.5-0.8, and calculate the amount of additional silicon material to be added based on the calcium-silicon ratio calculated in Step 1; Step 3. Weigh the calcium silicate material and silicate material according to the proportion, stir evenly, control the slurry consistency to 180 mm, and determine the amount of water; add 80% water and stir to obtain the initial slurry; determine the amount of aluminum powder paste according to the density of aerated concrete, add the remaining 20% ​​water and mix evenly, then add it to the initial slurry and stir to obtain the slurry. Step 4. After injecting the slurry obtained in step 3 into the mold, pre-cur it at 42-47℃ for 4 hours, and then demold it; then autoclave the green body to obtain autoclaved aerated concrete.

9. The method for preparing aerated concrete according to claim 8, characterized in that, During autoclaving, the temperature and pressure are gradually increased to 180℃ and 1.0MPa saturated steam pressure over 2 hours. After maintaining constant pressure for 8 hours, the pressure is gradually released over 0.5 hours to finally produce autoclaved aerated concrete.