Magnesium-modified narrow-spectrum green luminescent material, preparation method and application thereof, and laser display device

By introducing Mg2+ solid solution substitution into SrGa2S4:Eu2+ and optimizing the local coordination environment of Eu2+, magnesium-modified narrow-spectrum green luminescent materials were prepared. This solved the problem of low quantum efficiency of SrGa2S4:Eu2+ phosphor, achieving efficient narrow-spectrum green light emission and high quantum efficiency, which is suitable for high-end display technology.

CN121064832APending Publication Date: 2025-12-05LANZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202511189053.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-08-25
Publication Date
2025-12-05

AI Technical Summary

Technical Problem

The existing SrGa2S4:Eu2+ phosphor has low quantum efficiency, which makes it difficult to meet the requirements of high efficiency, low cost and sustainable manufacturing for high-end display technology.

Method used

Magnesium-modified narrow-spectrum green luminescent material (Sr1-xMgx)Ga2S4:0.04Eu2+ was prepared by introducing Mg2+ to perform solid solution substitution of SrGa2S4:Eu2+ and optimizing the local coordination environment of Eu2+. The synthesis was carried out by high-temperature solid-state reaction method.

Benefits of technology

It significantly improves the luminescence quantum efficiency, narrows the half-peak width, and achieves an external quantum efficiency of 53.1%, making it suitable for wide color gamut LCD displays and laser displays.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121064832A_ABST
    Figure CN121064832A_ABST
Patent Text Reader

Abstract

The invention provides a magnesium-modified narrow-spectrum green luminescent material, a preparation method and application thereof, and a laser display device, and belongs to the technical field of luminescent materials. The magnesium modified narrow-spectrum green light-emitting material has excellent light-emitting performance, when x is equal to 0.2, the emission wavelength of the (Sr0. 8Mg0. 2) Ga2S4: 0.04 Eu < 2 + > narrow-spectrum green light-emitting material under excitation of 450 nm blue light is 537.7 nm, chromaticity coordinates are (0.2916, 0.6766), the half-peak width is 47 nm, and the external quantum efficiency reaches 53.1%, which obviously exceeds that of undoped modified SrGa2S4: Eu < 2 + > fluorescent powder (the external quantum efficiency is 33.1%). The liquid crystal display has important application prospects in wide-color-gamut liquid crystal display and laser display, and has important research significance and application value for promoting the development of high-end display (such as laser display).
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present application relates to the technical field of luminescent materials, in particular to a magnesium-modified narrow-spectrum green luminescent material, a preparation method and application thereof, and a laser display device. BACKGROUND

[0002] Display technology is rapidly developing towards high color gamut, high brightness and low energy consumption, which puts forward more stringent requirements on the key material-fluorescent powder, especially green fluorescent powder, for realizing high color reproduction and excellent visual comfort. The high sensitivity of the human eye to the 520-560 nm green light band makes the emission characteristics (especially the half-width and quantum efficiency) of the fluorescent powder in this band directly determine the color gamut coverage and visual experience of the display device. High-end display technology (such as laser display) usually requires the half-width of green fluorescent powder to be ≤50 nm. Therefore, developing new green fluorescent powder with narrow-spectrum emission and high quantum efficiency has become a current research hotspot and an urgent need of the industry.

[0003] At present, traditional green fluorescent powder mainly includes rare earth ion-doped oxides, silicates, phosphates and chalcogenides. Silicate systems are widely used in medium and low-end displays due to their low cost and moderate performance. High-end displays mainly rely on β-SiAlON:Eu 2+ oxide fluorescent powder, which has relatively high luminous efficiency and color purity (half-width of about 54 nm), but has inherent defects such as extremely high synthesis temperature (usually higher than 1900℃), complex preparation process, high energy consumption, etc., which is difficult to meet the requirements of new generation display technology for high efficiency, low cost and sustainable manufacturing.

[0004] In recent years, sulfide fluorescent powder has become an important research direction due to its excellent luminescent performance and relatively low synthesis temperature (usually less than 1100℃). Among them, SrGa2S4:Eu 2+ fluorescent powder is considered as a strong candidate for the next generation of high-efficiency green fluorescent powder due to its potential narrow-spectrum emission characteristics (half-width of about 50 nm) and moderate synthesis temperature. However, the reported SrGa2S4:Eu 2+ fluorescent powder still has a large room for improvement in luminous quantum efficiency (EQE≤40%), which limits its practical application potential. SUMMARY

[0005] The purpose of the present application is to provide a magnesium-modified narrow-spectrum green luminescent material, a preparation method and application thereof, and a laser display device, which can improve the luminous quantum efficiency of green luminescent material.

[0006] In order to achieve the above-mentioned application purposes, the present application provides the following technical solutions:

[0007] The application provides a magnesium-modified narrow-spectrum green luminescent material. 1-x Mg x )Ga2S4:0.04Eu 2+ , wherein 0

[0008] Preferably, x=0.1-0.4.

[0009] Preferably, the magnesium-modified narrow-spectrum green luminescent material is crystallized in an orthorhombic Fddd space group and is composed of [SrS8] and [GaS4] polyhedral structure units.

[0010] When x=0.2, the molecular weight of the magnesium-modified narrow-spectrum green luminescent material is 345.24.

[0011] The application provides a preparation method of the magnesium-modified narrow-spectrum green luminescent material.

[0012] According to a required stoichiometric ratio, a Sr source, a Mg source, a Ga source and an Eu source are ground and mixed to obtain a mixture;

[0013] In a nitrogen atmosphere, S source vapor carried by nitrogen is introduced into the mixture to perform solid-phase sintering, so as to obtain the magnesium-modified narrow-spectrum green luminescent material.

[0014] Preferably, the Sr source includes SrCO3, SrO or SrS; the Mg source includes MgCO3, MgO or MgS; the Ga source includes Ga2O3 or Ga2S3; and the Eu source includes Eu2O3 or Eu2S3.

[0015] Preferably, the S source used in the S source vapor includes CS2.

[0016] Preferably, the temperature of the solid-phase sintering is 850-1050 ℃, the holding time is 4-6 h, and the temperature rising rate is 3-5 ℃ / min.

[0017] The application provides an application of the magnesium-modified narrow-spectrum green luminescent material or the magnesium-modified narrow-spectrum green luminescent material prepared by the preparation method as a green luminescent element in a laser display device.

[0018] The application provides a laser display device, which comprises an excitation light source and a light conversion element, and the light conversion element comprises the magnesium-modified narrow-spectrum green luminescent material or the magnesium-modified narrow-spectrum green luminescent material prepared by the preparation method.

[0019] The application provides a magnesium-modified narrow-spectrum green luminescent material, which has a chemical composition of (Sr1-x Mg x Ga2S4: 0.04Eu 2+ It belongs to the orthorhombic crystal system. Preferably, when x = 0.2, the molecular weight of this crystal is 345.24, the space group is Fddd, and the cell parameters are... This narrow-spectrum green luminescent material exhibits excellent luminescence performance: under 450 nm blue light excitation, the emission wavelength is 537.7 nm, the chromaticity coordinates are (0.2916, 0.6766), the full width at half maximum (FWHM) is 47 nm, and the external quantum efficiency reaches 53.1%, significantly surpassing that of undoped modified SrGa2S4:Eu 2+ Phosphors (with an external quantum efficiency of 33.1%) have significant application prospects in wide color gamut liquid crystal displays and laser displays, and are of great research significance and application value for promoting the development of high-end displays (such as laser displays).

[0020] This invention introduces Mg 2+ For SrGa2S4:Eu 2+ Solid solution substitution modification, Mg 2+ Solid solution achieves cell shrinkage, increases crystal rigidity, and optimizes Eu. 2+ The local coordination environment narrows the half-maximum width of the emission spectrum, effectively controlling the matrix lattice environment and Eu while maintaining its narrow-spectrum emission characteristics. 2+ The luminescent center is located, thereby significantly improving the luminescence quantum efficiency of the material.

[0021] This invention is the first to realize Mg 2+ A novel narrow-spectrum green luminescent material was successfully prepared by effective solid solution in the target matrix lattice. XRD crystal structure analysis confirmed that… Figure 13 ), Mg 2+ Ions dissolve into the crystal lattice and replace Sr 2+ The lattice points lead to cell shrinkage, which significantly enhances the overall rigidity of the crystal, thereby improving quantum efficiency; more importantly, this is achieved by using Mg... 2+ Solid solution-induced structural rigidification effectively optimized the luminescent center Eu. 2+ The local coordination environment surrounding the ions reduces the distortion of the coordination polyhedra. This optimized local structure is directly reflected in the luminescent properties of the material: on the one hand, Eu... 2+ The half-width at half maximum (FWHM) of the emission spectrum of the 5d→4f transition is significantly narrowed, realizing high-purity narrow-spectrum green luminescence. On the other hand, the quantum efficiency (QE) of the material is also significantly improved, mainly due to the fact that the enhanced crystal rigidity and the optimization of the local environment jointly suppress the nonradiative transition channels and increase the radiative recombination probability.

[0022] The magnesium-modified narrow-spectrum green luminescent material of this invention is based on Mg solid solution modification and is synthesized by high-temperature solid-phase reaction method. It is prepared by solid-phase sintering in a sulfur source atmosphere using Sr source, Mg source, Ga source and Eu source as raw materials. The method is simple and the raw materials are widely available. Attached Figure Description

[0023] Figure 1 SrGa2S4:0.04Eu prepared for Comparative Example 1 2+ A schematic diagram of the crystal structure;

[0024] Figure 2 SrGa2S4:0.04Eu prepared for Comparative Example 1 2+ The refined XRD pattern;

[0025] Figure 3 SrGa2S4:0.04Eu prepared for Comparative Example 1 2+ Excitation and emission spectra;

[0026] Figure 4 (Sr) prepared in Examples 1-5 1-x Mg x Ga2S4: 0.04Eu 2+ XRD refinement patterns of (x=0.1(a), x=0.2(b), x=0.3(c), x=0.4(d), x=0.5(e));

[0027] Figure 5 (Sr) prepared in Example 1 0.9 Mg 0.1 Ga2S4: 0.04Eu 2+ Excitation and emission spectra;

[0028] Figure 6 (Sr) prepared in Example 2 0.8 Mg 0.2 Ga2S4: 0.04Eu 2+ Excitation and emission spectra;

[0029] Figure 7 (Sr) prepared in Example 3 0.7 Mg 0.3 Ga2S4: 0.04Eu 2+ Excitation and emission spectra;

[0030] Figure 8 (Sr) prepared in Example 4 0.6 Mg 0.4 Ga2S4: 0.04Eu 2+ Excitation and emission spectra;

[0031] Figure 9(Sr) prepared in Example 5 0.5 Mg 0.5 Ga2S4: 0.04Eu 2+ Excitation and emission spectra;

[0032] Figure 10 (Sr) prepared in Example 2 0.8 Mg 0.2 Ga2S4: 0.04Eu 2+ Chromaticity coordinates under 450nm blue light excitation (CIE 1931);

[0033] Figure 11 (Sr) prepared in Example 2 0.8 Mg 0.2 Ga2S4: 0.04Eu 2+ Compared with the undoped modified SrGa2S4 in Comparative Example 1: 0.04Eu 2+ Comparison of quantum efficiency under 450nm blue light excitation;

[0034] Figure 12 (Sr) prepared in Example 2 0.8 Mg 0.2 Ga2S4: 0.04Eu 2+ Performance under 450nm laser excitation: (a) emission spectrum at different optical power densities, (b) optical flux and conversion efficiency at different laser power densities;

[0035] Figure 13 (Sr) prepared in Examples 1-5 1-x Mg x Ga2S4: 0.04Eu 2+ XRD patterns of luminescent materials (x = 0.1, 0.2, 0.3, 0.4, 0.5). Detailed Implementation

[0036] In this invention, unless otherwise specified, the raw materials or reagents required for preparation are all commercially available products well known to those skilled in the art.

[0037] This invention provides a magnesium-modified narrow-spectrum green luminescent material with the chemical composition (Sr) 1-x Mg x Ga2S4: 0.04Eu 2+ , where 0 < x ≤ 0.5.

[0038] In this invention, x = 0.1 to 0.4, more preferably 0.2 to 0.3.

[0039] In the present application, the magnesium modified narrow-spectrum green luminescent material crystallizes in orthorhombic space group Fddd, and is composed of [SrS8] and [GaS4] polyhedral structure units.

[0040] In the present application, when x=0.2, the molecular weight of the magnesium modified narrow-spectrum green luminescent material is 345.24.

[0041] The present application provides a preparation method of the magnesium modified narrow-spectrum green luminescent material as described in the above technical solution, which comprises the following steps:

[0042] According to the required stoichiometric ratio, the Sr source, the Mg source, the Ga source and the Eu source are ground and mixed to obtain a mixture;

[0043] Under a nitrogen atmosphere, S source vapor carried by nitrogen is introduced into the mixture to perform solid phase sintering, so as to obtain the magnesium modified narrow-spectrum green luminescent material.

[0044] In the present application, the Sr source preferably comprises SrCO3, SrO or SrS; the Mg source preferably comprises MgCO3, MgO or MgS; the Ga source preferably comprises Ga2O3 or Ga2S3; and the Eu source preferably comprises Eu2O3 or Eu2S3.

[0045] In the present application, the S source used in the S source vapor preferably comprises CS2.

[0046] In the present application, the Sr source, the Mg source, the Ga source and the Eu source are preferably ground and mixed uniformly according to the stoichiometric ratio, and are loaded into an alumina crucible. The alumina crucible is placed in a program-controlled tube furnace, and S source (loaded in a liquid gas washing bottle) is placed at the gas inlet. S source vapor formed is introduced into the tube furnace by using nitrogen as the carrier gas to perform solid phase sintering. After the heat preservation is completed, the temperature is cooled to room temperature at a cooling rate of 5℃ / min, so as to obtain the magnesium modified narrow-spectrum green luminescent material.

[0047] In the present application, the temperature of the solid phase sintering is preferably 850-1050℃, more preferably 950-1000℃, and the heat preservation time is preferably 4-6h, more preferably 5h. The temperature rising rate for rising to the temperature of the solid phase sintering is preferably 3-5℃ / min, more preferably 4-5℃ / min.

[0048] The present application provides an application of the magnesium modified narrow-spectrum green luminescent material as described in the above technical solution or the magnesium modified narrow-spectrum green luminescent material prepared by the preparation method as described in the above technical solution as a green luminescent element in a laser display device.

[0049] The application provides a laser display device, comprising an excitation light source and a light conversion element, wherein the light conversion element comprises the magnesium-modified narrow-spectrum green luminescent material according to the technical scheme or the magnesium-modified narrow-spectrum green luminescent material prepared by the preparation method according to the technical scheme. The laser display device is preferably a laser projection or a laser television; and the laser display device is used for converting blue laser into high-purity green light, so as to construct a full-color laser display system.

[0050] The specific embodiments of the application are described in detail below, but it should be understood that the protection scope of the application is not limited by the specific embodiments. Based on the examples in the application, all other examples obtained by those skilled in the art without creative labor are within the protection scope of the application.

[0051] The experimental methods in the embodiments of the application are all conventional methods unless otherwise specified; and the reagents and raw materials described below are all commercially available and are not treated unless otherwise specified.

[0052] Comparative Example 1

[0053] SrCO3, Ga2O3 and Eu2O3 as raw materials, and a high-temperature solid-phase method is used to prepare SrGa2S4:0.04Eu 2+ :

[0054] According to the stoichiometric ratio, 0.4218 grams of SrCO3, 0.5579 grams of Ga2O3 and 0.0209 grams of Eu2O3 are weighed, and the weighed raw materials are uniformly mixed and ground, and then placed in a clean alumina crucible; the alumina crucible is placed in a program-controlled tube furnace, CS2 (loaded in a liquid gas washing bottle) is placed at the gas inlet, and CS2 vapor formed is introduced into the tube furnace by taking nitrogen as a carrier gas, and the temperature is raised to 950℃ at a rate of 5℃ / min and kept for 4h for solid-phase sintering; after the heat preservation is completed, the temperature is cooled to room temperature at a rate of 5℃ / min, and SrGa2S4:0.04Eu 2+ is obtained.

[0055] Example 1

[0056] SrCO3, MgCO3, Ga2O3 and Eu2O3 as raw materials, and a high-temperature solid-phase method is used to prepare (Sr 0.9 Mg 0.1 )Ga2S4:0.04Eu 2+ :

[0057] According to stoichiometric ratio, 0.3779 grams of SrCO3, 0.0251 grams of MgCO3, 0.5579 grams of Ga2O3 and 0.0209 grams of Eu2O3 are weighed, the weighed raw materials are mixed uniformly, and then grinded and put into a clean alumina crucible; the alumina crucible is put into a program-controlled tubular furnace, CS2 (loaded in a liquid gas washing bottle) is placed at an air inlet, CS2 vapor formed is passed into the tubular furnace with nitrogen as a carrier gas, the temperature is raised to 950℃ at a raising rate of 5℃ / min, and then kept for 4 hours for solid phase sintering; after the keeping, the temperature is cooled to room temperature at a cooling rate of 5℃ / min, and (Sr 0.9 Mg 0.1 )Ga2S4:0.04Eu 2+ luminescent material is obtained.

[0058] Example 2

[0059] SrCO3, MgCO3, Ga2O3 and Eu2O3 are used as raw materials, and (Sr 0.8 Mg 0.2 )Ga2S4:0.04Eu 2+ :

[0060] According to stoichiometric ratio, 0.3779 grams of SrCO3, 0.0251 grams of MgCO3, 0.5579 grams of Ga2O3 and 0.0209 grams of Eu2O3 are weighed, the weighed raw materials are mixed uniformly, and then grinded and put into a clean alumina crucible; the alumina crucible is put into a program-controlled tubular furnace, CS2 (loaded in a liquid gas washing bottle) is placed at an air inlet, CS2 vapor formed is passed into the tubular furnace with nitrogen as a carrier gas, the temperature is raised to 950℃ at a raising rate of 5℃ / min, and then kept for 4 hours for solid phase sintering; after the keeping, the temperature is cooled to room temperature at a cooling rate of 5℃ / min, and (Sr 0.8 Mg 0.2 )Ga2S4:0.04Eu 2+ luminescent material is obtained.

[0061] Example 3

[0062] SrCO3, MgCO3, Ga2O3 and Eu2O3 are used as raw materials, and (Sr 0.7 Mg 0.3 )Ga2S4:0.04Eu 2+ :

[0063] According to stoichiometric ratio, 0.29 gram of SrCO3, 0.0753 gram of MgCO3, 0.5579 gram of Ga2O3 and 0.0209 gram of Eu2O3 are weighed, the weighed raw materials are mixed uniformly, grinded and then put into a clean alumina crucible; the alumina crucible is put into a program-controlled tubular furnace, CS2 (loaded in a liquid gas washing bottle) is placed at an air inlet, CS2 vapor formed is passed into the tubular furnace with nitrogen as a carrier gas, the temperature is raised to 950 ℃ at a raising rate of 5 ℃ / min and kept for 4 hours to perform solid phase sintering; after the keeping, the temperature is cooled to room temperature at a cooling rate of 5 ℃ / min, and (Sr 0.7 Mg 0.3 )Ga2S4:0.04Eu 2+ luminescent material is obtained.

[0064] Example 4

[0065] SrCO3, MgCO3, Ga2O3 and Eu2O3 are used as raw materials, and (Sr 0.6 Mg 0.4 )Ga2S4:0.04Eu 2+ :

[0066] According to stoichiometric ratio, 0.2460 gram of SrCO3, 0.1004 gram of MgCO3, 0.5579 gram of Ga2O3 and 0.0209 gram of Eu2O3 are weighed, the weighed raw materials are mixed uniformly, grinded and then put into a clean alumina crucible; the alumina crucible is put into a program-controlled tubular furnace, CS2 (loaded in a liquid gas washing bottle) is placed at an air inlet, CS2 vapor formed is passed into the tubular furnace with nitrogen as a carrier gas, the temperature is raised to 950 ℃ at a raising rate of 5 ℃ / min and kept for 4 hours to perform solid phase sintering; after the keeping, the temperature is cooled to room temperature at a cooling rate of 5 ℃ / min, and (Sr 0.6 Mg 0.4 )Ga2S4:0.04Eu 2+ luminescent material is obtained.

[0067] Example 5

[0068] SrCO3, MgCO3, Ga2O3 and Eu2O3 are used as raw materials, and (Sr 0.5 Mg 0.5 )Ga2S4:0.04Eu 2+ :

[0069] According to the stoichiometric ratio, 0.2021 g of SrCO3, 0.1255 g of MgCO3, 0.5579 g of Ga2O3, and 0.0209 g of Eu2O3 were weighed out. The weighed raw materials were mixed evenly, ground, and placed in a clean alumina crucible. The alumina crucible was placed in a temperature-controlled tube furnace, and CS2 (containing liquid gas washing bottle) was placed at the inlet. The generated CS2 vapor was introduced into the tube furnace using nitrogen as the carrier gas. The temperature was increased to 950℃ at a rate of 5℃ / min and held for 4 hours for solid-state sintering. After the holding period, the temperature was cooled to room temperature at a rate of 5℃ / min to obtain (SrCO3). 0.5 Mg 0.5 Ga2S4: 0.04Eu 2+ Luminescent materials.

[0070] Characterization and testing

[0071] Comparative Example 1 prepared SrGa2S4: 0.04Eu 2+ Crystal structure such as Figure 1 As shown, it includes [SrS8] and [GaS4] polyhedral structures.

[0072] Comparative Example 1 prepared SrGa2S4: 0.04Eu 2+ XRD refinement pattern as follows Figure 2 As shown, the excitation and emission spectra are as follows: Figure 3 As shown, under 450nm blue light excitation, its emission peak is located at 536.20nm and its full width at half maximum (FWHM) is 52.07nm.

[0073] The (Sr) prepared in Example 1 0.9 Mg 0.1 Ga2S4: 0.04Eu 2+ The refined XRD pattern of the luminescent material is as follows: Figure 4 As shown in (a), the excitation and emission spectra are as follows: Figure 5 As shown, under 450nm blue light excitation, its emission peak is located at 537.3nm and its full width at half maximum (FWHM) is 49.6nm.

[0074] Example 2 prepared (Sr 0.8 Mg 0.2 Ga2S4: 0.04Eu 2+ The refined XRD pattern of the luminescent material is as follows: Figure 4 As shown in (b), the excitation and emission spectra are as follows: Figure 6 As shown, the chromaticity coordinates are as follows Figure 10 As shown, under 450nm blue light excitation, its emission peak is located at 537.75nm with a full width at half maximum (FWHM) of 47nm and chromaticity coordinates of (0.2916, 0.6766).

[0075] (Sr 0.7 Mg 0.3 )Ga2S4:0.04Eu 2+ The XRD refinement pattern of the luminescent material prepared in Example 3 is shown in (a) of Figure 4 The excitation and emission spectra are shown in (b) of Figure 7 It can be seen that under 450 nm blue light excitation, the emission peak is located at 536.2 nm with a half-height width of 48 nm.

[0076] (Sr 0.6 Mg 0.4 )Ga2S4:0.04Eu 2+ The XRD refinement pattern of the luminescent material prepared in Example 4 is shown in (d) of Figure 4 The excitation and emission spectra are shown in (e) of Figure 8 It can be seen that under 450 nm blue light excitation, the emission peak is located at 538.5 nm with a half-height width of 47.6 nm.

[0077] (Sr 0.5 Mg 0.5 )Ga2S4:0.04Eu 2+ The XRD refinement pattern of the luminescent material prepared in Example 5 is shown in (e) of Figure 4 The excitation and emission spectra are shown in (f) of Figure 9 It can be seen that under 450 nm blue light excitation, the emission peak is located at 538.2 nm with a half-height width of 46.8 nm.

[0078] It is tested that the luminescent materials prepared in Examples 1-5 and Comparative Example 1 above belong to the orthorhombic system, crystallize in the orthorhombic system, and the space group is Fddd.

[0079] The quantum efficiency of (Sr 0.8 Mg 0.2 )Ga2S4:0.04Eu 2+ and the un-doped modified SrGa2S4:0.04Eu 2+ under 450 nm blue light excitation is tested, and the results are shown in Figure 11 The external quantum efficiency of (Sr 0.8 Mg 0.2 )Ga2S4:0.04Eu 2+ in Example 2 reaches 53.1%, which significantly surpasses the un-doped modified SrGa2S4:Eu 2+ fluorescent powder (external quantum efficiency is 33.1%) in Comparative Example 1.

[0080] The quantum efficiency of (Sr 0.8 Mg 0.2 )Ga2S4:0.04Eu 2+The luminescent materials were used in laser display devices and tested by building a laser excitation fluorescence conversion device and a phosphor wheel. Figure 12 Fig. 1(a) shows the emission spectra of the phosphor wheel under irradiation of different light power densities of 450 nm blue laser. All the emission spectra are composed of sharp emission of 450 nm laser and narrowband emission of phosphor. The overall emission intensity increases with the increase of excitation power. It is worth noting that even if the power density of the blue laser diode is as high as 72.64 W / mm 2 , the emission intensity does not decrease. Figure 12 Fig. 1(b) shows the relationship between luminous flux, conversion efficiency and incident laser power density, from Figure 12 It can be seen from Fig. 1(b) that the luminous flux will show a clear sub-linear relationship with the increase of incident laser power density. Specifically, when the incident laser power density increases from 14.60 W / mm 2 to 72.64 W / mm 2 , the luminous flux increases from 583.34 lm to 1371.32 lm; Figure 12 Fig. 1(b) also shows the change of conversion efficiency with incident laser power density, and the results show that the conversion efficiency continuously decreases with the increase of incident laser power density, which indicates that the energy in the phosphor is continuously lost when the phosphor is irradiated at high power density.

[0081] Figure 13 Fig. 2 shows the XRD patterns of (Sr 1-x Mg x )Ga2S4:0.04Eu 2+ (x=0.1, 0.2, 0.3, 0.4, 0.5) luminescent materials prepared for Examples 1-5, and the observation of characteristic diffraction peaks Figure 13 shifted to high angles on the right side proves that Mg 2+ solid solution causes the unit cell to shrink.

[0082] The above only describes the preferred embodiments of the present application, and it should be noted that for those skilled in the art, without departing from the principles of the present application, a number of improvements and refinements can be made, and these improvements and refinements should also be considered as the protection scope of the present application.

Claims

1. A magnesium-modified narrow-band green luminescent material, characterized by, Chemical composition is (Sr 1-x Mg x )Ga2S4:0.04Eu 2+ wherein 0 < x < 0.

5.

2. The magnesium-modified narrow-band green luminescent material of claim 1, wherein, The x is 0.1-0.

4.

3. The magnesium-modified narrow-band green luminescent material of claim 1, wherein, The magnesium-modified narrow-spectrum green luminescent material crystallizes in an orthorhombic Fddd space group and is composed of [SrS8] and [GaS4] polyhedral structure units. When x is 0.2, the molecular weight of the magnesium-modified narrow-spectrum green luminescent material is 345.

24.

4. The method for preparing the magnesium-modified narrow-band green luminescent material according to any one of claims 1 to 3, characterized in that, The method comprises the following steps: According to the required stoichiometric ratio, the Sr source, the Mg source, the Ga source and the Eu source are ground and mixed to obtain a mixture; Under a nitrogen atmosphere, S source vapor carried by nitrogen is introduced into the mixture to perform solid phase sintering, thereby obtaining the magnesium-modified narrow-spectrum green luminescent material.

5. The preparation method according to claim 4, characterized in that, The Sr source includes SrCO3, SrO or SrS; the Mg source includes MgCO3, MgO or MgS; the Ga source includes Ga2O3 or Ga2S3; and the Eu source includes Eu2O3 or Eu2S3.

6. The preparation method according to claim 5, characterized in that, The S source used in the S source vapor includes CS2.

7. The preparation method according to claim 6, characterized in that, The temperature of the solid phase sintering is 850-1050℃, the holding time is 4-6h, and the temperature rising rate to the temperature of the solid phase sintering is 3-5℃ / min.

8. The magnesium-modified narrow-spectrum green luminescent material of any one of claims 1-3 or the magnesium-modified narrow-spectrum green luminescent material prepared by the preparation method of any one of claims 4-7 is applied to a laser display device as a green luminescent element.

9. A laser display device, characterized by comprising: The laser display device comprises an excitation light source and a light conversion element, and the light conversion element comprises the magnesium-modified narrow-spectrum green luminescent material of any one of claims 1-3 or the magnesium-modified narrow-spectrum green luminescent material prepared by the preparation method of any one of claims 4-7.