Bismuth titanate-polydopamine-silver iodate composite catalyst driven by ultrasonic and visible light as well as preparation method and application of bismuth titanate-polydopamine-silver iodate composite catalyst

By modifying polydopamine on the surface of bismuth titanate nanosheets and depositing silver iodate nanosheets, a dual-energy ultrasonic-visible light driven composite catalyst was formed, which solved the problem of low H2O2 synthesis efficiency under proton donor-free conditions and achieved high efficiency and stable catalytic performance.

CN120961223APending Publication Date: 2025-11-18HUBEI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202511121560.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-08-12
Publication Date
2025-11-18

AI Technical Summary

Technical Problem

Existing photocatalytic technologies have low efficiency in synthesizing H2O2 through photocatalytic oxygen reduction reactions without proton donors. This is hampered by low carrier mobility and rapid recombination of electron/hole pairs, and traditional methods increase production costs.

Method used

A dual-energy ultrasonic-visible-light driven bismuth titanate-polydopamine-silver iodate composite catalyst was designed. By modifying the surface of bismuth titanate nanosheets with polydopamine and depositing silver iodate nanosheets, a two-dimensional/two-dimensional composite structure was formed. The piezoelectric field of the core and the S-shaped heterojunction were used to promote carrier separation, avoiding the use of proton donors.

Benefits of technology

It achieves efficient catalytic performance for the synthesis of H2O2, simplifies the preparation process, reduces costs, maintains stable catalytic ability in multiple cycles of use, and improves photocatalytic efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120961223A_ABST
    Figure CN120961223A_ABST
Patent Text Reader

Abstract

The invention discloses an ultrasonic and visible light dual-energy driven bismuth titanate-polydopamine-silver iodate composite catalyst as well as a preparation method and application thereof. The preparation method comprises the following steps: S1, preparing a BTO nanosheet; s2, modifying the BTO nanosheet by using polydopamine; and S3, compounding the AIO with the BTO modified by the polydopamine. Nanosheet-layer bismuth titanate is used as an inner core, polydopamine is grafted for surface modification, then composite silver iodate nanosheets are deposited on the outer layer, the composite catalyst of a two-dimensional / two-dimensional composite structure in which BTO and AIO make full contact is formed, the composite catalyst has an inner core piezoelectric electric field, an S-type heterojunction and other built-in electric fields, and the BTO / AIO composite catalyst has the advantages that the BTO / AIO composite structure is obtained; the separation path of ultrasonic and visible light-generated carriers is shortened through multiple channels, the separation speed of the carriers is increased, the composite catalyst can be successfully used as an efficient composite catalyst for synthesizing H2O2, and a proton donor is not needed. The composite catalyst is simple in preparation process, low in cost, stable in catalytic performance and beneficial to popularization and application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the fields of materials science and catalysis, specifically to an ultrasonic-visible light dual-energy driven bismuth titanate-polydopamine-silver iodate composite catalyst, its preparation method, and its application. Background Technology

[0002] The overexploitation of non-renewable resources worldwide has brought about a severe energy crisis for human development. Photocatalysis, characterized by its high efficiency and environmental friendliness, has shown great potential in the green synthesis of hydrogen peroxide (H2O2) and is considered one of the most effective methods to solve the energy crisis. Traditional photocatalytic oxygen reduction reactions for H2O2 synthesis typically require exogenous proton donors, such as ethanol and isopropanol. This not only increases production costs but also reduces the generation of reactive oxygen species. Furthermore, proton donors are highly sensitive to photogenerated holes (h... + Excessive consumption of protons directly reduces the energy conversion efficiency of photocatalytic systems. Furthermore, in the absence of proton donors, traditional photocatalytic technologies suffer from low carrier mobility and reduced electron / hole pair ratios. - / h + The rapid recombination process presents a challenge. Therefore, designing a proton-donor-free, highly efficient catalytic system for H2O2 production remains a significant challenge.

[0003] Bi4Ti3O 12 Bismuth oxide (BTO) is a two-dimensional (2D) layered ferroelectric material. It is produced by bismuth oxide [Bi₂O₂]. 2+ Plate and perovskite structure [Bi2Ti3O] 10 ] 2- The regular stacking of the units forms an Olivieris structure. This sandwich-like, sheet-like stacking structure enhances the separation of photogenerated carriers through the formation of an interlayer electric field. Furthermore, the geometry of the nanosheets gives them excellent external pressure response, resulting in elastic deformation and a larger piezoelectric potential. This allows internal carriers to migrate to the surface via shorter paths, reducing recombination and promoting catalytic reactions, thus significantly improving catalytic efficiency. However, broad-spectrum light absorption and sufficient redox capacity remain challenges for this single-component photocatalyst. Moreover, severe charge recombination further limits photocatalytic efficiency. The construction of a stepped (S)-type heterojunction not only suppresses carrier recombination and achieves spatial separation but also maintains strong redox capacity, thereby improving the solar energy to H2O2 conversion efficiency.

[0004] AgIO3 (AIO) is a typical layered oxide photocatalyst. Its bandgap structure and crystal form are compatible with BTO, allowing for the construction of 2D / 2D S-type heterojunctions. Notably, compared to other common oxide photocatalysts, AIO can undergo photoexcitation-induced surface reconstruction to form narrow-bandgap AgI (AI). This not only broadens the light absorption range of the composite catalyst but also constructs a novel in-situ S-type heterojunction interface (AIO / AI) on the AIO surface, thereby shortening the carrier separation path. Furthermore, the formation of interfacial chemical bonds creates high-speed carrier transport channels, optimizing interfacial electron transport kinetics and significantly improving catalytic efficiency. In addition, to mitigate the difficulty of direct contact between the BTO and AIO phases due to lattice mismatch and interfacial stress, we developed a polydopamine (PDA)-modified BTO strategy. PDA can act as a flexible buffer region, further enhancing interfacial adhesion. Summary of the Invention

[0005] This invention provides an ultrasonic-visible light dual-energy driven bismuth titanate-polydopamine-silver iodate composite catalyst, its preparation method, and its application, aiming to overcome the shortcomings of existing technologies in the lack of efficient H2O2 generation catalytic systems characterized by proton-free donors.

[0006] The technical solution of this invention to solve the above-mentioned technical problems is as follows: A method for preparing an ultrasonic-visible light dual-energy driven bismuth titanate-polydopamine-silver iodate composite catalyst, comprising the following steps:

[0007] Preparation of S1.BTO nanosheets: KCl and NaCl were ground and homogenized in a mortar. Bi2O3 and TiO2 were then added to the mortar in proportion. After thorough grinding, the mixture was heated to 900℃ in air at a uniform rate and calcined for more than 2 hours. After cooling, it was washed multiple times with hot deionized water and then thoroughly dried to obtain BTO nanosheets for later use.

[0008] S2. Modification of BTO nanosheets with polydopamine: Dopamine was dissolved in Tris-HCl buffer to obtain a dopamine solution. Then, the BTO nanosheets prepared in S1 were dispersed in the dopamine solution to obtain a mixture. The mixture was stirred continuously at room temperature. After the reaction was complete, the product was collected by centrifugation. Then, it was washed several times with deionized water and ethanol alternately. Finally, it was dried in a vacuum drying oven to obtain polydopamine-modified BTO nanosheets, denoted as BTO@PDA nanosheets.

[0009] S3. Composite of AIO with polydopamine-modified BTO: Add BTO@PDA nanosheets and AgNO3 to a mixed solvent of deionized water and glycerol in a certain ratio. After ultrasonic treatment, a second mixture is obtained. Add I2O5 aqueous solution dropwise to the second mixture. After the addition is complete, a reaction solution is obtained. The molar ratio of Ag to I in the reaction solution is 1:1. Stir continuously for 20-60 min, filter to obtain the product, and then wash it repeatedly with deionized water and ethanol alternately. Then, vacuum dry at 40-70℃ for 4-12 h to obtain BTO@PDA / AIO nanosheets, which is the bismuth titanate-polydopamine-silver iodate composite catalyst.

[0010] Based on the above technical solution, the present invention can also make the following further specific choices or better choices.

[0011] Specifically, the molar ratio of KCl to NaCl in S1 is 1:0.7-1.5, the molar ratio of Bi2O3 to TiO2 is 1:1.5, and the mass ratio of Bi2O3 to KCl in the mortar is 0.47-0.94:2.24.

[0012] Specifically, in S1, the grinding and homogenization treatment refers to grinding for 10-20 minutes, thorough grinding refers to grinding for 1-3 hours, uniform heating refers to heating and rectification at 3.5-4.0℃ / min, the temperature of the hot deionized water used during washing is 80-100℃, and thorough drying refers to drying at 60-120℃ for 8-12 hours.

[0013] Specifically, the pH of the Tris-HCl buffer in S2 is 8.5, and the dopamine solution is prepared by mixing dopamine and Tris-HCl buffer at a volume ratio of 0.03-0.05g:100mL. The mass ratio of BTO nanosheets to dopamine in the first mixture is 0.24:0.03-0.05.

[0014] Specifically, continuous stirring and full reaction in S2 refers to continuous stirring and reaction at a speed of 550-1000 r / min for 10-24 hours.

[0015] Specifically, drying in S2 refers to drying in a vacuum drying oven at a temperature of 50-80℃ for 10-12 hours.

[0016] Specifically, in the mixed solvent of S3, the volume ratio of deionized water to glycerol is 30:5-10, the mass ratio of BTO@PDA nanosheets to AgNO3 is 0.2:0.017-0.068, and the volume ratio of BTO@PDA nanosheets to deionized water in mixed solution two is 0.2g:30-40mL.

[0017] Specifically, the concentration of the I₂O₅ aqueous solution in S₃ is (1.25-5)×10⁻⁶. -3mol / L, with a dropping rate of 1 drop every 1-3 seconds.

[0018] The present invention also provides an ultrasonic-visible light dual-energy driven bismuth titanate-polydopamine-silver iodate composite catalyst, which is prepared by the above method.

[0019] This invention also claims the application of the ultrasound-visible light dual-energy driven bismuth titanate-polydopamine-silver iodate composite catalyst in the preparation of hydrogen peroxide, wherein ultrasound and visible light are used as the reaction driving conditions during preparation.

[0020] Compared with the prior art, the beneficial effects of the present invention are:

[0021] The ultrasound-visible light dual-energy driven bismuth titanate-polydopamine-silver iodate composite catalyst (BTO@PDA / AIO catalyst) designed in this invention uses sheet-like bismuth titanate as the core, grafted with polydopamine for surface modification, and then deposited with composite silver iodate nanosheets on the outer layer, forming a two-dimensional / two-dimensional composite structure with full contact between BTO and AIO. It possesses built-in electric fields such as the core piezoelectric field and the S-shaped heterojunction. The multi-channel design shortens the separation path of ultrasonic and visible light-generated carriers, and the multi-element driving mechanism promotes the carrier separation rate. It can be successfully used as a highly efficient composite catalyst for ultrasound / visible light dual-energy driven synthesis of H2O2 without the need for a proton donor. The preparation process of this composite catalyst is simple, the experiment is highly reproducible, the raw materials are widely available, and the cost is low, which is conducive to industrial application. Its catalytic performance is stable, maintaining high catalytic capacity even after multiple cycles of use, and it can be used for a long time. Attached Figure Description

[0022] Figure 1 Field emission scanning electron microscope (FESEM) images of the composite catalysts and some intermediate products prepared in Example 3, Comparative Example 1, and Comparative Example 2 of this invention, where (a) is BTO, (b) is BTO@PDA, (c) is AIO, (d) is BTO@PDA / AIO-3, (e) is BTO / AIO-1, and (f) is BTO / AIO-3.

[0023] Figure 2 XRD patterns of the composite catalysts and some intermediate products prepared in the corresponding embodiments;

[0024] Figure 3 The graphs show the catalytic ability test results, where (a) is the UV absorption graph of BTO@PDA / AIO-3 catalyzing the generation of H2O2, (b) is the performance graph of photocatalytic generation of H2O2 for different samples, and (c) is the efficiency graph of BTO@PDA / AIO-3 generating H2O2 under different conditions.

[0025] Figure 4 This is a catalytic diagram of 6 cycles of BTO@PDA / AIO-3. Detailed Implementation

[0026] The technical solutions provided by the present invention will be clearly and completely described below with reference to the accompanying drawings and specific embodiments. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0027] Unless otherwise specified, all raw materials used in the following examples are commercially available products, and all methods used are conventional methods in the art.

[0028] To facilitate comparison of the microstructures of BTO nanosheets and AIO nanosheets, and also to easily observe the difference between the catalyst obtained by directly combining the two and the catalyst obtained by first modifying BTO nanosheets with polydopamine and then combining them with AIO nanosheets, this invention, in addition to preparing BTO nanosheets in the following examples, also separately prepared pure AIO nanosheets, as detailed below:

[0029] Preparation of AIO nanosheets: 60 mL of I2O5 solution containing 0.067 g of I2O5 was added to 200 mL of aqueous solution containing 0.68 g of AgNO3. After stirring the reaction thoroughly, the product was obtained by filtration. After washing with deionized water and ethanol alternately several times, the product was dried under vacuum to obtain powder, which is AIO nanosheets.

[0030] The following examples illustrate in detail the ultrasonic-visible light dual-energy driven bismuth titanate-polydopamine-silver iodate composite catalyst and its preparation method provided by the present invention.

[0031] Example 1

[0032] A method for preparing an ultrasonic-visible light dual-energy driven bismuth titanate-polydopamine-silver iodate composite catalyst, comprising the following steps:

[0033] Preparation of S1.BTO nanosheets: 2.24g KCl and 2.64g NaCl were placed in an agate mortar and ground and homogenized for 10min. Then, 0.70g Bi2O3 and 0.18g TiO2 were added to the mortar and ground thoroughly for 2h. The homogenized powder and the mortar were placed in air and heated to 900℃ at a heating rate of 4℃ / min. The powder was calcined at this temperature for 2h. After the product cooled naturally, it was washed three times with deionized water at 80℃. Finally, it was dried at 60℃ for 12h to obtain BTO nanosheets (powder) for later use.

[0034] S2. Modification of BTO nanosheets with polydopamine: 0.05 g of dopamine was dissolved in 100 mL of Tris-HCl buffer (pH 8.5) to form a dopamine solution. Then, 0.24 g of BTO nanosheet powder was dispersed in the dopamine solution to obtain mixture one. The mixture was stirred continuously at 650 r / min at room temperature for 24 h. After the reaction was complete, the product was collected by centrifugation. The product was then washed three times alternately with deionized water and ethanol. Finally, it was dried in a vacuum drying oven at 50 °C for 12 h to obtain polydopamine-modified BTO nanosheets, denoted as BTO@PDA nanosheets.

[0035] S3. Composite of AIO with polydopamine-modified BTO: 0.2 g of BTO@PDA nanosheets and 0.017 g of AgNO3 were added to a mixed solvent consisting of 30 mL of deionized water and 10 mL of glycerol. After ultrasonic treatment, a second mixture was obtained. 20 mL of I2O5 aqueous solution with a molar concentration of 1.25 mmol / L was added dropwise to the second mixture at a rate of 1 drop / second. After the addition was complete, a reaction solution was obtained. The molar ratio of Ag to I in the reaction solution was 1:1. The mixture was stirred continuously for 60 min, filtered to obtain the product, and then washed repeatedly with deionized water and ethanol alternately. The product was then vacuum dried at 50 °C for 12 h to obtain the bismuth titanate-polydopamine-silver iodate composite catalyst, denoted as BTO@PDA / AIO-1.

[0036] Example 2

[0037] The steps are basically the same as in Example 1, except that the amount of AgNO3 in S3 is 0.023g and the concentration of I2O5 aqueous solution is adjusted accordingly. The bismuth titanate-polydopamine-silver iodate composite catalyst finally obtained in this example is denoted as BTO@PDA / AIO-2.

[0038] Example 3

[0039] The steps are basically the same as in Example 1, except that the amount of AgNO3 in S3 is 0.034g and the concentration of I2O5 aqueous solution is adjusted accordingly. The bismuth titanate-polydopamine-silver iodate composite catalyst finally obtained in this example is denoted as BTO@PDA / AIO-3.

[0040] Example 4

[0041] The steps are basically the same as in Example 1, except that the amount of AgNO3 in S3 is 0.051g and the concentration of I2O5 aqueous solution is adjusted accordingly. The bismuth titanate-polydopamine-silver iodate composite catalyst finally obtained in this example is denoted as BTO@PDA / AIO-4.

[0042] Example 5

[0043] The steps are basically the same as in Example 1, except that the amount of AgNO3 in S3 is 0.068g and the concentration of I2O5 aqueous solution is adjusted accordingly. The bismuth titanate-polydopamine-silver iodate composite catalyst finally obtained in this example is denoted as BTO@PDA / AIO-5.

[0044] Example 6

[0045] A method for preparing an ultrasonic-visible light dual-energy driven bismuth titanate-polydopamine-silver iodate composite catalyst, comprising the following steps:

[0046] Preparation of S1.BTO nanosheets: 2.24g KCl and 1.23g NaCl were placed in an agate mortar and ground and homogenized for 15min. Then, 0.47g Bi2O3 and 0.12g TiO2 were added to the mortar and ground thoroughly for 1.5h. The homogenized powder and the mortar were placed in air and heated to 900℃ at a heating rate of 4.5℃ / min. The powder was calcined at this temperature for 2 hours. After the product cooled naturally, it was washed three times with 100℃ deionized water. Finally, it was dried at 120℃ for 8h to obtain BTO nanosheets (powder) for later use.

[0047] S2. Modification of BTO nanosheets with polydopamine: 0.03 g of dopamine was dissolved in 100 mL of Tris-HCl buffer (pH 8.5) to form a dopamine solution. Then, 0.24 g of BTO nanosheet powder was dispersed in the dopamine solution to obtain mixture one. The mixture was stirred continuously at 1100 r / min for 10 h at room temperature. After the reaction was complete, the product was collected by centrifugation. The product was then washed three times alternately with deionized water and ethanol. Finally, it was dried in a vacuum drying oven at 80 °C for 10 h to obtain polydopamine-modified BTO nanosheets, denoted as BTO@PDA nanosheets.

[0048] S3. Composite of AIO with polydopamine-modified BTO: 0.2 g of BTO@PDA nanosheets and 0.017 g of AgNO3 were added to a mixed solvent consisting of 30 mL of deionized water and 10 mL of glycerol. After ultrasonic treatment, a second mixture was obtained. 20 mL of I2O5 aqueous solution with a molar concentration of 1.25 mmol / L was added dropwise to the second mixture at a rate of 1 drop / 2 seconds. After the addition was complete, a reaction solution was obtained. The molar ratio of Ag to I in the reaction solution was 1:1. The mixture was stirred continuously for 40 min, filtered to obtain the product, and then washed repeatedly with deionized water and ethanol alternately. The product was then vacuum dried at 40 °C for 12 h to obtain the bismuth titanate-polydopamine-silver iodate composite catalyst, denoted as BTO@PDA / AIO-6.

[0049] Example 7

[0050] A method for preparing an ultrasonic-visible light dual-energy driven bismuth titanate-polydopamine-silver iodate composite catalyst, comprising the following steps:

[0051] Preparation of S1.BTO nanosheets: 2.24g KCl and 1.96g NaCl were placed in an agate mortar and ground and homogenized for 10min. Then, 0.94g Bi2O3 and 0.24g TiO2 were added to the mortar and ground thoroughly for 1h. The homogenized powder and the mortar were placed in air and heated to 900℃ at a heating rate of 3.5℃ / min. The powder was calcined at this temperature for 2 hours. After the product cooled naturally, it was washed three times with deionized water at 90℃. Finally, it was dried at 100℃ for 10h to obtain BTO nanosheets (powder) for later use.

[0052] S2. Modification of BTO nanosheets with polydopamine: Dissolve 0.03-0.05 g of dopamine in 100 mL of Tris-HCl buffer (pH 8.5) to obtain a dopamine solution. Then disperse 0.24 g of BTO nanosheet powder in the dopamine solution to obtain mixture one. Stir continuously at 550 r / min at room temperature for 24 h. After the reaction is complete, centrifuge to collect the product. Then wash with deionized water and ethanol three times alternately. Finally, dry in a vacuum drying oven at 50 °C for 12 h to obtain polydopamine-modified BTO nanosheets, denoted as BTO@PDA nanosheets.

[0053] S3. Composite of AIO with polydopamine-modified BTO: 0.2 g of BTO@PDA nanosheets and 0.034 g of AgNO3 were added to a mixed solvent consisting of 30 mL of deionized water and 10 mL of glycerol. After ultrasonic treatment, a second mixture was obtained. 20 mL of I2O5 aqueous solution with a molar concentration of 2.5 mmol / L was added dropwise to the second mixture at a rate of 1 drop / 3 seconds. After the addition was complete, a reaction solution was obtained. The molar ratio of Ag to I in the reaction solution was 1:1. The mixture was stirred continuously for 20 min, filtered to obtain the product, and then washed repeatedly with deionized water and ethanol alternately. The product was then vacuum dried at 70 °C for 4 h to obtain the bismuth titanate-polydopamine-silver iodate composite catalyst, denoted as BTO@PDA / AIO-7.

[0054] Comparative Example 1

[0055] A method for preparing a polydopamine-free bismuth titanate-silver iodate composite catalyst, the specific steps of which are as follows:

[0056] S1. Preparation of BTO nanosheets: 2.24g KCl and 2.64g NaCl were placed in an agate mortar and ground and homogenized for 10min. Then, 0.70g Bi2O3 and 0.18g TiO2 were added to the mortar and ground thoroughly for 2h. The homogenized powder and the mortar were placed in air and heated to 900℃ at a heating rate of 4℃ / min. The powder was calcined at this temperature for 2h. After the product cooled naturally, it was washed three times with deionized water at 80℃. Finally, it was dried at 60℃ for 12h to obtain BTO nanosheets (powder) for later use.

[0057] S2. Preparation of BTO-AIO composite catalyst: 0.2 g of BTO nanosheets and 0.017 g of AgNO3 were added to a mixed solvent consisting of 30 mL of deionized water and 10 mL of glycerol. After ultrasonic treatment, a mixed solution was obtained. 20 mL of I2O5 aqueous solution with a molar concentration of 1.25 mmol / L was added dropwise to the mixed solution at a rate of 1 drop / second. After the addition was complete, a reaction solution was obtained. The molar ratio of Ag to I in the reaction solution was 1:1. The mixture was stirred continuously for 60 min, filtered to obtain the product, and then washed repeatedly with deionized water and ethanol alternately. Subsequently, it was vacuum dried at 60 °C for 12 h to obtain the bismuth titanate-silver iodate composite catalyst, denoted as BTO / AIO-1.

[0058] Comparative Example 2

[0059] The steps are basically the same as those in Comparative Example 1, with the only difference being that the amount of AgNO3 used in S2 is 0.34g and the concentration of the I2O5 aqueous solution is adjusted accordingly. The final bismuth titanate-silver iodate composite catalyst is denoted as BTO / AIO-3.

[0060] To verify the successful fabrication of the acoustic-visible-light dual-energy driven bismuth titanate-polydopamine-silver iodate composite catalyst of this invention, field emission scanning electron microscopy (FEM) was performed on the following samples: BTO nanosheets prepared in step S1 of Example 1, BTO@PDA prepared in step S2, BTO@PDA / AIO-3 prepared in Example 3, BTO / AIO-1 prepared in Comparative Example 1, BTO / AIO-3 prepared in Comparative Example 2, and AIO prepared separately. The obtained SEM images are shown below. Figure 1 As shown in a to f. Specifically, as Figure 1 As shown in the field emission scanning electron microscope (FE-SEM) images corresponding to a and b, both BTO and AIO are 2D nanosheet structures. Initially, we attempted to construct a heterojunction with direct contact between BTO and AIO to enhance electron transfer; however, as... Figure 1As shown in e and f, in the BTO / AIO composite materials corresponding to high and low concentrations of AIO, BTO and AIO are grown separately without being tightly bonded, leading to easy recombination of photogenerated electrons and holes and poor performance in generating hydrogen peroxide. The main reason for the above problems in direct composite is that the highly exposed (008) crystal planes of BTO nanosheets (such as...) Figure 2 a) Low surface energy leads to weak interfacial bonding between the two phases, making them easily peeled off. Therefore, we propose a method of modifying BTO nanosheets with PDA (polydopamine) to introduce active groups and strengthen interfacial bonding, while using PDA as a flexible buffer layer to reduce interfacial stress and lattice mismatch between the two phases. Figure 1 As shown in c and d, PDA will be uniformly attached to the BTO surface, which is conducive to the deposition of AIO, and finally forms a BTO@PDA / AIO composite catalyst.

[0061] The present invention also performed XRD analysis on the BTO@PDA prepared in Example 1, BTO@PDA / AIO-1 prepared in Example 1, BTO@PDA / AIO-2 prepared in Example 2, BTO@PDA / AIO-3 prepared in Example 3, BTO@PDA / AIO-4 prepared in Example 4, and BTO@PDA / AIO-5 prepared in Example 5, and the results are as follows. Figure 2 As shown. Analysis Figure 2 It can be seen that the intensity of the characteristic peak of the (041) crystal plane increases with the increase of AIO loading, verifying the successful preparation of the BTO@PDA / AIO composite catalyst. In addition, no impurity phases appeared in the composite catalyst, and each sample also showed good crystal form and good mechanical strength.

[0062] To verify that the catalyst possesses dual-energy ultrasonic and visible light-driven hydrogen peroxide preparation capabilities, the composite catalysts prepared in each example and some intermediate products were used as samples for the following catalytic performance tests:

[0063] A 300 W xenon lamp was used as the light source, and an ultrasonic disperser was used to provide ultrasound. First, 10 mg of the composite catalyst or corresponding intermediate product from the respective embodiment was mixed with 20 mL of deionized water in a double-layered quartz beaker and stirred in the dark for 20 min to reach adsorption-desorption equilibrium. Then, the light source and ultrasound were turned on to initiate the catalytic reaction. Next, 0.2 mL of the reaction solution was filtered through a filter and diluted with 0.8 mL of water. Then, 2 mL of a mixed solution of potassium iodide (0.1 mol / L) and 0.05 mL of ammonium molybdate (0.01 mol / L) was added, and the mixture was allowed to stand for 10 min. Finally, the concentration of H2O2 produced was analyzed at 350 nm using a UV-Vis spectrometer. Figure 3 a). For example Figure 3As shown in b, all prepared catalysts exhibited good performance in solar energy conversion to H2O2 without the addition of proton donor sacrificial agents. Among them, BTO@PDA / AIO-3 in Example 3 showed the best performance, with a corresponding catalytic efficiency as high as 83.99 mM g. -1 h -1 Furthermore, to investigate the effects of different conditions on the H2O2 generation efficiency, various test conditions were introduced under the same conditions, including darkness, ultrasound (US), ultrasound and light (US+light), nitrogen (N2), oxygen (O2), ethanol, chloroform, silver nitrate (AgNO3), disodium ethylenediaminetetra( ... Figure 3 As shown in Figure c, under the assistance of ultrasound, the BTO@PDA / AIO catalyst exhibits a piezoelectric effect, forming a piezoelectric internal electric field that promotes the directional movement and separation of charge carriers, resulting in a 26.3% increase in catalytic efficiency compared to single photoexcitation. Corresponding gas and free radical scavenging experiments indicate that this composite catalyst converts its own generated hydroxyl radicals and superoxide radicals into H2O2 through a dual-channel reaction involving oxygen reduction and water oxidation. This promotes the separation of photogenerated electron-hole pairs, avoids carrier recombination, and enables efficient piezoelectric photocatalytic production of H2O2 in air without the need for a proton donor sacrificial agent. After centrifugation, washing, and drying, the used BTO@PDA / AIO-3 catalyst was reused as a catalyst and tested in six cycles according to the above catalytic testing procedures. The experimental results are shown in [Figure number missing]. Figure 4 It can be seen that the product obtained by the present invention has stable catalytic activity.

[0064] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for preparing an ultrasonic-visible light dual-energy driven bismuth titanate-polydopamine-silver iodate composite catalyst, characterized in that, Includes the following steps: Preparation of S1.BTO nanosheets: KCl and NaCl were ground and homogenized in a mortar. Bi2O3 and TiO2 were then added to the mortar in proportion. After thorough grinding, the mixture was heated to 900℃ in air at a uniform rate and calcined for more than 2 hours. After cooling, it was washed multiple times with hot deionized water and then thoroughly dried to obtain BTO nanosheets for later use. S2. Modification of BTO nanosheets with polydopamine: Dopamine was dissolved in Tris-HCl buffer to obtain a dopamine solution. Then, the BTO nanosheets prepared in S1 were dispersed in the dopamine solution to obtain a mixture. The mixture was stirred continuously at room temperature. After the reaction was complete, the product was collected by centrifugation. Then, it was washed several times with deionized water and ethanol alternately. Finally, it was dried in a vacuum drying oven to obtain polydopamine-modified BTO nanosheets, denoted as BTO@PDA nanosheets. S3. Composite of AIO with polydopamine-modified BTO: Add BTO@PDA nanosheets and AgNO3 to a mixed solvent of deionized water and glycerol in a certain ratio. After ultrasonic treatment, a second mixture is obtained. Add I2O5 aqueous solution dropwise to the second mixture. After the addition is complete, a reaction solution is obtained. The molar ratio of Ag to I in the reaction solution is 1:

1. Stir continuously for 20-60 min, filter to obtain the product, and then wash it repeatedly with deionized water and ethanol alternately. Then, vacuum dry at 40-70℃ for 4-12 h to obtain BTO@PDA / AIO nanosheets, which is the bismuth titanate-polydopamine-silver iodate composite catalyst.

2. The preparation method of the ultrasonic-visible light dual-energy driven bismuth titanate-polydopamine-silver iodate composite catalyst according to claim 1, characterized in that, The molar ratio of KCl to NaCl in S1 is 1:0.7-1.5, the molar ratio of Bi2O3 to TiO2 is 1:1.5, and the mass ratio of Bi2O3 to KCl in the mortar is 0.47-0.94:2.

24.

3. The preparation method of the ultrasonic-visible light dual-energy driven bismuth titanate-polydopamine-silver iodate composite catalyst according to claim 1, characterized in that, In S1, grinding and homogenization treatment refers to grinding for 10-20 minutes, thorough grinding refers to grinding for 1-3 hours, uniform heating refers to heating and rectification at 3.5-4.0℃ / min, the temperature of the hot deionized water used for washing is 80-100℃, and thorough drying refers to drying at 60-120℃ for 8-12 hours.

4. The preparation method of the ultrasonic-visible light dual-energy driven bismuth titanate-polydopamine-silver iodate composite catalyst according to claim 1, characterized in that, The pH of the Tris-HCl buffer in S2 is 8.

5. The dopamine solution is prepared by mixing dopamine and Tris-HCl buffer at a volume ratio of 0.03-0.05 g: 100 mL. The mass ratio of BTO nanosheets to dopamine in the first mixture is 0.24: 0.03-0.

05.

5. The preparation method of the ultrasonic-visible light dual-energy driven bismuth titanate-polydopamine-silver iodate composite catalyst according to claim 1, characterized in that, The continuous stirring and full reaction in S2 refers to the continuous stirring and reaction at a speed of 550-1000 r / min for 10-24 h.

6. The preparation method of the ultrasonic-visible light dual-energy driven bismuth titanate-polydopamine-silver iodate composite catalyst according to claim 1, characterized in that, The drying in S2 refers to drying in a vacuum drying oven at a temperature of 50-80℃ for 10-12 hours.

7. The preparation method of the ultrasonic-visible light dual-energy driven bismuth titanate-polydopamine-silver iodate composite catalyst according to claim 1, characterized in that, In the mixed solvent of S3, the volume ratio of deionized water to glycerol is 30:5-10, and the mass ratio of BTO@PDA nanosheets to AgNO3 is 0.2:0.017-0.

068. In mixed solution two, the volume ratio of BTO@PDA nanosheets to deionized water is 0.2g:30-40mL.

8. The preparation method of the ultrasonic-visible light dual-energy driven bismuth titanate-polydopamine-silver iodate composite catalyst according to claim 1, characterized in that, The concentration of the I₂O₅ aqueous solution in S₃ is (1.25-5)×10⁻⁶. -3 mol / L, with a dropping rate of 1 drop every 1-3 seconds.

9. A dual-energy ultrasonic-visible-light driven bismuth titanate-polydopamine-silver iodate composite catalyst, characterized in that, It is prepared by the method according to any one of claims 1 to 8.

10. The application of the ultrasonic-visible light dual-energy driven bismuth titanate-polydopamine-silver iodate composite catalyst as described in claim 9, characterized in that, It is used as a catalyst in the preparation of hydrogen peroxide, with ultrasound and visible light as the reaction driving conditions.