Hot continuous rolling production method of X70M pipeline steel without Mo and Ni

By designing a Mo- and Ni-free chemical composition and employing a low-temperature rolling and coiling process, the problem of improving low-temperature tear resistance and reducing the yield strength ratio of X70M grade pipeline steel while reducing alloy costs was solved, thus achieving an economical and efficient production method.

CN121082686APending Publication Date: 2025-12-09TANGSHAN IRON & STEEL GROUP +2

Patent Information

Application Number
CN202511148396.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-08-17
Publication Date
2025-12-09

AI Technical Summary

Technical Problem

Under the condition of reducing alloy costs, how to improve the low-temperature tear resistance and reduce the yield strength ratio of X70M grade pipeline steel to meet the economic benefits of steel enterprises and the technical requirements of engineering steel.

Method used

By employing a Mo- and Ni-free chemical composition design, combined with a step heating, low-temperature rolling, and low-temperature coiling process, and by controlling the content of elements such as carbon, manganese, chromium, and niobium, the formation of acicular ferrite and Mao island structures is promoted, unfavorable phase transformations are avoided, and a refined microstructure is achieved.

Benefits of technology

Without adding expensive alloying elements, the cost of the alloy is significantly reduced, the low-temperature tear resistance and tensile strength of the pipeline steel are improved, the yield strength ratio is kept at a low level, and the safety of the pipeline during service is guaranteed.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121082686A_ABST
    Figure CN121082686A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of pipeline steel production, and discloses a hot continuous rolling production method of Mo and Ni-free X70M pipeline steel, which comprises the processes of slab heating, rough rolling, finish rolling, laminar cooling and coiling, and the pipeline steel comprises the following chemical components in percentage by mass: 0.060 to 0.090 percent of C, 0.10 to 0.25 percent of Si, 1.50 to 1.70 percent of Mn, 0.20 to 0.30 percent of Cr, 0.045 to 0.070 percent of Nb, 0.020 to 0.050 percent of Al, less than or equal to 0.005 percent of S, less than or equal to 0.012 percent of P, 0.020 to 0.030 percent of Ti, less than or equal to 0.0050 percent of N and the balance of Fe and inevitable impurities. According to the pipeline steel, Mo and Ni are not added, the alloy cost is extremely low, meanwhile, a hot rolled steel strip of the pipeline steel has good low-temperature tearing resistance and low yield ratio, and the safety in the pipeline service process can be guaranteed.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present application relates to the technical field of pipeline steel production, in particular to a Mo-free and Ni-free X70M pipeline steel and a production method thereof. BACKGROUND

[0002] X70M grade pipeline steel has become the mainstream steel for major pipeline engineering construction at home and abroad. In the increasingly fierce situation of the steel industry, cost control has become an important measure for steel enterprises to develop high value-added products while achieving good economic benefits. It is difficult for traditional high-grade pipeline steel to achieve good technical performance indicators at a lower alloy cost. Therefore, it is difficult to meet the benefit requirements of steel enterprises and the technical requirements of engineering steel. Especially with the increasing complexity and harshness of pipeline service environment, the low-temperature tear resistance and yield ratio as important performance indicators of pipeline steel products are becoming more and more stringent. Low-temperature tear resistance directly determines the service life and service safety of the pipeline, and the yield ratio gradually becomes more stringent from ≤0.93 of API and national standard to ≤0.90, and even some engineering steels currently require control at ≤0.85. Therefore, as described above, it will face great difficulty and challenge to improve the comprehensive mechanical properties of the material while reducing the production cost.

[0003] Steel enterprises have conducted relevant research on pipeline steel. CN117467891A discloses a low-cost X70 grade high-strength pipeline steel plate coil and a production method thereof, which is strengthened by Mn-Nb-Cr and trace amounts of Ti. However, the finish rolling temperature needs to be controlled below 950℃ for low-temperature rolling, so the intermediate blank may need a longer steel waiting time, which has a greater impact on the production rhythm. In addition, the yield strength Rt0.5 of the product is between 500-524MPa, and the strength margin is not large, so there is a high risk that the yield strength of the steel pipe will be insufficient below the lower limit of 585MPa after pipe making. CN116970870A discloses a low-yield ratio X70 grade pipeline steel hot-rolled plate and a manufacturing method thereof. Although this patent can control the yield ratio to ≤0.85, it is achieved by adding Mo and Ni and other valuable alloying elements, which has a high alloy cost, and the product has relatively poor market competitiveness and economic benefits. CN111321354B discloses an X70M hot-rolled steel strip and a manufacturing method thereof. The patent has a-60℃ ultra-low temperature impact resistance, but also adds a high content of Mo element, resulting in a high alloy cost. SUMMARY

[0004] To address the aforementioned technical problems, this invention develops a hot continuous rolling production method for Mo- and Ni-free X70M pipeline steel. This hot-rolled pipeline steel strip does not contain the precious alloying elements Mo and Ni, resulting in extremely low alloy costs. Simultaneously, the hot-rolled pipeline steel strip exhibits excellent low-temperature tear resistance and a low yield strength ratio, ensuring the safety of the pipeline during service.

[0005] To achieve the above-mentioned objectives, the present invention adopts the following technical solution: A hot continuous rolling production method for Mo- and Ni-free X70M pipeline steel includes slab heating, rough rolling, finish rolling, laminar flow cooling, and coiling processes. The chemical composition and mass percentage of pipeline steel are as follows: C: 0.060-0.090%, Si: 0.10-0.25%, Mn: 1.50-1.70%, Cr: 0.20-0.30%, Nb: 0.045-0.070%, Al: 0.020-0.050%, S≤0.005%, P≤0.012%, Ti: 0.020-0.030%, N≤0.0050%, with the balance being Fe and unavoidable impurities.

[0006] Furthermore, in the slab heating process, a step heating method is adopted, with the temperature of the second heating section being 1150-1200℃, the temperature of the third heating section being 1170-1250℃, and the temperature of the soaking section being 1170-1230℃. Furthermore, in the roughing process, a two-stand roughing mill is adopted, with a rolling pass distribution pattern of 3+5, an intermediate billet thickness of 45-60mm, full-pass descaling, and a short-term 10-40s temperature control before the last pass to meet the finishing mill inlet temperature requirements. Furthermore, in the finishing rolling process, 7 passes of finishing rolling are adopted, with a finishing rolling inlet temperature ≤980℃ and a finishing rolling temperature of 800-840℃; Furthermore, in the laminar flow cooling process, centralized front-end cooling is adopted, and the laminar flow cooling rate is 18-25℃ / s; Furthermore, in the winding process, the winding temperature is 350-440℃.

[0007] Furthermore, in the slab heating process, the total time of the three heating sections and the soaking section is ≥85min, and the total furnace dwell time is 210-330min.

[0008] Furthermore, the microstructure of the hot-rolled steel strip for pipelines consists of acicular ferrite and a small amount of Mao islands. Acicular ferrite is the main matrix, and a small amount of fine Mao islands are evenly distributed on the matrix, with an average size of less than 1.5 μm.

[0009] Further, the pipeline steel hot-rolled steel strip has yield strength of 515-580 MPa, tensile strength of 630-740 MPa, elongation A 50 ≥ 35%, yield strength / tensile strength ratio ≤ 0.80, impact energy at -20 DEG C ≥ 300 J, and falling weight shear area at -30 DEG C ≥ 90%.

[0010] Further, the pipeline steel hot-rolled steel strip has thickness of 8-18 mm.

[0011] The main alloying element roles and action mechanisms in the Mo-free and Ni X70M pipeline steel are as follows: C: Carbon is the most significant and economical strengthening element in steel, which can not only play a solid solution strengthening role, but also can play a significant precipitation strengthening role in combination with Nb, Ti and other micro-alloying elements, and a certain carbon content in the steel can accelerate the transformation of acicular ferrite or martensite island in the accelerated cooling process, further promote the phase transformation strengthening effect, and is beneficial to reduce the yield ratio of the steel, so as to ensure that the steel strip of the application can reach the X70M level, the carbon content should not be less than 0.060%, otherwise the content of acicular ferrite or martensite island in the steel is insufficient, which can lead to the decrease of tensile strength and finally lead to the increase of yield ratio of the steel; but the carbon content should not be too high, otherwise the plasticity and toughness of the steel will be significantly reduced, which can affect the low temperature impact performance, falling weight tear performance and welding performance, so the carbon content should be controlled between 0.060-0.090%.

[0012] Si: In the application, silicon element can play a solid solution strengthening role, which is easy to be dissolved in ferrite, improve the strength of ferrite matrix, and can compensate for the decrease of yield strength caused by not adding Mo and Ni elements to a certain extent, but the silicon element should not be added too high, otherwise it will affect the surface quality of the steel strip and is not conducive to the toughness of the steel, so the silicon content should be controlled between 0.10-0.25%.

[0013] Mn: In the steel, manganese element can play a significant solid solution strengthening role in the steel, which can improve the hardenability of the steel, promote the formation of acicular ferrite or martensite island, and is beneficial to reduce the yield ratio of the steel, and in a certain range, the impact toughness of the steel will not decrease significantly while the strength is improved, so the manganese content in the application is controlled between 1.50-1.70%.

[0014] Cr: Chromium is an important alloying element in steel, which can significantly improve the hardenability of the steel, inhibit the precipitation of pearlite, promote the formation of bainite and martensite structure, and form fine carbides with carbon, which is beneficial to improve the strength of the steel and reduce the yield ratio of the steel. On the other hand, the addition of chromium in the steel can also improve the compactness of the surface iron oxide skin and improve the structure of the iron oxide skin, so the chromium content is controlled between 0.20-0.30% Nb: In the present application, a certain content of niobium element is added, on the one hand, in combination with C and N, fine dispersed Nb(C, N) is formed, which plays a strong precipitation strengthening role, and can significantly inhibit the growth of austenite grains; on the other hand, the niobium dissolved in the steel can significantly improve the recrystallization temperature of austenite, which is beneficial to retain more deformation storage energy in the steel during finish rolling, provide more nucleation sites for subsequent cooling transformation, promote the refinement of microstructure, and improve the low temperature crack arrest performance of the steel. However, the niobium element should not be controlled too high, otherwise it is easy to cause the grain to be too refined, and the yield strength ratio of the steel to increase. Therefore, the niobium element is controlled at 0.045%-0.070%.

[0015] In the hot continuous rolling production method of Mo-free, Ni X70M pipeline steel in the present application, the process condition design reasons are as follows: In the present application, the low temperature tear resistance of the steel is realized by low temperature rolling and low temperature coiling. Low temperature rolling can realize the rolling of the steel in the non-recrystallization zone, which can make the austenite flatten to the maximum extent, provide storage energy and nucleation sites for subsequent phase transformation, and promote the refinement of the final structure. Therefore, it is required to control the finish rolling inlet temperature below 980℃ by short-time swing steel; and under the mode of low temperature coiling and front concentrated cooling, the overall cooling speed of the steel is large, and the proeutectoid ferrite and pearlite precipitation can be reduced, and the formation of acicular ferrite is promoted, thereby improving the low temperature tear resistance of the steel. Therefore, the coiling temperature is controlled in the range of 350-440℃.

[0016] In the present application, the low yield ratio of the steel is realized by a certain C content, and on the other hand, at a lower coiling temperature, the proeutectoid ferrite and pearlite precipitation can be significantly inhibited, the formation of acicular ferrite and martensite-austenite island and other low temperature hard phase structures is promoted, which is beneficial to improve the tensile strength of the steel, thereby reducing the yield ratio of the steel.

[0017] The beneficial effects produced by the above composition and technical scheme are as follows: Under the composition system without adding Mo and Ni precious alloy elements, the alloy cost of the steel is significantly reduced; by using lower rolling temperature and coiling temperature, the overall organization of the steel is refined, the proeutectoid ferrite and pearlite organization which is not conducive to the low temperature tear resistance performance is avoided, and the steel can meet the anti-tear performance under the condition of-30℃ low temperature. On the other hand, by using appropriate C content and low temperature coiling process, the acicular ferrite phase transformation and the formation of certain martensite-austenite island structure are promoted, the tensile strength of the steel is improved, the lower yield ratio is realized, and the safety of the pipeline in the service process can be guaranteed. BRIEF DESCRIPTION OF DRAWINGS

[0018] Figure 1 The OM photo of the steel strip produced in Example 1; Figure 2SEM photos of the steel strip produced in Example 1 were taken. DETAILED DESCRIPTION

[0019] The application will be further described in detail below in conjunction with the specific embodiments.

[0020] A hot continuous rolling production method of Mo-free and Ni X70M pipeline steel, comprising slab heating, rough rolling, finish rolling, laminar cooling and coiling processes; the chemical composition and mass percentage of the pipeline steel are as follows: C: 0.060-0.090%, Si: 0.10-0.25%, Mn: 1.50-1.70%, Cr: 0.20-0.30%, Nb: 0.045-0.070%, Al: 0.020-0.050%, S≤0.005%, P≤0.012%, Ti: 0.020-0.030%, N≤0.0050%, and the balance of Fe and inevitable impurities.

[0021] In the slab heating process, step-by-step heating is adopted, the temperature of the second heating section is 1150-1200℃, the temperature of the third heating section is 1170-1250℃, and the temperature of the soaking section is 1170-1230℃; the total time of the third heating section and the soaking section is ≥85min, and the total residence time is 210-330min.

[0022] In the rough rolling process, two-stand rough rolling is adopted, the rolling pass distribution mode is 3+5, the intermediate blank thickness is 45-60mm, the full pass descaling is started, and the temperature is controlled by short-time steel swinging 10-40s before the last pass to meet the finish rolling inlet temperature requirement; In the finish rolling process, seven-pass finish rolling is adopted, the finish rolling inlet temperature is ≤980℃, and the finish rolling temperature is 800-840℃; In the laminar cooling process, concentrated cooling is adopted in the front section, and the laminar cooling cooling rate is 18-25℃ / s; In the coiling process, the coiling temperature is 350-440℃.

[0023] The thickness specification of the pipeline steel hot-rolled steel strip is 8-18mm.

[0024] The chemical composition of the pipeline steel hot-rolled steel strip in Examples 1-6 is shown in Table 1, the rolling parameters are shown in Table 2, and the physical properties are shown in Table 3.

[0025] Table 1 Chemical composition and mass percentage of the steel strip in Examples 1-6 (%)

[0026] Table 2 Rolling parameters of the steel strip in Examples 1-6

[0027] Table 3 Physical properties of steel strips of Examples 1-6

[0028] The steel strip produced in Example 1 was analyzed for morphology by optical microscopy (OM) and scanning electron microscopy (SEM), as shown in Figs. 1 and 2, respectively. Figure 1 Figure 2 As can be seen from Fig. 1, the microstructure of the steel strip of Example 1 is mainly acicular ferrite as matrix, with a small amount of fine-sized M / A island structure dispersed and uniformly distributed on the matrix. Figure 1 As can be seen from Fig. 2, the average size of the M / A island structure in the steel strip is below 1.5 μm. Figure 2

[0029] As can be seen from Table 3, the yield strength of the hot-rolled steel strip of the pipeline steel of the present application is 515-580 MPa, the tensile strength is 630-740 MPa, the elongation A 50 ≥ 35%, the yield strength ratio is ≤ 0.80, the impact energy at -20°C is ≥ 300 J, and the falling weight shear area at -30°C is ≥ 90%, with excellent low-temperature tear resistance and low yield strength ratio, which can ensure the operational safety of the pipeline during service.

[0030] The above description is only preferred embodiments of the present application, and it should be pointed out that, for those skilled in the art, several improvements and refinements can be made without departing from the principles of the present application, and these improvements and refinements should also be considered as falling within the scope of the present application.​​

Claims

1. A hot continuous rolling production method for Mo- and Ni-free X70M pipeline steel, characterized in that, This includes slab heating, rough rolling, finish rolling, laminar flow cooling, and coiling processes; The chemical composition and mass percentage of the pipeline steel are as follows: C: 0.060-0.090%, Si: 0.10-0.25%, Mn: 1.50-1.70%, Cr: 0.20-0.30%, Nb: 0.045-0.070%, Al: 0.020-0.050%, S≤0.005%, P≤0.012%, Ti: 0.020-0.030%, N≤0.0050%, with the balance being Fe and unavoidable impurities.

2. The hot continuous rolling production method for Mo- and Ni-free X70M pipeline steel according to claim 1, characterized in that, In the slab heating process, a step heating method is adopted, with the temperature of the second heating section being 1150-1200℃, the temperature of the third heating section being 1170-1250℃, and the temperature of the soaking section being 1170-1230℃. In the roughing process, a two-stand roughing mill is used, with a rolling pass distribution pattern of 3+5, an intermediate billet thickness of 45-60mm, full-pass descaling, and a short-term 10-40s temperature control before the last pass to meet the finishing mill inlet temperature requirements. In the aforementioned finishing rolling process, 7 passes of finishing rolling are adopted, with a finishing rolling inlet temperature ≤980℃ and a final rolling temperature of 800-840℃; In the laminar flow cooling process, front-end centralized cooling is adopted, and the laminar flow cooling rate is 18-25℃ / s; In the winding process, the winding temperature is 350-440℃.

3. The hot continuous rolling production method for Mo- and Ni-free X70M pipeline steel according to claim 2, characterized in that, In the slab heating process, the total time of the three heating sections and the soaking section is ≥85min, and the total furnace dwell time is 210-330min.

4. The hot continuous rolling production method for Mo- and Ni-free X70M pipeline steel according to claim 1, characterized in that, The microstructure of the hot-rolled steel strip for pipeline steel consists of acicular ferrite and a small amount of Mao islands.

5. The hot continuous rolling production method for Mo- and Ni-free X70M pipeline steel according to claim 4, characterized in that, The average size of the Mao Island is less than 1.5 μm.

6. The hot continuous rolling production method for Mo- and Ni-free X70M pipeline steel according to claim 1, characterized in that, The hot-rolled steel strip for the pipeline has a yield strength of 515-580 MPa, a tensile strength of 630-740 MPa, and an elongation of A. 50 ≥35%, yield strength ratio ≤0.80, impact energy at -20℃ ≥300J, drop shear area at -30℃ ≥90%.

7. The hot continuous rolling production method for Mo- and Ni-free X70M pipeline steel according to claim 1, characterized in that, The thickness of the hot-rolled steel strip for pipelines is 8-18mm.

Citation Information

Patent Citations

  • An X70M hot-rolled steel strip and its manufacturing method

    CN111321354B

  • Low-yield-ratio X70-grade pipeline steel hot-rolled coiled plate and manufacturing method thereof

    CN116970870A

  • Low-cost X70-grade high-strength pipeline steel plate coil and production method thereof

    CN117467891A

Cited By

  • Low-cost thick-specification high-toughness X70 pipeline steel and production method thereof

    CN122128630A