Sludge synergistic curing agent based on microbial mineralization and nano-compounding and preparation method of sludge synergistic curing agent
By using a sludge synergistic solidifying agent combining microbial mineralization and nanocomposite materials, and leveraging the synergistic effect of components such as biochar-loaded nano-iron and attapulgite, the problem of insufficient stability and strength in sludge treatment in existing technologies has been solved, achieving highly efficient pollutant treatment, efficient dewatering and rapid solidification of sludge, and stabilization of heavy metals and organic matter.
Patent Information
- Application Number
- CN202511572349.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-10-30
- Publication Date
- 2025-11-28
- Estimated Expiration
- 2045-10-30
AI Technical Summary
Existing sludge solidification agents lack stability and strength when treating complex sludge, making it difficult to effectively stabilize heavy metals and organic matter simultaneously. They are also prone to cracking and cannot meet the needs of complex scenarios.
A sludge synergistic solidifying agent combining microbial mineralization and nanocomposite is used. Through the synergistic effect of components such as biochar loaded with nano iron and attapulgite, rapid dehydration, high-strength solidification and long-term stabilization of pollutants are achieved.
It achieves efficient dewatering and rapid solidification of sludge, efficient adsorption and stabilization of heavy metals and organic pollutants, and the solidified body meets the mechanical properties standards, has few structural defects, is economically reasonable, and meets engineering application and environmental protection requirements.
Smart Images

Figure CN121020937A_ABST
Abstract
Description
TECHNICAL FIELD
[0001] The present application relates to the field of solid waste treatment technology in environmental engineering, and particularly relates to a sludge synergistic solidifying agent based on microbial mineralization and nano-composite and a preparation method thereof. BACKGROUND
[0002] With the development of urbanization and industry, the discharge amount of sludge from municipal sewage treatment plants, dredging sludge from rivers and lakes, and industrial contaminated spoil is gradually increasing. If not properly treated, it will occupy land and pollute the environment through soil penetration and water diffusion, threatening the ecology and human health. At present, the industry commonly uses solidification and stabilization technology, that is, adding a solidifying agent to convert pollutants into stable, standard, and low secondary pollution risk solidified bodies, which are then landfilled or resourcefully utilized.
[0003] The existing solidification technology has the problems of long solidification period, low efficiency, and difficulty in emergency response. On the other hand, the stabilization effect is limited, and the solidified body may slowly release pollutants during long-term storage. In addition, the solidified body is prone to cracking due to water evaporation and temperature changes, forming pollution penetration channels. Furthermore, it is difficult to simultaneously stabilize both heavy metals and organic matter in complex sludge, and there is still a risk of exceeding the standard or release after treatment, which cannot meet the needs of complex scenarios.
[0004] In order to reduce costs, some solidification technologies introduce industrial waste residues such as steel slag and slag as auxiliary materials, which are widely available and low in price, can reduce the amount of high-priced inorganic cementing materials, and also meet the requirements of circular economy. In order to accelerate dewatering and shorten the period, some technologies use high molecular flocculants to allow colloidal particles and water to quickly aggregate and settle. At the same time, some technologies optimize the ratio of cement, lime, and other inorganic cementing materials to improve the strength and stability of the solidified body and reduce cracking.
[0005] However, free calcium in industrial waste residues can cause the solidified body to be alkaline, affecting the strength and destroying the acid-base balance of the soil. High molecular flocculants are easily biodegradable, which may destroy the stability of pollutants and lead to secondary release. Optimizing the ratio can only alleviate the problem, but cannot fundamentally solve it, and cannot break through the problem of simultaneous stabilization of heavy metals and organic matter in complex sludge. Therefore, it is an urgent need in the industry to develop a new composite solidifying agent that has efficient dewatering, rapid solidification, and multiple pollution control. SUMMARY
[0006] In order to solve the problems of insufficient stability and strength of the existing sludge solidifying agent, the present application aims to provide a sludge synergistic solidifying agent based on microbial mineralization and nano-composite and a preparation method thereof. Through the synergistic effect of the adsorption performance of biochar, the reduction and stabilization effect of nano-iron, and the cementation effect of the composite cementing system, rapid dewatering, high-strength solidification, and long-term stabilization of pollutants are achieved. The sludge synergistic solidifying agent is suitable for the harmless treatment and resource utilization of river dredging sludge, industrial sludge, and other high-water-content, high-organic-matter, and heavy-metal-polluted sludge.
[0007] To achieve the above object, the present application provides the following technical solutions: The present application provides a kind of sludge synergistic stabilizer based on microbial mineralization and nanocomposite, including 20%~30% fly ash, 15%~20% sulphoaluminate cement, 10%~15% modified phosphogypsum powder, 15%~20% biochar load nano iron, 5%~10% attapulgite, 6%~10% polyaspartic acid-co-acrylamide, 4%~5% sodium carboxymethyl cellulose, 3%~5% silica ash, 1%~3% magnesium carbonate and 1%~2% tartaric acid by mass percentage.
[0008] The fly ash includes 45%~50% SiO2, 25%~30% Al2O3, 4%~6% Fe2O3 and 15%~20% CaO by mass percentage, and the rest is impurities.
[0009] The sulphoaluminate cement includes 40%~45% calcium sulphoaluminate, 25%~30% dicalcium silicate, 10%~15% tetracalcium aluminoferrite by mass percentage, and the rest is impurities.
[0010] The preparation method of the modified phosphogypsum powder comprises: The citric acid solution and the phosphogypsum powder are mixed in a liquid-solid mass ratio of 1: (2~3), and the reaction is carried out at 60~70℃ until the pH is 6.5~7.5. The solid phase after the reaction is dried to obtain the modified phosphogypsum powder. The mass fraction of the citric acid solution is 3%~5%.
[0011] The preparation method of the biochar load nano iron comprises: The biochar is added into FeSO4 7H2O solution to obtain a first mixed solution. The concentration of the FeSO4 7H2O solution is 0.1~0.2 mol / L. The mass-volume ratio of the biochar and the FeSO4 7H2O solution is 1g: (10~15) mL. In an inert gas, NaBH4 solution is added to the first mixed solution in a molar ratio of Fe 2+ to BH4 - of 1: (2~3) to obtain biochar load nano iron. The concentration of the NaBH4 solution is 0.2~0.3 mol / L.
[0012] The preparation method of the attapulgite comprises: The attapulgite raw material is added into water in a solid-liquid mass ratio of 1: (5~8) and mixed uniformly. After standing, the upper layer of the suspension is taken. The reaction is carried out at 80-100 DEG C by adding hydrochloric acid solution to the upper layer suspension, and the solid phase after the reaction is washed, dried and ground to obtain the attapulgite.
[0013] The preparation method of the polyaspartic acid-co-acrylamide comprises the following steps: L-aspartic acid and acrylamide are dissolved in water to obtain a second mixed solution, and the molar ratio of L-aspartic acid to acrylamide is 1:(3-4); Ammonium persulfate is added to the second mixed solution, and the reaction is carried out at 60-70 DEG C in an inert atmosphere to obtain a reaction product, which is evaporated, precipitated and vacuum dried to obtain the polyaspartic acid-co-acrylamide, and the mass of the added ammonium persulfate is 2%-3% of the total mass of L-aspartic acid and acrylamide.
[0014] The application also provides a preparation method of the sludge synergistic stabilizer based on microbial mineralization and nanocomposites. Fly ash, sulphoaluminate cement and modified phosphogypsum powder are mixed to obtain a first stabilizer mixture; Biochar loaded nano-iron and attapulgite are added to the first stabilizer mixture to obtain a second stabilizer mixture; The polyaspartic acid-co-acrylamide is prepared into a polyaspartic acid-co-acrylamide solution, and the sodium carboxymethyl cellulose is prepared into a sodium carboxymethyl cellulose solution, and the polyaspartic acid-co-acrylamide solution and the sodium carboxymethyl cellulose solution are added to the second stabilizer mixture to obtain a third stabilizer mixture; Silica ash, magnesium carbonate and tartaric acid are added to the third stabilizer mixture and uniformly mixed to obtain the sludge stabilizer.
[0015] The mass fraction of the polyaspartic acid-co-acrylamide solution is 10%-15%.
[0016] The mass fraction of the sodium carboxymethyl cellulose solution is 5%-10%.
[0017] Compared with the prior art, the application has the beneficial effects that: The composite cementing phase composed of fly ash, sulphoaluminate cement and modified phosphogypsum powder generates cementitious products such as ettringite and C-S-H gel through hydration reaction to build a stable solidification body framework, and the cementitious products can effectively fill the pores inside the silt to realize silt dewatering and solidification. The component limitation of the composite cementing phase can ensure sufficient generation of hydration products, so that the unconfined compressive strength of the solidification body is stably up to ≥300kPa after 3 days; if the mass proportion of the composite cementing phase is too high, not only the cost will increase, but also the solidification body may crack due to excessive shrinkage during solidification. The functional adsorption phase composed of biochar loaded with nano-iron and attapulgite can efficiently remove pollutants in the silt; the biochar loaded with nano-iron has adsorption performance and reduction activity, which can not only adsorb heavy metal ions and organic pollutants in the silt, but also convert highly toxic heavy metals into low toxicity forms through the reduction of nano-iron, thereby greatly reducing the environmental risk of pollutants; the attapulgite can effectively improve the water absorption of the system, avoiding the problem of excessive water in the solidification body due to the excessive water absorption of the material, thereby causing strength reduction, and providing protection for the coordinated improvement of pollution stabilization and mechanical properties. The organic phase composed of poly-aspartic acid-co-acrylamide and sodium carboxymethyl cellulose tightly wraps the silt particles through the entanglement of the polymer chain and hydrogen bonding, thereby significantly enhancing the cohesiveness and toughness of the solidification body and effectively reducing the cracking risk caused by uneven structural stress during maintenance. Silica fume, magnesium carbonate and tartaric acid are used as functional regulators to fine-tune the hydration reaction rate, optimize the microstructure, and improve the early strength and late stability of the balanced solidification body. The silt synergistic solidification agent of the present application can realize efficient dewatering and solidification of the silt and improve the mechanical properties through synergistic effect and precise control of the amount of each component, and can also efficiently adsorb, reduce and stabilize heavy metals and organic pollutants, finally achieving the comprehensive effect of meeting the engineering application and environmental protection requirements, such as meeting the mechanical performance standard of the silt solidification body, long-term stability of pollutants, few structural defects and reasonable economic efficiency.
[0018] The preparation method of the silt synergistic solidification agent provided by the present application first uniformly disperses the composite cementing phase composed of fly ash, sulphoaluminate cement and modified phosphogypsum powder to ensure balanced strength during solidification of the cementing phase, then uniformly disperses the functional adsorption phase to avoid agglomeration, adds the organic phase through a solution to control the water content of the solidification agent system, and finally uniformly disperses the functional regulators such as silica fume, magnesium carbonate and tartaric acid to obtain a silt synergistic solidification agent with uniform composition and stable performance. BRIEF DESCRIPTION OF DRAWINGS
[0019] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings needed to be used in the embodiments will be briefly introduced as follows. It should be understood that the following drawings only show some of the embodiments of the present application, and therefore should not be considered as limiting the scope. For those skilled in the art, other related drawings can also be obtained without creative labor.
[0020] Figure 1 Micro-morphology of biochar loaded with nano-iron; Figure 2 ICP-MS (Inductively coupled plasma mass spectrometry) characterization of the absorption peak spectrum of the nano-iron loading amount in biochar loaded with nano-iron. DETAILED DESCRIPTION
[0021] In order to make the technical problems, technical solutions and beneficial effects of the present application more clearly understood, the following embodiments will be further described in detail. It should be understood that the specific embodiments described herein are only used to explain the present application, and are not used to limit the present application.
[0022] In the present application, the term "and / or" describes the association relationship of the associated objects, which means that there can be three kinds of relationships, for example, A and / or B, which can represent the following cases: A exists alone, A and B exist together, and B exists alone. Wherein A and B can be singular or plural. The character " / " generally represents an "or" relationship between the associated objects before and after it.
[0023] In the present application, "at least one" means one or more, and "a plurality of" means two or more. "At least one of the following" or similar expressions means any combination of these items, including any combination of single item or multiple items. For example, "at least one of a, b, or c", or "at least one of a, b, and c", can represent a, b, c, a-b (i.e. a and b), a-c, b-c, or a-b-c, wherein a, b, and c can be single or multiple.
[0024] It should be understood that in various embodiments of the present application, the size of the serial number of each process does not mean the order of execution, and part or all of the steps can be executed in parallel or in sequence, and the execution order of each process should be determined according to its function and inherent logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.
[0025] The terminology used in the description of the application herein is for the purpose of describing particular embodiments only and is not intended to be limiting of the application. As used in the description of the application and the appended claims, the singular forms "a", "an" and "the" are intended to include the plural forms as well, unless the context clearly indicates otherwise.
[0026] The weight of the related components mentioned in the specification of the embodiments of the application can not only refer to the specific content of each component, but also represent the proportional relationship between the weights of each component, therefore, as long as the content of the related components in the specification of the embodiments of the application is proportionally enlarged or reduced, it is within the scope disclosed in the specification of the embodiments of the application. Specifically, the mass mentioned in the specification of the embodiments of the application can be μg, mg, g, kg and other mass units commonly known in the chemical field.
[0027] Unless otherwise specified, the particle size of the particles in the application is determined by a laser particle size analyzer, the specific surface area is determined by the BET method (Brunauer, Emmett and Teller, gas adsorption method), the water content is determined by the drying method, the model of the jet mill in the embodiments is QLM-100, the model of the jaw crusher is PE-150x25, the model of the Raymond mill is 3R4119, the model of the tubular furnace is GSL-1600X, the model of the double-screw metering scale is LXC-50, and the metering accuracy is ±1%. The pipe diameter of the pneumatic conveying pipeline is DN100, the air pressure is 0.2MPa, the model of the double-shaft paddle mixer is WZ-200, the effective volume is 0.5m 3 , and the paddles are arranged in a staggered manner with "left-handed + right-handed".
[0028] The application provides a kind of sludge synergic stabilizer based on microbial mineralization and nanocomposite, including 20%~30% fly ash, 15%~20% sulphoaluminate cement, 10%~15% modified phosphogypsum powder, 15%~20% biochar loaded nano iron, 5%~10% attapulgite, 6%~10% polyaspartic acid-co-acrylamide, 4%~5% sodium carboxymethyl cellulose, 3%~5% silica fume, 1%~3% magnesium carbonate and 1%~2% tartaric acid by mass percentage.
[0029] The limitation of the use amount of each component of the composite cementing phase composed of fly ash, sulphoaluminate cement and modified phosphogypsum powder in the sludge synergic stabilizer provided by the application can ensure sufficient hydration products, and the 3-day unconfined compressive strength is ≥300kPa; the use amount ratio of the composite gel phase is too high, which can increase the cost and cause cracking due to excessive shrinkage. The biochar loaded nano iron and attapulgite form a functional adsorption phase, and the functional adsorption phase can adsorb Cr 6+ , Pb 2+Heavy metal ions and organic pollutants such as polycyclic aromatic hydrocarbons and phenols, nano-iron reduces highly toxic heavy metals, and realizes long-term stabilization of pollutants; the biochar loaded with nano-iron needs to reach 15% to 20% to ensure that the leaching rate of heavy metals is ≤0.1 mg / L; 5% to 10% of the attapulgite can avoid the decrease in strength caused by excessive water absorption; the organic phase composed of polyaspartic acid-co-acrylamide and sodium carboxymethyl cellulose can wrap the sludge particles through the entanglement of the polymer chain and the hydrogen bond, improve the cohesiveness and toughness of the solidified body, and reduce the cracking period, wherein, more than 10% of polyaspartic acid-co-acrylamide will increase the plasticity of the solidified body, and less than 6% will be insufficient in cohesiveness; 4% to 5% of sodium carboxymethyl cellulose can avoid the strength hysteresis caused by excessive water retention; silica fume, magnesium carbonate and tartaric acid are performance adjusters, which are used to fine-tune the hydration reaction rate, optimize the microstructure, and balance the early strength and late stability of the solidified body, wherein, more than 5% of silica fume will increase the water demand, more than 3% of magnesium carbonate will inhibit the strength growth, and more than 2% of tartaric acid will cause the final setting time to be too long, ensuring the long-term stabilization of heavy metals and organic pollutants.
[0030] In some embodiments, a method for preparing fly ash, comprising: The fly ash raw material is selected from the secondary fly ash of a thermal power plant, which meets the GB / T1596-2017 standard, and high-calcium fly ash generated by a circulating fluidized bed boiler is preferred, and the initial particle size is ≤150 μm.
[0031] The secondary fly ash of the thermal power plant is subjected to superfine treatment by an air flow mill to obtain fly ash, and the crushing pressure during the treatment process is 0.8 MPa, and the rotating speed of the grading wheel is 3000 r / min; the particle size distribution of the fly ash is D10=2 μm, D50=6 μm, and D90=12 μm, and the specific surface area is 450-550 m 2 / g; The fly ash includes 45% to 50% of SiO2, 25% to 30% of Al2O3, 4% to 6% of Fe2O3, 15% to 20% of CaO, and the rest is impurities, and the water demand ratio is ≤105%; the pozzolanic activity is sufficient to react with Ca(OH)2 to generate C-S-H gel.
[0032] The activity of the treated fly ash is detected: 50 g of fly ash is mixed with 200 mL of saturated Ca(OH)2 solution, and cured at 80℃ for 7 days, and the Ca 2+ concentration reduction value is ≥30 mg / L, which proves that the pozzolanic activity meets the standard.
[0033] In some embodiments, a method for preparing sulphoaluminate cement, comprising: The sulphoaluminate cement is a 42.5-grade fast-hardening sulphoaluminate cement, which meets the GB20472-2006 standard, has an initial setting time of 25-30 min, a final setting time of 90-120 min, and a 28d compressive strength of ≥42.5 MPa.
[0034] The sulphoaluminate cement includes 40%-45% calcium sulphoaluminate, 25%-30% dicalcium silicate, 10%-15% tetracalcium aluminoferrite, and the rest impurities in terms of mass percentage; these components can generate ettringite with needle-shaped crystals during hydration, thereby significantly improving early strength; the mass fraction of free CaO is ≤1.0%, which avoids expansion and cracking in the later hydration stage; and the mass fraction of SO3 is 8%-10%, which ensures the amount of ettringite generated.
[0035] In some embodiments, the method for preparing modified phosphogypsum powder includes: The phosphogypsum raw material is phosphogypsum from phosphorus chemical waste residue, has an initial water content of ≤15%, and mainly includes dihydrate calcium sulfate (CaSO4 2H2O) with a mass fraction of ≥90%. The phosphogypsum from phosphorus chemical waste residue is first crushed to a particle size of ≤5 mm by a jaw crusher, and then quartz, feldspar, and other impurities are removed through a 200-mesh vibrating screen to obtain phosphogypsum powder. The pH of the unmodified phosphogypsum powder is 10-12.
[0036] A citric acid solution with a mass fraction of 3%-5% is prepared using analytical pure citric acid.
[0037] The citric acid solution and the phosphogypsum powder are mixed at a liquid-solid mass ratio of 1:(2-3), placed in a constant-temperature water bath at 60-70°C, mechanically stirred and soaked for 12 h at a stirring rate of 150 r / min. The pH value is detected every 2 h during the period until the pH stabilizes at 6.5-7.5. Vacuum filtration is performed at a vacuum degree of -0.08 MPa. After filtration, air-drying is performed at 80°C until the water content is below 5% to obtain modified phosphogypsum powder. The modified phosphogypsum powder is crushed to 300 mesh by a Raymond mill for use. The particle size of the modified phosphogypsum powder is ≤50 μm, ensuring dispersibility.
[0038] It should be noted that the free CaO in the phosphogypsum powder is neutralized by citric acid to reduce alkalinity, and part of the impurities such as phosphorus and fluorine are dissolved to avoid inhibiting the hydration reaction.
[0039] In some embodiments, the method for preparing biochar loaded with nano-iron includes: The biomass raw material is ground until the particle size is 2-3 cm, washed with deionized water for 3 times, dried at 60°C until the water content is below 10%, and then ground until the particle size is 1-2 mm. The biomass raw material includes corn cobs, corn stalks, wheat stalks, branches, wood chips, and the like.
[0040] The dried biomass raw material is placed in a tube furnace, nitrogen is introduced to drive oxygen for 30 min, the flow rate of nitrogen is 500 mL / min, and the temperature is raised to 500℃ at a rate of 10℃ / min, and the carbonization treatment is carried out for 3 h, and then the carbonization treatment is naturally cooled to room temperature, and then sieved through a 100 mesh sieve to obtain biochar, and the particle size of the biochar is less than 150 μm.
[0041] The specific surface area of the biochar is 350~400 m 2 / g; the total pore volume of the biochar is 0.25~0.3 cm 3 / g, and the pore size distribution is mainly micropores with a pore size of 2~5 nm, which is beneficial to the adsorption of small molecule organic matter, and the pH value of the biochar is 7.0~7.5, which avoids the influence of strong alkalinity on the activity of nano-iron.
[0042] FeSO4 7H2O is dissolved in deionized water to prepare a FeSO4 7H2O solution with a concentration of 0.1~0.2 mol / L.
[0043] The biochar is added to the FeSO4 7H2O solution and magnetically stirred at a speed of 300 r / min for 30 min to obtain a first mixture, and the Fe 2+ is fully adsorbed on the surface of the biochar; the mass-volume ratio of the biochar to the FeSO4 7H2O solution is 1 g: (10~15) mL.
[0044] In an inert gas, the molar ratio of Fe 2+ to BH4 - is 1: (2~3), and NaBH4 solution is added dropwise to the first mixture for reaction, wherein the concentration of the NaBH4 solution is 0.2~0.3 mol / L, the dropwise addition rate of NaBH4 is 1 mL / min, and the flow rate of the inert gas is 200 mL / min; after 1 h of reaction, the reaction solution is vacuum filtered to obtain black nano-iron particles, the black nano-iron particles are washed with deionized water for 3 times to remove residual salt, and then washed with anhydrous ethanol for 1 time to reduce agglomeration, and then vacuum dried at 60℃ and a vacuum degree of -0.09 MPa for 8 h to obtain black powder, which is the biochar-loaded nano-iron.
[0045] The prepared biochar-loaded nano-iron is tested for related performance, and the particle size of the biochar-loaded nano-iron is characterized by TEM (Transmission Electron Microscope), and the biochar-loaded nano-iron is dispersed in anhydrous acetone before testing to ensure uniform distribution during observation, facilitating clear observation of the microstructure. Figure 1As shown in the figure, the darker areas represent nano-iron. The smaller the nano-iron particles, the better the experimental results are achieved. The nano-iron in the biochar-supported platform is stably granular, and a small amount of even higher-quality nano-iron (reaching 30 nm) exists. Statistically, approximately 86% of the regions have nano-iron particles reaching 50-100 nm.
[0046] The loading of nano-iron was determined by ICP-MS, such as... Figure 2 As shown, four groups of solutions were set up: a blank group (Control), a standard solution group (Standard), an Agilent 7700 group, and a Thermo Fisher iCAPTQ group. The prepared solutions were introduced into an ICP-MS and monitored in real time. 56 The Fe signal ensures that the iron signal of each separated component can be accurately captured. An increase in the Fe signal in ICP-MS indicates a high content of nano-iron particles. Based on the absorption peaks at 11 min and 15 min, and in accordance with the instructions for use of the standard solutions, the loading of nano-iron in the test samples was statistically determined to be 8%–10%.
[0047] TEM characterization revealed that the iron nanoparticles supported on biochar had a particle size of 50–100 nm, and ICP-MS analysis showed that the iron loading was 8–10%. The iron nanoparticles were uniformly distributed on the biochar surface without significant agglomeration. Biochar-supported iron nanoparticles exhibit a dual "reduction-adsorption" mechanism; biochar possesses a high porosity and oxygen-containing functional groups, and zero-valent iron exhibits high surface activity and reducing power, enabling biochar-supported iron nanoparticles to effectively adsorb and immobilize heavy metal ions in sludge; Fe binds Cr... 6+ Reduced to Cr 3+ Carboxyl groups on the surface of biochar and Cr 3+ Forming stable chelates, Cr 3+ The leaching concentration is controlled below 0.02 mg / L.
[0048] In some embodiments, the method for preparing attapulgite includes: The raw material for attapulgite clay is selected from attapulgite clay produced in Linze, Gansu Province, with a purity of over 85% and a mass fraction of attapulgite minerals of over 80%. The raw material for attapulgite clay is ground until the particle size is below 1mm.
[0049] Add the ground attapulgite raw material to deionized water at a solid-liquid mass ratio of 1:(5~8), stir at 500 r / min for 30 min, let stand for 2 h after stirring evenly, and take the upper suspension; purify the attapulgite raw material to remove impurities such as quartz sand.
[0050] The upper layer suspension is added with 3-5% hydrochloric acid solution by mass fraction, and the reaction is carried out at 80-100°C for 2h under stirring to remove carbonate impurities. After the reaction, the reaction solution is filtered, the solid phase after filtration is washed with deionized water until neutral, and is dried at 100-120°C, and then is ultra-finely pulverized to obtain the attapulgite, which has a particle size D50 of 2-3μm, a specific surface area of more than 200m 2 / g, a Cation Exchange Capacity (CEC) of more than 20meq / 100g as determined by the ammonium acetate method.
[0051] It should be noted that the attapulgite has a layered structure, the layered structure adsorbs heavy metals through ion exchange, and the fibrous crystals are inserted into the solidified body to enhance the crack resistance. The adsorption capacity of the interlayer pores of the attapulgite for benzene series is more than 30mg / g, the aromatic structure of the biochar adsorbs polycyclic aromatic hydrocarbons through π-π interaction, and the removal rate of organic pollutants is more than 90% under the combined action, and the desorption rate is less than 5% after oscillation for 60d.
[0052] In some embodiments, the preparation method of poly-aspartic acid-co-acrylamide comprises: L-aspartic acid and acrylamide are dissolved in water to obtain a second mixed solution, the mass fraction of the second mixed solution is 30%, and the molar ratio of L-aspartic acid to acrylamide is 1:(3-4); Ammonium persulfate is added to the second mixed solution and mixed uniformly, and a polymerization reaction is initiated in an inert gas at a constant temperature water bath of 60-70°C for 4h to obtain a reaction product, which is a light yellow viscous liquid; the reaction product is concentrated to a solid content of ≥30% by rotary evaporation at 60°C and a vacuum degree of-0.08MPa, and then purified by ethanol precipitation, and dried at 80-100°C and a vacuum degree of-0.08MPa, and then ground through an 80-mesh sieve to obtain poly-aspartic acid-co-acrylamide; the mass of ammonium persulfate added is 2-3% of the total mass of L-aspartic acid and acrylamide.
[0053] The prepared poly-aspartic acid-co-acrylamide has a number average molecular weight of 5000-8000 as determined by Gel Permeation Chromatography (GPC), and a chelating value for Ca 2+ of more than 100mg / g as determined by Ethylene Diamine Tetraacetic Acid (EDTA) titration method; and a viscosity of a 2% poly-aspartic acid-co-acrylamide aqueous solution at 25°C of more than 300mPa s as determined by a rotational viscometer.
[0054] Polyaspartic acid-co-acrylamide is added into deionized water, and stirred at a speed of 500 r / min until completely dissolved to obtain a polyaspartic acid-co-acrylamide solution for standby, and the mass fraction of the polyaspartic acid-co-acrylamide solution is 10%-15%.
[0055] It should be noted that the carboxyl group of the aspartic acid unit chelates metal ions, and the amide group of the acrylamide unit forms a hydrogen bond with soil particles to construct a three-dimensional network structure.
[0056] In some embodiments, the degree of substitution of carboxymethyl cellulose sodium (CMC-Na) is 0.8-1.0, the degree of substitution is 80-100 carboxymethyl groups introduced per 100 glucose units, and the purity is above 99%.
[0057] The viscosity of a 2% carboxymethyl cellulose sodium aqueous solution is 500-800 mPa s at 25°C and a speed of 60 r / min, the pH value is 6.5-7.5, and the water-insoluble substance is below 0.5%, so as to ensure that the CMC-Na is uniformly dispersed in the silt.
[0058] The CMC-Na is removed from the agglomerates through an 80-mesh sieve, and the CMC-Na is added into deionized water at 60°C and stirred at a speed of 500 r / min until completely dissolved to obtain a carboxymethyl cellulose sodium solution for standby, and the mass fraction of the carboxymethyl cellulose sodium solution is 5%-10%.
[0059] It should be noted that the carboxymethyl cellulose sodium can improve the workability of the solidifying agent and the silt, reduce dust in the stirring process, and keep water during the curing period to prevent surface cracking.
[0060] In some embodiments, the silica ash is a by-product of ferrosilicon smelting in a ferroalloy plant, the mass fraction of SiO2 in the silica ash is ≥90%, the specific surface area is 15000-20000 m 2 / g, the particle size is 0.1-0.5 μm observed by electron microscopy, and the density is 2.2-2.3 g / cm 3 .
[0061] It should be noted that the silica ash is a superfine particle, which can fill the pores of the C-S-H gel system to improve the compactness, and react with Ca(OH)2 to generate additional C-S-H gel to enhance the strength of the interface transition zone.
[0062] In some embodiments, the magnesium carbonate is light magnesium carbonate, and the purity of the light magnesium carbonate is above 95%, the particle size is below 10 μm, the whiteness is above 90%, and the moisture is below 2%.
[0063] It should be noted that the Mg(OH)2 generated by the slow hydration reaction of magnesium carbonate reduces the alkalinity of the liquid phase, delays the generation rate of ettringite, and avoids cracks caused by concentrated early heat release.
[0064] In some embodiments, the tartaric acid is analytical pure tartaric acid, wherein the content of C4H6O6 is above 99.5%, and the particle size is 50-100 μm, and it is easily soluble in water.
[0065] It should be noted that tartaric acid has a retarding effect, which inhibits the nucleation of hydrated calcium silicate by adsorbing on the surface of cement particles, controls the initial setting time of the silt synergistic solidification agent to 4-6 h, meets the construction operation window, and the final setting time is below 12 h.
[0066] The preparation method of the above-mentioned silt synergistic solidification agent based on microbial mineralization and nanocomposites comprises: S1, mixing fly ash, sulphoaluminate cement and modified phosphogypsum powder to obtain a first solidification agent mixture; S2, adding biochar loaded nano-iron and attapulgite to the first solidification agent mixture to obtain a second solidification agent mixture; S3, adding polyaspartic acid-co-acrylamide to water to obtain a polyaspartic acid-co-acrylamide solution, adding sodium carboxymethyl cellulose to water to obtain a sodium carboxymethyl cellulose solution, and mixing the polyaspartic acid-co-acrylamide solution and the sodium carboxymethyl cellulose solution in the second solidification agent mixture to obtain a third solidification agent mixture; S4, mixing silica fume, magnesium carbonate and tartaric acid in the third solidification agent mixture to obtain a silt synergistic solidification agent.
[0067] In some embodiments, the silt synergistic solidification agent is prepared by a double-shaft mixer; in S1, the mixture is stirred at a speed of 200 r / min for 8 min, and the composition deviation is ≤2% at 3 sampling points, ensuring uniformity of the powder; in S2, the mixture is stirred at a speed of 300 r / min for 5 min to disperse the nanoparticles by shear force; in S3, the mixture is stirred at a speed of 250 r / min for 10 min, and the polyaspartic acid-co-acrylamide solution and the sodium carboxymethyl cellulose solution are slowly added during the stirring process; the water content of the composite system is controlled to be ≤10%; in S4, the mixture is stirred at a speed of 200 r / min for 5 min, and the particle size of the silt synergistic solidification agent is ≤1 mm detected by sieving method. During the mixing process, the speed is dynamically adjusted according to the material state to prevent dust, and the final mixing uniformity is ≥95% verified by fluorescence labeling method.
[0068] In the preparation process of the silt synergistic solidification agent, the temperature is controlled to be 20-30℃, and when the environmental temperature is too low, the jacket is turned on for heating, and at the same time, the organic phase is prevented from being degraded due to high temperature.
[0069] The prepared sludge synergistic curing agent is stored in double-layer polyethylene bags, the inner layer of the double-layer polyethylene bag is vacuum packaged, the outer layer is moisture-proof, each bag is 25 kg, is stored in a dry environment at ≤30 DEG C, the shelf life is 6 months, regular sampling inspection is carried out, and the guarantee active decline rate is ≤5%.
[0070] The quality detection index of the sludge synergistic curing agent needs to meet the following requirements: (1) Component uniformity, 3 samples are randomly taken, the mass fraction of SiO2 and Al2O3 is determined, and the relative deviation is ≤3%.
[0071] (2) Particle size distribution, wet screening is adopted, and the residue on a 300 mesh sieve is less than 5%.
[0072] (3) Activity index, the 28d compressive strength ratio is ≥95% (GB / T12957-2005 method) by mixing with reference cement at a mass ratio of 1:3.
[0073] (4) Heavy metal adsorption performance, the static adsorption amount of Cr 6+ is more than 20 mg / g, and the initial concentration of the test object Cr 6+ is 100 mg / L.
[0074] Through the above fine process control, the sludge synergistic curing agent realizes the synergistic effect of "gel skeleton construction-pollutant adsorption and solidification-toughness network reinforcement" in sludge treatment, the 3d unconfined compressive strength is ≥300 kPa, and the heavy metal leaching concentration is ≤0.05 mg / L (GB 5085.3-2007 standard).
[0075] The application also provides an application method of the sludge synergistic curing agent, comprising: The sludge is treated by adopting a two-stage screening process, a grid is adopted in the first stage, the aperture of the grid is 10 mm, and large impurities such as branches and plastics are removed; a vibrating screen is adopted in the second stage, the vibrating screen is 20 mesh, the amplitude is 3-5 mm, the frequency is 50 Hz, and the sand and stone particles with a particle size greater than 0.85 mm are separated, so that the particle size uniformity of the sludge entering the subsequent process is ensured; the screened sludge is sent into a horizontal homogenizing tank for conditioning and homogenization, the effective volume of the horizontal homogenizing tank is 10 m 3, the double-layer stirring paddle is arranged in the pool, the upper paddle diameter is 1.2 m, the lower paddle diameter is 0.8 m, the rotating speed is 60 r / min, the stirring is continuously carried out for 30 min, the infrared moisture meter is used for on-line monitoring, the sludge moisture content is controlled within ± 2%; if the initial moisture content of the sludge is greater than 85%, the pretreated dried sludge is added to the homogenizing pool through the screw conveyor, the moisture content of the dried sludge is less than or equal to 30%, the dried sludge is added until the moisture content is reduced to 75% to 80%, and the sludge is in a stirrable state; if the moisture content is less than 70%, deionized water is added to adjust, and the sludge is ensured to be in a flowable state, and the consistency index is 1.2 to 1.5. The sludge is pretreated, the initial moisture content of the sludge is reduced, the large impurities are removed, and conditions for uniform mixing of the solidifying agent are created.
[0076] The sludge is accurately proportioned and mixed with the solidifying agent through a double-screw metering scale, wherein the main material screw conveys the sludge and the solidifying agent, the rotating speed is 50 to 100 r / min, the rotating speed is adjusted according to actual needs; the auxiliary material screw conveys the sludge, the rotating speed is automatically matched according to the sludge and the solidifying agent addition amount, the two are linked and controlled through a PLC system, and the mass ratio of the sludge and the solidifying agent is 1: (5 to 7), so that the uniformity of the solidification reaction is ensured.
[0077] The sludge and the solidifying agent are sent into a double-shaft paddle mixer through a pneumatic conveying pipeline, a Venturi nozzle is arranged at the end of the pipeline, the sludge and the solidifying agent are dispersed into mist with a particle size of less than 0.5 mm, are uniformly sprayed into the sludge flow, the flow speed of the sludge is 1.5 to 2 m / s, and local agglomeration is avoided. The sludge and the solidifying agent are mixed in the double-shaft paddle mixer at a rotating speed of 150 r / min for 15 min, three-point sampling is detected through sampling, and the mixing uniformity is ensured to be more than 90%.
[0078] The mixed material is uniformly laid on a construction area, a film is covered on the surface, the air permeability of the film is 500 g / m 2 more than 24 h, and primary curing is carried out for 24 to 48 h in an environment with a humidity of 80% to 90%; the primary curing is mainly to promote the rapid generation of ettringite.
[0079] The film is removed, and natural curing is carried out for 48 h to 7 d in a natural environment, an automatic spraying system is used in the natural curing process, water is sprayed once every 6 h, the spraying amount is 1% of the mass of the solidified body, the surface moisture content is maintained to be more than 80%, and meanwhile, the environmental temperature is controlled to be 15 to 25 DEG C through a sunshade, so that the surface is prevented from being directly irradiated by sunlight to cause surface shrinkage.
[0080] Through gradient humidity control, the hydration reaction is promoted to proceed in an orderly manner, and the solidified body is prevented from cracking. When the unconfined compressive strength of the solidified body is more than 300 kPa and the moisture content is less than 55% after 3 days, the curing is completed.
[0081] The sludge synergic curing agent can inhibit the generation of micro cracks during maintenance period by adding 0.5% of polypropylene fibers, the length of the polypropylene fibers is 12 mm, the tensile strength is above 600 MPa, the mass loss rate of the polypropylene fibers is below 3% and the strength retention rate is above 85% after 25 freezing and thawing cycle tests of freezing for 4 h at-20 DEG C and thawing for 4 h at 20 DEG C.
[0082] In the following examples, each material used can be obtained through an ordinary channel unless otherwise specified; the test method used is a conventional method in the art.
[0083] Example 1 Preparation of the substrate: The fly ash of the second grade of the thermal power plant is subjected to superfine treatment by using an air flow mill, the crushing pressure is 0.8 MPa during the treatment process, and the rotating speed of the grading wheel is 3000 r / min; the particle size distribution of the fly ash is as follows: D10=2.1 μm, D50=5.8 μm, D90=11.7 μm, and the specific surface area is 486 m 2 / g; the fly ash comprises 45% of SiO2, 28.6% of Al2O3, 6% of Fe2O3, 16.5% of CaO, and the rest is impurities in terms of mass percentage.
[0084] The sulphoaluminate cement comprises 40% of calcium sulphoaluminate, 25.7% of dicalcium silicate, 12.6% of tetracalcium aluminoferrite, and the rest is impurities in terms of mass percentage.
[0085] The citric acid solution and the phosphogypsum powder are mixed according to the liquid-solid mass ratio of 1:3, and are placed in a constant temperature water bath at 60 DEG C, and are subjected to mechanical stirring and soaking for 12 h, the stirring speed is 150 r / min, the pH value is detected every 2 h during the period, until the pH value is stabilized at 6.8; vacuum filtration is carried out under the vacuum degree of-0.08 MPa, and after the filtration, air drying is carried out at 80 DEG C until the water content is 4.7%, and the modified phosphogypsum powder is obtained; the modified phosphogypsum powder is crushed to 300 meshes by using a Raymond mill for use, and the mass fraction of the citric acid solution is 3%.
[0086] The biochar is added into a FeSO4 2+ 7H2O solution, and is subjected to magnetic stirring at the rotating speed of 300 r / min for 30 min to obtain a first mixed solution; under nitrogen, NaBH4 solution is added dropwise into the first mixed solution according to the molar ratio of Fe - and BH4 3 is 1:2 to carry out a reaction, the reaction liquid is vacuum filtered after the reaction for 1 h to obtain black nano iron particles, the black nano iron particles are washed with deionized water for 3 times, and are washed with anhydrous ethanol for 1 time, and are vacuum dried at 60 DEG C under the vacuum degree of-0.09 MPa for 8 h to obtain a black powder, which is the biochar loaded nano iron, wherein, the biochar and FeSO4 7H2O solution is 1g:10mL, the concentration of FeSO4 The concentration of 7H2O solution is 0.1mol / L; the concentration of NaBH4 solution is 0.2mol / L; through detection, the particle size of nano-iron in the biochar loaded nano-iron is 72nm, and the loading amount of nano-iron is 8.6%. According to the solid-liquid mass ratio of 1:5, the ground attapulgite raw material is added into deionized water, stirred at a speed of 500r / min for 30min, uniformly stirred and then placed for 2h, and the upper suspension is taken; 5% hydrochloric acid solution is added into the upper suspension, stirred at 80℃ for 2h for reaction, and after reaction, the reaction liquid is filtered, the solid phase after filtration is washed to neutral with deionized water, dried at 100℃, and then ultra-finely pulverized to obtain attapulgite; the CEC of the attapulgite after purification is 22.3meq / 100g.
[0087] L-aspartic acid and acrylamide are dissolved in water to obtain a second mixed solution, and the molar ratio of L-aspartic acid to acrylamide is 1:3; ammonium persulfate is added into the second mixed solution and uniformly mixed, and a polymerization reaction is initiated in a nitrogen atmosphere at a constant temperature water bath of 60℃ for 4h to obtain a reaction product; the reaction product is concentrated to a solid content of 30% by rotary evaporation at 60℃ and a vacuum degree of-0.08MPa, purified by ethanol precipitation, dried at 80℃ and a vacuum degree of-0.08MPa, and then ground through an 80-mesh sieve to obtain polyaspartic acid-co-acrylamide; the mass of ammonium persulfate added is 3% of the total mass of L-aspartic acid and acrylamide.
[0088] The silica ash is selected from a by-product of ferrosilicon smelting in a ferroalloy plant, the SiO2 content is 90%, the particle size is 0.1-0.5μm, and the density is 2.2g / cm 3 .
[0089] The magnesium carbonate is selected from light magnesium carbonate; and the tartaric acid is selected from analytical pure tartaric acid.
[0090] The sludge synergistic solidification agent is prepared based on the above-mentioned substrate, which comprises: In mass percentage, 26.8% of fly ash, 15% of sulphoaluminate cement, and 10% of modified phosphogypsum powder are mixed to obtain a first solidification agent mixture.
[0091] 20% of biochar loaded nano-iron and 6.3% of attapulgite are added into the first solidification agent mixture to obtain a second solidification agent mixture.
[0092] 10% of polyaspartic acid-co-acrylamide was added into water to prepare a polyaspartic acid-co-acrylamide solution with a mass fraction of 15%, and 4% of sodium carboxymethyl cellulose was added into water to prepare a sodium carboxymethyl cellulose solution with a mass fraction of 5%, and the polyaspartic acid-co-acrylamide solution and the sodium carboxymethyl cellulose solution were added into the second curing agent mixture and uniformly mixed to obtain a third curing agent mixture. 4.2% of silica fume, 2.7% of magnesium carbonate and 1% of tartaric acid were added into the third curing agent mixture and uniformly mixed to obtain the silt cooperative curing agent.
[0093] The silt cooperative curing agent prepared in this example was mixed with silt, the initial moisture content of the silt was 82.5%, dry silt was added until the moisture content was reduced to 77.3%, and the mass ratio of the silt cooperative curing agent to the silt was 1:5.8. After mixing, primary curing was performed in an environment with a humidity of 86% for 48 h, followed by natural curing for 7 d; the cured body was tested, and the 3-day unconfined compressive strength was 326 kPa, the Cr 6+ The leaching concentration was 0.042 mg / L, and the removal rate of benzene series was 91.7%.
[0094] Example 2 Preparation of the substrate: The secondary fly ash of a thermal power plant was superfined by a jet mill to obtain fly ash, and the crushing pressure was 0.8 MPa and the rotational speed of the classification wheel was 3000 r / min during the superfine treatment process; the particle size distribution of the fly ash was D10=1.9 μm, D50=6.2 μm and D90=12.3 μm, and the specific surface area was 462 m 2 / g; in terms of mass percentage, the fly ash comprised 50% of SiO2, 26.5% of Al2O3, 4.2% of Fe2O3, 15% of CaO, and the rest was impurities.
[0095] In terms of mass percentage, the sulphoaluminate cement comprised 42.5% of calcium sulphoaluminate, 25% of dicalcium silicate, 10% of tetracalcium aluminoferrite, and the rest was impurities.
[0096] The citric acid solution and the phosphogypsum powder were mixed in a liquid-solid mass ratio of 1:2.5, placed in a constant-temperature water bath at 65 ℃, mechanically stirred and soaked for 12 h, the stirring rate was 150 r / min, and the pH value was detected every 2 h during the period until the pH value was stabilized at 7.5; vacuum filtration was performed under a vacuum degree of -0.08 MPa, and after the filtration, air drying was performed at 80 ℃ until the moisture content was 4.3% to obtain modified phosphogypsum powder; the modified phosphogypsum powder was crushed to 300 mesh by a Raymond mill for use, and the mass fraction of the citric acid solution was 5%.
[0097] The biochar was added into FeSO4 7H2O solution at a rotation speed of 300 r / min for 30 min to obtain a first mixed solution; under nitrogen, NaBH4 solution was added dropwise into the first mixed solution according to a molar ratio of Fe 2+ and BH4 - of 1:3 to react, and the reaction liquid was vacuum filtered after 1 h to obtain black nano-iron particles; the black nano-iron particles were washed with deionized water for 3 times and then washed with anhydrous ethanol for 1 time, and then vacuum dried at 60℃ under a vacuum degree of-0.09 MPa for 8 h to obtain black powder, which was biochar loaded nano-iron, wherein the mass-volume ratio of FeSO4 7H2O solution was 1 g:12 mL, and the concentration of the FeSO4 7H2O solution was 0.2 mol / L; the concentration of the NaBH4 solution was 0.2 mol / L; through detection, the particle size of the nano-iron in the biochar loaded nano-iron was 65 nm, and the loading amount of the nano-iron was 9.3%. The ground attapulgite raw material was added into deionized water according to a solid-liquid mass ratio of 1:8, stirred at a rotation speed of 500 r / min for 30 min, and then uniformly stirred and statically placed for 2 h to obtain upper suspension; 5% hydrochloric acid solution was added into the upper suspension to react at 100℃ for 2 h, and then the reaction liquid was filtered; the solid phase after filtration was washed with deionized water until neutral, dried at 100℃, and then ultra-finely pulverized to obtain attapulgite; the CEC of the attapulgite after purification was 21.7 meq / 100 g.
[0098] L-aspartic acid and acrylamide were dissolved in water to obtain a second mixed solution, and the molar ratio of L-aspartic acid and acrylamide was 1:3.5; ammonium persulfate was added into the second mixed solution to mix uniformly, and a polymerization reaction was initiated in a nitrogen environment in a constant temperature water bath at 60℃ for 4 h to obtain a reaction product; the reaction product was concentrated to a solid content of 30% by rotary evaporation in an environment at 65℃ under a vacuum degree of-0.08 MPa, and then purified by ethanol precipitation and dried in an environment at 80℃ under a vacuum degree of-0.08 MPa before being ground through an 80-mesh sieve to obtain polyaspartic acid-co-acrylamide; the mass of the added ammonium persulfate was 2% of the total mass of L-aspartic acid and acrylamide.
[0099] The silica ash was a by-product of ferrosilicon smelting in a ferroalloy plant, the SiO2 content was 90%, the particle size was 0.1-0.5 μm, and the density was 2.2 g / cm 3 .
[0100] The magnesium carbonate was light magnesium carbonate, and the tartaric acid was analytical pure tartaric acid.
[0101] The sludge synergistic solidification agent was prepared based on the above substrate, including: 20% of fly ash, 17% of sulphoaluminate cement, 15% of modified phosphogypsum powder are mixed to obtain a first solidification agent mixture.
[0102] 18.2% of biochar loaded nano-iron and 10% of attapulgite are added to the first solidification agent mixture to obtain a second solidification agent mixture.
[0103] 6% of polyaspartic acid-co-acrylamide is added to water to prepare a polyaspartic acid-co-acrylamide solution with a mass fraction of 10%, and 5% of sodium carboxymethyl cellulose is added to water to prepare a sodium carboxymethyl cellulose solution with a mass fraction of 10%. The polyaspartic acid-co-acrylamide solution and the sodium carboxymethyl cellulose solution are added to the second solidification agent mixture and mixed uniformly to obtain a third solidification agent mixture. 3.8% of silica fume, 3% of magnesium carbonate and 2% of tartaric acid are added to the third solidification agent mixture and mixed uniformly to obtain a silt cooperative solidification agent.
[0104] The silt cooperative solidification agent prepared in this example is mixed with silt, the initial moisture content of the silt is 84.2%, dry silt is added until the moisture content is reduced to 78.5%, and the mass ratio of the silt cooperative solidification agent to the silt is 1:6.3. After mixing, the primary curing is carried out in an environment with a humidity of 83% for 48h, and then natural curing is carried out for 7d; the cured body is tested, the 3-day unconfined compressive strength is 312kPa, the Cr 6+ The leaching concentration is 0.038mg / L, and the removal rate of polycyclic aromatic hydrocarbons is 92.3%.
[0105] Example 3 Preparation of substrate: Secondary fly ash from a thermal power plant is superfined by air flow grinding to obtain fly ash, the grinding pressure during the treatment process is 0.8MPa, and the rotational speed of the classification wheel is 3000r / min; the particle size distribution of the fly ash is D10=2.2μm, D50=5.9μm, D90=11.5μm, and the specific surface area is 512m 2 / g; the fly ash includes 46.2% of SiO2, 30% of Al2O3, 4% of Fe2O3, 17.5% of CaO, and the rest is impurities.
[0106] The sulphoaluminate cement includes 44.6% of calcium sulphoaluminate, 30% of dicalcium silicate, 13.8% of tetracalcium aluminoferrite, and the rest is impurities.
[0107] The citric acid solution and the phosphogypsum powder are mixed according to a liquid-solid mass ratio of 1:3, and are placed in a constant-temperature water bath at 70 DEG C, and are mechanically stirred and soaked for 12 hours, the stirring rate is 150 r / min, and during the period, the pH value is detected every 2 hours until the pH value is stabilized at 6.5; vacuum filtration is carried out under a vacuum degree of -0.08 MPa, and after the filtration, air drying is carried out at 80 DEG C until the water content is 5.1%, and the modified phosphogypsum powder is obtained; the modified phosphogypsum powder is crushed to 300 meshes by using a Raymond mill for later use, and the mass fraction of the citric acid solution is 4%.
[0108] The biochar is added into a FeSO4 7H2O solution, and is magnetically stirred at a rotating speed of 300 r / min for 30 min to obtain a first mixed solution; under nitrogen, NaBH4 solution is added dropwise into the first mixed solution according to a molar ratio of Fe 2+ and BH4 - of 1:2.5 to carry out a reaction, and after the reaction for 1 hour, the reaction liquid is vacuum filtered to obtain black nano-iron particles, the black nano-iron particles are washed with deionized water for 3 times, and are washed with anhydrous ethanol for 1 time, and are vacuum dried at 60 DEG C under a vacuum degree of -0.09 MPa for 8 hours to obtain a black powder, which is the biochar-loaded nano-iron, wherein, the mass-volume ratio of the biochar and the FeSO4 7H2O solution is 1g:15mL, and the concentration of the FeSO4 7H2O solution is 0.15 mol / L; the concentration of the NaBH4 solution is 0.3 mol / L; through detection, the particle size of the nano-iron in the biochar-loaded nano-iron is 83 nm, and the loading amount of the nano-iron is 8.9%. The ground attapulgite raw material is added into deionized water according to a solid-liquid mass ratio of 1:7, and is stirred at a rotating speed of 500 r / min for 30 min, and after being uniformly stirred, is placed for 2 hours, and the upper layer of the suspension is taken; a hydrochloric acid solution with a mass fraction of 3% is added into the upper layer of the suspension, and is stirred at 90 DEG C for 2 hours to carry out a reaction, and after the reaction, the reaction liquid is filtered, the solid phase after the filtration is washed with deionized water until neutral, and is dried at 100 DEG C, and is then ultra-finely crushed to obtain attapulgite; the CEC of the attapulgite after the purification is 23.1 meq / 100g.
[0109] L-aspartic acid and acrylamide were dissolved in water to obtain a second mixture, the molar ratio of L-aspartic acid and acrylamide being 1:4; ammonium persulfate was added into the second mixture and mixed uniformly, and a polymerization reaction was initiated in a nitrogen atmosphere in a constant temperature water bath at 60°C for 4h to obtain a reaction product; the reaction product was concentrated to a solid content of 30% by rotary evaporation in a vacuum environment at 60°C and a vacuum degree of-0.08MPa, and then purified by ethanol precipitation; after drying at 80°C and a vacuum degree of-0.08MPa, the product was ground through an 80-mesh sieve to obtain polyaspartic acid-co-acrylamide; the mass of ammonium persulfate was 2.2% of the total mass of L-aspartic acid and acrylamide.
[0110] Silica ash was selected from a by-product of ferrosilicon smelting in a ferroalloy plant, the SiO2 content was 90%, the particle size was 0.1-0.5μm, and the density was 2.2g / cm 3 .
[0111] Magnesium carbonate was selected from light magnesium carbonate; and tartaric acid was selected from analytical pure tartaric acid.
[0112] The sludge synergistic curing agent was prepared based on the above-mentioned substrate, comprising: 30% fly ash, 18.7% sulphoaluminate cement and 10% modified phosphogypsum powder were mixed to obtain a first curing agent mixture.
[0113] 15% biochar loaded nano-iron and 5% attapulgite were added into the first curing agent mixture to obtain a second curing agent mixture.
[0114] 8.7% polyaspartic acid-co-acrylamide was added into water to prepare a polyaspartic acid-co-acrylamide solution with a mass fraction of 12%, and 4.8% carboxymethyl cellulose sodium was added into water to prepare a carboxymethyl cellulose sodium solution with a mass fraction of 8%; the polyaspartic acid-co-acrylamide solution and the carboxymethyl cellulose sodium solution were added into the second curing agent mixture and mixed uniformly to obtain a third curing agent mixture. 5% silica ash, 1.6% magnesium carbonate and 1.2% tartaric acid were added into the third curing agent mixture and mixed uniformly to obtain the sludge synergistic curing agent.
[0115] The sludge synergistic curing agent prepared in this example was mixed with sludge, the initial moisture content of the sludge was 79.6%, dry sludge was added until the moisture content was reduced to 75.8%, and the mass ratio of the sludge synergistic curing agent to the sludge was 1:5.5; after mixing, the sludge was cured for 48h in an environment with a humidity of 87% for primary curing, and then cured naturally for 6.5d; the cured body was tested, and the 3-day unconfined compressive strength was 341kPa, the Pb 2+ The leaching concentration was 0.035mg / L, and the phenolic compound removal rate was 90.8%.
[0116] Example 4 Substrate preparation: Secondary fly ash from thermal power plants was ultra-finely processed using an air jet mill to obtain fly ash. The milling pressure during the process was 0.8 MPa, and the classifying wheel speed was 3000 r / min. The particle size distribution of the fly ash was: D10 = 2.0 μm, D50 = 6.1 μm, D90 = 12.1 μm, with a specific surface area of 475 m². 2 / g; by mass percentage, fly ash comprises 48.3% SiO2, 25% Al2O3, 5.2% Fe2O3, 20% CaO, with the remainder being impurities.
[0117] By mass percentage, sulfoaluminate cement comprises 45% calcium sulfoaluminate, 28.2% dicalcium silicate, 15% tetracalcium aluminoferrite, and the remainder being impurities.
[0118] Citric acid solution and phosphogypsum powder were mixed at a liquid-to-solid mass ratio of 1:2 and placed in a constant temperature water bath at 70°C. The mixture was mechanically stirred and soaked for 12 hours at a stirring rate of 150 r / min. During this period, the pH value was measured every 2 hours until the pH value stabilized at 7.0. Vacuum filtration was performed under a vacuum of -0.08 MPa. After filtration, the powder was dried at 80°C with forced air until the moisture content reached 4.5%, thus obtaining modified phosphogypsum powder. The modified phosphogypsum powder was then pulverized to 300 mesh using a Raymond mill for later use. The mass fraction of the citric acid solution was 4%.
[0119] Adding biochar to FeSO4 The solution was magnetically stirred at 300 rpm for 30 minutes in 7H2O to obtain the first mixture; then, under nitrogen atmosphere, Fe was added... 2+ and BH4 - The molar ratio of the two components was 1:2. NaBH4 solution was added dropwise to the first mixture to initiate the reaction. After 1 hour of reaction, the reaction solution was vacuum filtered to obtain black iron nanoparticles. The black iron nanoparticles were washed three times with deionized water and then once with anhydrous ethanol. They were then vacuum dried at 60°C and a vacuum degree of -0.09 MPa for 8 hours to obtain a black powder, which is the biochar-supported iron nanoparticle. The biochar and FeSO4 components... The mass-to-volume ratio of the 7H₂O solution is 1 g: 15 mL, and the FeSO₄ content is... The concentration of the 7H2O solution was 0.1 mol / L; the concentration of the NaBH4 solution was 0.25 mol / L; the detection showed that the particle size of the nano-iron in the biochar-supported nano-iron was 58 nm, and the loading of nano-iron was 9.1%. The ground attapulgite raw material is added to deionized water in a solid-liquid mass ratio of 1:6, stirred at a speed of 500 r / min for 30 min, uniformly stirred, and then left to stand for 2 h, and the upper layer of the suspension is taken; 4% hydrochloric acid solution is added to the upper layer of the suspension, and the reaction is carried out at 80°C for 2 h, after the reaction, the reaction liquid is filtered, and the solid phase after filtration is washed to neutral with deionized water, and then dried at 100°C, and then ultra-finely pulverized to obtain attapulgite; the CEC of the attapulgite after purification is 20.8 meq / 100 g.
[0120] L-aspartic acid and acrylamide are dissolved in water to obtain a second mixed solution, and the molar ratio of L-aspartic acid to acrylamide is 1:3; ammonium persulfate is added to the second mixed solution and uniformly mixed, and a polymerization reaction is initiated in a nitrogen atmosphere in a constant temperature water bath at 60°C for 4 h to obtain a reaction product; the reaction product is concentrated to a solid content of 30% by rotary evaporation in a vacuum environment at 70°C and a vacuum degree of-0.08 MPa, and then purified by ethanol precipitation, and then dried at 80°C and a vacuum degree of-0.08 MPa, and then ground through an 80-mesh sieve to obtain polyaspartic acid-co-acrylamide; the mass of ammonium persulfate is 2.8% of the total mass of L-aspartic acid and acrylamide.
[0121] The silica ash is selected from a ferrosilicon smelting by-product of an iron alloy factory, has a SiO2 content of 90%, a particle size of 0.1-0.5 μm, and a density of 2.2 g / cm 3 .
[0122] The magnesium carbonate is selected from light magnesium carbonate; and the tartaric acid is selected from analytical pure tartaric acid.
[0123] The sludge synergistic solidifying agent is prepared based on the above-mentioned substrate, and includes: The first solidifying agent mixture is obtained by mixing 24.3% fly ash, 20% sulfoaluminate cement, and 12.3% modified phosphogypsum powder.
[0124] The second solidifying agent mixture is obtained by adding 17.3% biochar-loaded nano-iron and 8.5% attapulgite to the first solidifying agent mixture.
[0125] The polyaspartic acid-co-acrylamide solution with a mass fraction of 12% is prepared by adding 7.8% polyaspartic acid-co-acrylamide to water, and the carboxymethyl cellulose sodium solution with a mass fraction of 8% is prepared by adding 4.3% carboxymethyl cellulose sodium to water, and the third solidifying agent mixture is obtained by adding the polyaspartic acid-co-acrylamide solution and the carboxymethyl cellulose sodium solution to the second solidifying agent mixture and uniformly mixing. The sludge synergistic solidifying agent is obtained by adding 3% silica ash, 1% magnesium carbonate, and 1.5% tartaric acid to the third solidifying agent mixture and uniformly mixing.
[0126] The sludge prepared in this example is mixed with the sludge co-curing agent, the initial moisture content of the sludge is 83.7%, dry sludge is added until the moisture content is reduced to 76.9%, the mass ratio of the sludge co-curing agent to the sludge is 1:6.1. After mixing, the primary curing is carried out in an environment with a humidity of 84% for 48h, and then natural curing is carried out for 7d; the cured body is tested, the 3-day unconfined compressive strength is 332kPa, the Cr 6+ The leaching concentration is 0.045mg / L, and the comprehensive removal rate of organic pollutants is 91.2%.
[0127] The endpoints of the ranges and any values disclosed in the present application are not limited to the precise values recited. The ranges and values should be interpreted as being approximate. Individual endpoints of the ranges, the endpoints of the ranges and the individual values can be combined with one another to form new ranges or values, which are to be construed as being specifically disclosed herein. In the following, the individual technical solutions can be combined with one another to form new technical solutions, which are to be construed as being specifically disclosed herein.
[0128] The above examples are only used to illustrate the technical solutions of the present application but not to limit it. Although the present application has been described in detail with reference to the above examples, the ordinary skilled in the art can still modify or replace the specific embodiments of the present application, and any modification or replacement which does not depart from the spirit and scope of the present application is within the protection scope of the claims of the present application.
Claims
1. A sludge synergistic solidifying agent based on microbial mineralization and nanocomposite, characterized in that, By weight percentage, it includes 20%–30% fly ash, 15%–20% sulfoaluminate cement, 10%–15% modified phosphogypsum powder, 15%–20% biochar-supported nano-iron, 5%–10% attapulgite, 6%–10% polyaspartic acid-co-acrylamide, 4%–5% sodium carboxymethyl cellulose, 3%–5% silica fume, 1%–3% magnesium carbonate, and 1%–2% tartaric acid.
2. The sludge synergistic solidification agent based on microbial mineralization and nanocomposite as described in claim 1, characterized in that, By mass percentage, the fly ash comprises 45%~50% SiO2, 25%~30% Al2O3, 4%~6% Fe2O3, 15%~20% CaO, and the remainder is impurities.
3. The sludge synergistic solidifying agent based on microbial mineralization and nanocomposite as described in claim 1, characterized in that, By mass percentage, the sulfoaluminate cement comprises 40%~45% calcium sulfoaluminate, 25%~30% dicalcium silicate, 10%~15% tetracalcium aluminoferrite, and the remainder being impurities.
4. The sludge synergistic solidifying agent based on microbial mineralization and nanocomposite as described in claim 1, characterized in that, The method for preparing the modified phosphogypsum powder includes: The citric acid solution and phosphogypsum powder were mixed at a liquid-to-solid mass ratio of 1:(2~3) and reacted at 60~70℃ until the pH reached 6.5~7.
5. The solid phase after the reaction was dried to obtain modified phosphogypsum powder. The mass fraction of the citric acid solution was 3%~5%.
5. The sludge synergistic solidifying agent based on microbial mineralization and nanocomposite as described in claim 1, characterized in that, The method for preparing biochar-supported iron nanoparticles includes: Adding biochar to FeSO4 The first mixture was obtained from the 7H2O solution, FeSO4 The concentration of the 7H2O solution was 0.1~0.2 mol / L; biochar and FeSO4 The mass-to-volume ratio of the 7H₂O solution is 1 g: (10~15) mL; In inert gases, according to Fe 2+ and BH4 - The molar ratio was 1:(2~3). NaBH4 solution was added to the first mixture to react and obtain biochar-supported iron nanoparticles. The concentration of NaBH4 solution was 0.2~0.3mol / L.
6. The sludge synergistic solidifying agent based on microbial mineralization and nanocomposite as described in claim 1, characterized in that, The method for preparing the attapulgite soil includes: Add the attapulgite raw material to water and mix evenly according to the solid-liquid mass ratio of 1: (5~8). After standing, take the upper suspension. Hydrochloric acid solution is added to the upper suspension and reacted at 80~100℃. The solid phase after reaction is washed, dried and ground to obtain attapulgite. The mass fraction of hydrochloric acid solution is 3%~5%.
7. The sludge synergistic solidifying agent based on microbial mineralization and nanocomposite as described in claim 1, characterized in that, The method for preparing the polyaspartic acid-co-acrylamide includes: L-Aspartic acid and acrylamide were dissolved in water to obtain a second mixture, with a molar ratio of L-aspartic acid to acrylamide of 1:(3~4). Ammonium persulfate was added to the second mixture, and the reaction was carried out at 60-70°C under an inert atmosphere to obtain the reaction product. The reaction product was evaporated, precipitated and vacuum dried to obtain polyaspartic acid-co-acrylamide. The mass of ammonium persulfate added was 2%-3% of the total mass of L-aspartic acid and acrylamide.
8. A method for preparing a sludge synergistic solidifying agent based on microbial mineralization and nanocomposite according to any one of claims 1-7, characterized in that, include: The first curing agent mixture is obtained by mixing fly ash, sulfoaluminate cement, and modified phosphogypsum powder. A second curing agent mixture is obtained by adding biochar-supported nano-iron and attapulgite to the first curing agent mixture. Polyaspartic acid-co-acrylamide was prepared into a polyaspartic acid-co-acrylamide solution, and sodium carboxymethyl cellulose was prepared into a sodium carboxymethyl cellulose solution. The polyaspartic acid-co-acrylamide solution and the sodium carboxymethyl cellulose solution were added to the second curing agent mixture and mixed to obtain the third curing agent mixture. Add silica fume, magnesium carbonate and tartaric acid to the third curing agent mixture and mix evenly to obtain sludge curing agent.
9. The preparation method of the sludge synergistic solidification agent based on microbial mineralization and nanocomposite according to claim 8, characterized in that, The mass fraction of the polyaspartic acid-co-acrylamide solution is 10%~15%.
10. The preparation method of the sludge synergistic solidification agent based on microbial mineralization and nanocomposite according to claim 8, characterized in that, The sodium carboxymethyl cellulose solution has a mass fraction of 5% to 10%.
Citation Information
Patent Citations
Mud curing agent
CN108911448A
Soft foundation material prepared through solidification of sludge and preparation method of soft foundation material
CN109384444A
Preparation method and application of copper-iron carbon nano gel bead
CN111151226A
Phosphogypsum hardening agent and preparation method and application thereof
CN114230301A
Ardealite-based grouting material for tunnel engineering and preparation and application thereof
CN118930210A
Cited By
Drying agent for sludge with high water content, high salinity and high organic matter as well as preparation method and application of drying agent
CN121342304A