Method for manufacturing magnetic recording medium

By combining spin coating with ultraviolet or heat treatment, the problem of foreign matter residue after polishing of the lubricating layer is solved, achieving efficient lubricating layer formation and improving the surface coverage and corrosion resistance of magnetic recording media.

CN121641085APending Publication Date: 2026-03-10LISSENNOCO HARD DRIVE CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202511207826.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-08-30
Filing Date
2025-08-27
Publication Date
2026-03-10

AI Technical Summary

Technical Problem

In the current manufacturing process of magnetic recording media, the polishing process of the lubricating layer leads to a decrease in lubricity, and solvent washing is difficult to completely remove the lubricant, resulting in foreign matter residue, which affects the surface coverage of the magnetic recording media and the complexity of the manufacturing process.

Method used

A high molecular weight, high polarity first lubricant and a low molecular weight, low polarity or non-polarity second lubricant are coated by spin coating. The second lubricant is removed by ultraviolet irradiation or heat treatment to form a lubricating layer with high coverage.

Benefits of technology

It effectively removes foreign matter from the surface of magnetic recording media, improves the coverage of the lubricating layer, simplifies the manufacturing process, and enhances the corrosion resistance and recording density of magnetic recording media.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121641085A_ABST
    Figure CN121641085A_ABST
Patent Text Reader

Abstract

The method for manufacturing the magnetic recording medium can efficiently remove foreign matters on the surface of the magnetic recording medium, and the coating rate of a lubricating layer is high. A method for manufacturing a magnetic recording medium in which a lubricating layer is formed on a laminate in which a magnetic recording layer and a protective layer are sequentially laminated on a substrate, the method comprising: a step for applying a first lubricant and a second lubricant on the laminate, the present invention relates to a method for polishing a laminate comprising a first lubricant and a second lubricant, a step for polishing the surface of the laminate coated with the first lubricant and the second lubricant with a polishing material, and a step for removing the second lubricant from the laminate, the second lubricant being applied by a spin coating method, the polishing step comprising: a step for pressing and rubbing a tape containing the polishing material against the surface of the laminate; the step for removing the second lubricant includes at least one of a step for irradiating the laminate coated with the first lubricant and the second lubricant with ultraviolet light and a step for heating the laminate coated with the first lubricant and the second lubricant.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present application relates to a manufacturing method of a magnetic recording medium. BACKGROUND

[0002] In recent years, magnetic storage devices are mounted on various products such as personal computers, moving image recorders, and data servers, and their importance is increasing. The magnetic storage device is a device having a magnetic recording medium that stores electronic data by magnetic recording, and for example, has a hard disk drive (HDD).

[0003] A general magnetic recording medium has a multilayer film laminated structure in which a base layer, an intermediate layer, a magnetic recording layer, and a protective layer are sequentially formed on a non-magnetic substrate, and a lubricating layer is coated on the surface of the protective layer. The protective layer and the lubricating layer are provided to prevent the durability from deteriorating due to wear damage caused by contact sliding of the magnetic recording medium with a magnetic head. As the protective layer, a hard carbon film is generally used, and the lubricating layer is formed by coating a liquid perfluoropolyether compound or the like on the surface.

[0004] To improve the adhesion of the protective layer to the lubricating layer, various treatments for the lubricating layer are known. For example, in Patent Literature 1, a method is disclosed in which a heat treatment is applied to the coated lubricating layer, and further, a light irradiation treatment using an ultraviolet lamp is performed.

[0005] Further, to remove foreign matter and protrusions on the surface of the protective layer, the surface of the magnetic recording medium is belt polished by a polishing belt. At this time, to prevent the surface of the protective layer from being damaged by belt polishing, it is known that the belt polishing is performed after the formation of the lubricating layer.

[0006] Further, in Patent Literature 2, a manufacturing method of a magnetic recording medium is disclosed in which, after the formation of the protective layer, a first lubricant having no terminal group is coated on the surface thereof, and after the belt polishing, the first lubricant is removed using a solvent, and a second lubricant having a terminal group is coated.

[0007] PRIOR ART DOCUMENTS

[0008] PATENT LITERATURE

[0009] Patent Literature 1: Japanese Patent Application Laid-Open No. 11-25452

[0010] Patent Literature 2: Japanese Patent Application Laid-Open No. 2002-222519 SUMMARY

[0011] PROBLEMS TO BE SOLVED BY THE INVENTION

[0012] In the production of a magnetic recording medium, polishing is performed after the formation of a lubricating layer, so that the occurrence of scratches and the like is reduced by the lubricity of the lubricating layer. However, depending on the lubricant used for the lubricating layer and the film thickness of the lubricating layer, polishing is not always suitable.

[0013] In the production method of the magnetic recording medium of Patent Document 2, after processing using a first lubricant suitable for polishing, the first lubricant is removed, and a second lubricating layer suitable for the magnetic recording medium is applied. However, in this case, the following problems arise. That is, contaminants dissolved in a solvent used for the removal of the lubricant and the like adhere again to the processed substrate, and become a cause of foreign matter on the surface of the magnetic recording medium. Furthermore, it is difficult to completely remove the lubricant combined with the protective layer using a solvent, and the remaining solvent becomes a cause of foreign matter on the surface of the magnetic recording medium, and the manufacturing process of the magnetic recording medium becomes complicated while the coverage of the surface of the magnetic recording medium using the lubricating layer is reduced.

[0014] One embodiment of the present application is made in view of the above-described circumstances, and aims to provide a production method of a magnetic recording medium capable of efficiently removing foreign matter from the surface of the magnetic recording medium, and having a high coverage using a lubricating layer.

[0015] Method for solving the problem

[0016] The present application has the configuration shown below.

[0017] [1] A production method of a magnetic recording medium, which is a production method of a magnetic recording medium in which a lubricating layer is formed on a laminate in which a magnetic recording layer and a protective layer are sequentially stacked on a substrate, the production method comprising:

[0018] a step of applying a first lubricant and a second lubricant on the laminate,

[0019] a step of polishing the surface of the laminate on which the first lubricant and the second lubricant are applied by an abrasive,

[0020] a step of removing the second lubricant on the laminate,

[0021] the application of the second lubricant uses a spin coating method,

[0022] the step of polishing includes a step of pressing a belt including the abrasive against the surface of the laminate and rubbing it,

[0023] the step of removing the second lubricant includes at least one of a step of irradiating ultraviolet light on the laminate on which the first lubricant and the second lubricant are applied and a step of performing a heat treatment on the laminate on which the first lubricant and the second lubricant are applied.

[0024] [2] The production method of the magnetic recording medium according to [1], wherein the average molecular weight of the first lubricant is higher than the average molecular weight of the second lubricant,

[0025] the polarity of the first lubricant is higher than the polarity of the second lubricant.

[0026] [3] The production method of the magnetic recording medium according to [1] or [2], wherein the average molecular weight of the second lubricant is 300 to 1000, and the number of polar groups is 2 or less, or the second lubricant does not have a polar group.

[0027] [4] The production method of the magnetic recording medium according to any one of [1] to [3], wherein the average molecular weight of the first lubricant is 900 to 3000, and the number of polar groups is in the range of 4 to 8.

[0028] [5] The production method of the magnetic recording medium according to any one of [1] to [4], wherein the film thickness of the first lubricant applied to the laminate is

[0029] the film thickness of the second lubricant is

[0030] [6] The production method of the magnetic recording medium according to any one of [1] to [5], wherein the step of irradiating the ultraviolet rays is performed in a non-reactive gas atmosphere or in a vacuum.

[0031] [7] The production method of the magnetic recording medium according to any one of [1] to [6], wherein the step of the heat treatment is performed in a non-reactive gas atmosphere.

[0032] Effects of the Invention

[0033] According to one embodiment of the present application, foreign matter on the surface of a magnetic recording medium can be efficiently removed, and the coverage with a lubricating layer can be improved. BRIEF DESCRIPTION OF DRAWINGS

[0034] Figure 1 is a cross-sectional view showing an example of a magnetic recording medium produced by the production method of the magnetic recording medium according to the embodiment of the present application.

[0035] Figure 2 is a view showing an example of an outline of the production method of the magnetic recording medium according to the embodiment of the present application.

[0036] Figure 3A is a view showing an example of a lubricant application device using a dipping method, and shows a state in which the laminate 11 is dipped in the solution 52.

[0037] Figure 3BThe diagram illustrating an example of a lubricant coating apparatus using the immersion method shows the state in which the laminate 11 is lifted from the solution 52.

[0038] Figure 4 A diagram illustrating an example of a lubricant coating apparatus using a spin coating method.

[0039] Figure 5 A diagram illustrating an example of a lubricant coating apparatus using a steam method.

[0040] Figure 6 An enlarged cross-sectional view showing an example of a belt containing abrasive material used during polishing.

[0041] Figure 7 This figure shows an example of a polishing apparatus used in the process of polishing the surface of a laminate with an abrasive material. Detailed Implementation

[0042] Hereinafter, embodiments of the present invention will be described in detail with reference to the accompanying drawings. Furthermore, for ease of understanding, the same symbols are used to denote the same constituent elements in each drawing, and repetitive descriptions are omitted where appropriate. Additionally, the scale of each component in the drawings may sometimes differ from the actual scale. In this specification, the tilde “~” indicating a numerical range means that, unless otherwise stated, the values ​​described before and after it include both the lower and upper limits. In a numerical range indicated by “~”, where only the unit of the upper limit is described, the lower limit is also described in the same unit.

[0043] The following describes a method for manufacturing a magnetic recording medium according to an embodiment of the present invention. A magnetic recording medium manufactured using the method described in this embodiment will also be explained.

[0044] <Magnetic Recording Media>

[0045] Figure 1 This is a cross-sectional view showing an example of a magnetic recording medium manufactured by the manufacturing method of the magnetic recording medium according to this embodiment. Figure 1 As shown, the magnetic recording medium 1 has a lubricating layer 12 on both sides of the laminate (also called the laminated body) 11.

[0046] The laminate 11 is stacked on both sides of the substrate 111, and has a magnetic recording layer 112 and a protective layer 113 stacked sequentially from the substrate 111 side.

[0047] The substrate 111 is formed of a non-magnetic material. For example, the substrate 111 can be a metal substrate formed of a metallic material such as aluminum alloy, or a non-metallic substrate formed of a non-metallic material such as glass. Furthermore, the surface of these metal or non-metallic substrates can be formed with a NiP alloy layer, for example, using a plating or sputtering method.

[0048] The magnetic recording layer 112 is a layer provided for recording and reproducing information, for example, by using magnetic energy supplied by the magnetic head of the HDD to reverse the direction of magnetization and maintain its magnetized state, thereby being provided for storing data.

[0049] The magnetic recording layer 112 uses FePt alloys with an L10 structure, CoPt alloys with an L10 structure, and CoCrPt alloys with an hcp structure, etc.

[0050] In the formation of the magnetic recording layer 112, known methods such as sputtering and ion beam deposition can be used.

[0051] The protective layer 113 is provided to inhibit the corrosion of the magnetic recording layer 112 and to protect the surface of the magnetic recording medium 1 from damage when the magnetic head contacts the magnetic recording medium 1, thereby improving the corrosion resistance of the magnetic recording medium 1.

[0052] The protective layer 113 can be formed from known materials, such as hard carbon film or diamond-like carbon (DLC).

[0053] In the formation of the protective layer 113, known methods such as sputtering and ion beam deposition can be used.

[0054] The protective layer 113 can be hydrogenated or nitrided. Hydrogenating or nitriding the surface of the protective layer 113 improves its adhesion to the lubricating layer 12 formed thereon. Specifically, the first lubricant applied to the protective layer 113 is polar, thus forming a strong bond between the hydrogen and nitrogen atoms on the surface of the protective layer 113. In particular, nitriding is preferably performed on the surface of the protective layer 113.

[0055] The lubricating layer 12 is provided to suppress the wear of the magnetic head and the surface of the magnetic recording medium 1 when the magnetic head comes into contact with the magnetic recording medium 1, and to improve the corrosion resistance of the magnetic recording medium 1.

[0056] The thickness of the lubricating layer 12 is preferably... The thickness of lubrication layer 12 is This allows for the suppression of surface wear of the magnetic recording medium 1, improvement of its corrosion resistance, and shortening of the distance between the magnetic head and the magnetic recording medium 1 in the HDD, thereby achieving high recording density.

[0057] In addition, in this embodiment, the magnetic recording medium 1 may have one or more of the following between the substrate 111 and the magnetic recording layer 112: an adhesive layer, a soft magnetic substrate layer, a seed layer, and an orientation control layer. More than one of these layers may be stacked.

[0058] In this embodiment, the magnetic recording medium 1 may be stacked to include multiple magnetic recording layers 112. At this time, non-magnetic recording layers may be stacked on top of each other among the magnetic recording layers 112.

[0059] <Methods for Manufacturing Magnetic Recording Media>

[0060] An example of a summary of the method for manufacturing a magnetic recording medium according to this embodiment is shown in Figure 2 . Figure 2 As shown, the method for manufacturing a magnetic recording medium according to this embodiment includes: a process of forming a laminate 11 on both sides of a substrate 111 by sequentially stacking a magnetic recording layer 112 and a protective layer 113 (laminate formation process); a process of coating a first lubricant 121 and a second lubricant 122 onto the laminate 11 (coating process); a process of polishing the surface of the laminate 11 coated with the first lubricant 121 and the second lubricant 122 using an abrasive material (polishing process); and a process of removing the second lubricant 122 from the laminate 11 (see reference). Figure 2 The coating process includes a spin coating method for applying the second lubricant, a polishing process including a process of pressing a strip containing abrasive material onto the surface of the laminate and rubbing it (rubbing process), and a removal process including at least one of a process of irradiating the laminate coated with the first lubricant and the second lubricant with ultraviolet light (ultraviolet irradiation process) and a process of heat-treating the laminate coated with the first lubricant and the second lubricant (heat treatment process).

[0061] Furthermore, the method for manufacturing the magnetic recording medium according to this embodiment may include other steps such as forming an adhesive layer, a soft magnetic substrate layer, a seed layer, or an orientation control layer between the substrate 111 and the magnetic recording layer 112. Additionally, when the method for manufacturing the magnetic recording medium according to this embodiment includes multiple magnetic recording layers 112 stacked together, it may include steps such as forming non-magnetic recording layers between the magnetic recording layers 112.

[0062] The method for manufacturing a magnetic recording medium according to this embodiment involves coating the surface of a laminate 11 with a first lubricant 121 and a second lubricant 122, and then polishing the surface of the laminate 11 with an abrasive. Then, the second lubricant 122 on the laminate 11 is removed by applying an ultraviolet irradiation treatment 31 or a heat treatment 32. As a result, the first lubricant 121 remains on the surface of the protective layer 113 of the laminate 11, and the remaining first lubricant 121 becomes the lubricating layer 12 of the magnetic recording medium 1, forming the lubricating layer 12.

[0063] In this embodiment, the removal of the second lubricant 122 is performed using ultraviolet irradiation treatment 31 or heat treatment 32. As described above, the lubricant used in the polishing process is removed by conventional solvent washing. However, according to the research of the inventors, in addition to the removed lubricant, contaminants generated during polishing are also dissolved in the solvent used for washing, and this solvent temporarily remains on the surface of the protective layer 113, which is the surface being washed. It is known that these residual contaminants and lubricant re-adhere to the protective layer 113, becoming foreign matter on the surface of the magnetic recording medium 1. Furthermore, it is difficult to completely remove the lubricant bonded to the protective layer 113 by solvent washing, and it is known that slightly residual lubricant becomes a cause of foreign matter on the surface of the magnetic recording medium 1.

[0064] In this embodiment, the removal of the second lubricant 122 on the laminate 11 is performed using a dry treatment of ultraviolet irradiation 31 or heat treatment 32. Therefore, the second lubricant 122, or any contaminants dissolved therein, rapidly vaporizes and leaves the surface of the laminate 11, thus preventing them from becoming foreign matter on the surface of the magnetic recording medium 1. Furthermore, the conditions of ultraviolet irradiation 31 or heat treatment 32 are such that the second lubricant 122 can be vaporized, thereby completely removing the second lubricant 122 from the laminate 11. In addition, the formation process of the lubricating layer 12 is simple, thus providing a highly productive method for manufacturing magnetic recording media.

[0065] [Laminated body formation process]

[0066] In the method for manufacturing a magnetic recording medium according to this embodiment, firstly, in Figure 1 A laminate 11 is formed on both sides of a substrate 111 prepared as shown, wherein a magnetic recording layer 112 and a protective layer 113 are sequentially stacked (laminate formation process).

[0067] The laminate 11 can be formed using conventional film-forming methods for the magnetic recording layer 112 and the protective layer 113.

[0068] First, magnetic recording layers 112 are formed on both sides of the substrate 111. As a method for forming the magnetic recording layers 112, general film formation methods such as sputtering can be used.

[0069] In sputtering, a target containing a material that forms the magnetic recording layer 112 can be used.

[0070] As a target for the material comprising the magnetic recording layer 112, for example, FePt alloys with an L10 structure, CoPt alloys with an L10 structure, CoCrPt alloys with an hcp structure, etc., can be used.

[0071] As a sputtering method, DC sputtering, DC magnetron sputtering, and RF sputtering can be used.

[0072] When forming the magnetic recording layer 112, RF (Radio Frequency) bias, DC bias, pulsed DC bias, and pulsed DC bias can be used as needed.

[0073] As reactive gases, O2, H2O, N2, etc. can be used.

[0074] The sputtering gas pressure is adjusted appropriately to optimize the properties of each layer, typically within the range of 0.1 Pa to 30 Pa.

[0075] Next, a protective layer 113 is formed on the magnetic recording layer 112. The method for forming the protective layer 113 is not particularly limited; for example, it can be formed using RF-CVD (Radio Frequency-Chemical Vapor Deposition), which decomposes a hydrocarbon-containing feed gas using high-frequency plasma; IBD (Ion Beam Deposition), which ionizes the feed gas using electrons emitted from a filament and forms a film; or FCVA (Filtered Cathodic Vacuum Arc), which forms a film using a solid carbon target without a feed gas.

[0076] [Coating Process]

[0077] Next, Figure 2 As shown, a first lubricant 121 and a second lubricant 122 are sequentially applied to both sides of the laminate 11 (coating process).

[0078] Furthermore, the two sides of the laminate 11 refer to the two main surfaces of the laminate 11 coated with the first lubricant 121 and the second lubricant 122. The first lubricant 121 and the second lubricant 122 can be applied to the other main surface of the laminate 11 after being applied to one main surface, or they can be applied to both main surfaces of the laminate 11 simultaneously.

[0079] When the first lubricant 121 is applied to the protective layer 113, ideally, the entire protective layer 113 is covered by the first lubricant 121, but a portion of the surface of the protective layer 113 may remain uncoated. In this case, the second lubricant 122 may be applied to the areas not covered by the first lubricant 121.

[0080] Preferably, the average molecular weight of the first lubricant 121 is higher than that of the second lubricant 122, and the polarity of the first lubricant 121 is higher than that of the second lubricant 122. Therefore, when the laminate 11 is subjected to ultraviolet irradiation treatment 31 or heat treatment 32 in the removal process described later, it is easier to retain the first lubricant 121 in the laminate 11 while simultaneously removing the second lubricant 122 from the laminate 11.

[0081] The organic compounds used as the first lubricant 121 and the second lubricant 122 include functional groups such as hydroxyl, amino, amide, carbonyl, carboxyl, cyano, phenyl, and methyl. Among these, the functional groups (polar groups) that are polar include hydroxyl, amino, amide, carbonyl, carboxyl, and cyano.

[0082] Preferably, the average molecular weight of the first lubricant 121 is 900 to 3000, and the structural formula of the first lubricant 121 contains 4 to 8 polar groups. Therefore, in the removal process described later, when the second lubricant 122 is removed by ultraviolet irradiation treatment 31 or heat treatment 32, the first lubricant 121 can be removed without vaporization, and the selection of ultraviolet irradiation treatment 31 and heat treatment 32 to vaporize the second lubricant 122 can be easily performed.

[0083] Preferably, the average molecular weight of the second lubricant 122 is 300 to 1000, and the structural formula of the second lubricant 122 contains two or fewer polar groups, or contains no polar groups. Therefore, in the removal process described later, when the second lubricant 122 is removed by ultraviolet irradiation treatment 31 or heat treatment 32, the first lubricant 121 can be prevented from vaporizing, and the selection of ultraviolet irradiation treatment 31 and heat treatment 32 to vaporize the second lubricant 122 can be easily performed.

[0084] The polar groups of the first lubricant 121 and the second lubricant 122 are preferably hydroxyl, amide, or cyano groups, with hydroxyl being particularly preferred. By having the aforementioned preferred polar groups, the first lubricant 121 can be applied to the lubrication layer 12 of the magnetic recording medium 1, and the second lubricant 122 can be suitable for polishing the surface of the laminate 11. Furthermore, during the aforementioned ultraviolet irradiation treatment 31 or heat treatment 32, the effect of rapidly removing contaminants dissolved in the second lubricant 122 is improved. In addition, by leaving the first lubricant 121 on the laminate 11, the adhesion between the protective layer 113 and the first lubricant 121 can be improved, thereby further reducing surface foreign matter and further improving the coverage of the magnetic recording medium 1 utilizing the lubrication layer 12.

[0085] The first lubricant 121 forms a lubricating layer 12 of the magnetic recording medium 1. Therefore, the film thickness of the first lubricant 121 is... This is preferable in terms of suppressing surface wear of the magnetic recording medium 1, improving the corrosion resistance of the magnetic recording medium 1, shortening the distance between the magnetic head and the magnetic recording medium 1 in the HDD, and achieving high recording density.

[0086] The preferred film thickness of the second lubricant 122 is... If the film thickness of the second lubricant 122 is 5~ This allows for the polishing of the surface of the laminate 11. Furthermore, the removal of the second lubricant 122 by ultraviolet irradiation treatment 31 or heat treatment 32 can be performed in a short time, thereby improving the productivity of the magnetic recording medium 1.

[0087] In the application of the first lubricant 121, known methods such as impregnation, spin coating, and steam coating can be used.

[0088] The impregnation method involves impregnating the laminate 11 in a liquid containing a lubricant, then lifting the laminate 11 at a certain speed to form a film of the first lubricant 121 on the surface of the laminate 11. The spin coating method involves coating the laminate 11 with a liquid containing a lubricant, then rotating the laminate 11 at high speed for a certain period to form a film of the first lubricant 121 on the laminate 11. The vapor method involves placing the laminate 11 in a vacuum container, introducing a lubricant that has been heated and vaporized into the vacuum container, thereby forming a film of the first lubricant 121 on the laminate 11.

[0089] use Figure 3A and Figure 3B This is an example illustrating the formation of a film of the first lubricant 121 using the impregnation method.

[0090] Figure 3A As shown, a solution 52 containing the first lubricant 121 is added to a solution tank 51. The arm 53, to which the laminate 11 is fixed, is lowered vertically at a certain speed in the solution 52, immersing the laminate 200 in the solution 52. Then, the arm 53 is raised vertically at a certain speed, placing... Figure 3B The state shown allows a film of the first lubricant 121 to be formed on the surface of the laminate 11. Here, the laminate 11 is held in the arm 53 such that its inner periphery is engaged with a V-shaped groove provided in the arm 53. The arm 53 is mounted in a manner that allows it to move vertically relative to the support column 54. The film thickness of the first lubricant 121 can be controlled by the lifting speed of the arm 53.

[0091] use Figure 4 This illustrates an example of the formation of a film of the first lubricant 121 using a spin coating method. The lubricant coating apparatus 60 using the spin coating method is as follows: Figure 4As shown, a solution containing lubricant is prepared in tank 61. After the solution is sprayed from nozzle 63 onto both surfaces of the laminate 11 held by spindle 62, the laminate 11 is rotated at high speed for a certain period by motor 64, thereby forming a film of the first lubricant 121 on the laminate 11 through centrifugal force. Excess solution is discharged from drain 65 to the outside of the device. The thickness of the first lubricant 121 film can be controlled by the rotational speed of spindle 62.

[0092] use Figure 5 This illustrates an example of the formation of a film of the first lubricant 121 using a steam method. The lubricant coating apparatus 70 using a steam method is as follows: Figure 5 As shown, after the laminate 11 is placed on the mounting stage 72 inside the processing chamber 71, the processing chamber 71 is evacuated using a vacuum pump 73. Then, a lubricant 74, which is vaporized by heating, is introduced into the processing chamber 71, thereby forming a lubricant film on the laminate 11. The processing chamber 71 is then evacuated, and the pressure inside the processing chamber 71 is brought to atmospheric pressure before the processed substrate is removed from the processing chamber 71. The thickness of the first lubricant 121 film can be controlled by the amount of vaporized lubricant introduced.

[0093] The second lubricant 122 is coated using a spin coating method. Using a spin coating method for the second lubricant 122 provides the following advantages: When coating the second lubricant 122, it is necessary to avoid dissolving the already formed film of the first lubricant 121. Compared to other methods, the spin coating method allows for high-speed coating of the second lubricant 122 onto the first lubricant 121, thereby reducing the influence of the first lubricant 121 on the film during coating. Furthermore, if the spin coating method is used, the in-plane film thickness distribution of the coated film of the second lubricant 122 is less likely to increase, and unlike methods such as immersion, there is no need to add an immersion tank containing the second lubricant 122, thus providing advantages such as reducing variations in the liquid composition of the second lubricant 122.

[0094] [Polishing process]

[0095] Next, the surface of the laminate 11 is polished using an abrasive material (polishing process).

[0096] Polishing process such as Figure 2 As shown, the polishing process includes a rubbing step in which the abrasive belt 20 is pressed against the surface of the laminate 11 and rubbed. The polishing process can also utilize a method of pressing the abrasive belt 20 against the surface of the laminate 11 and rubbing it. The polishing method and polishing apparatus will be described in detail using the accompanying drawings.

[0097] Figure 6 An enlarged cross-sectional view showing an example of the abrasive belt 20 used during polishing. Figure 6As shown, the abrasive belt 20 abrades the laminate 11 by sliding the abrasive surface S relative to the surface of the laminate 11.

[0098] The abrasive belt 20 has an abrasive layer 22 on the support 21. The abrasive layer 22 has abrasive grains 221 and an adhesive 222 that bonds the abrasive grains 221 together with each other and bonds the abrasive grains 221 to the support 21, so that the abrasive grains 221 are adhered to the abrasive layer 22.

[0099] The material constituting the support 21 is not particularly limited, and various resins such as polyethylene terephthalate can be used.

[0100] Abrasive grains 221 can be used as abrasive materials included in the abrasive belt 20. Examples of abrasive grains 221 include particles of chromium oxide, α-alumina, silicon carbide, non-magnetic iron oxide, diamond, γ-alumina, α,γ-alumina, fused alumina, corundum, and synthetic diamond. Abrasive grains 221 can be particles formed from these materials. These can be one type or a suitable combination of two or more types.

[0101] There are no particular limitations on the adhesive 222; for example, thermosetting resins, thermoplastic resins, and photosensitive resins can be used. One type of resin can be used alone, or two or more types can be used in combination as the adhesive 222.

[0102] In addition, a lubricating film 23 can be provided on the surface of the grinding surface S.

[0103] Figure 7 This figure shows an example of a polishing apparatus used in the process of polishing the surface of the laminate 11 with an abrasive material. Figure 7 As shown, the polishing apparatus 80 includes: a set of polishing belts 20 (polishing belts 20A and 20B) arranged opposite each other to hold the laminate 11 from both sides, a rotation support mechanism 81, and a belt moving mechanism 82. In the polishing apparatus 80, the polishing belts 20A and 20B are arranged opposite each other to hold the laminate 11 from both sides, allowing for efficient polishing of both sides of the laminate 11 simultaneously.

[0104] The rotating support mechanism 81 supports the central opening of the laminate 11, causing the laminate 11 to rotate in the circumferential direction (arrow r direction).

[0105] The moving mechanism 82 presses the grinding belts 20A and 20B relative to each other along the radial direction of the stack 11 while pressing them in the direction of arrow F on the surfaces of the two rotating laminates 11.

[0106] In addition, the belt moving mechanism 82 has a pair of grinding belt pressing mechanisms 821 and a pair of grinding belt moving systems 822 that clamp the laminate 11 from both sides via grinding belts 20A and 20B.

[0107] A pair of grinding belt pressing mechanisms 821 includes a first grinding belt pressing mechanism 821A and a second grinding belt pressing mechanism 821B. A pair of grinding belt moving systems 822 includes a first grinding belt moving system 822A and a second grinding belt moving system 822B.

[0108] That is, the belt moving mechanism 82 has: a first grinding belt pressing mechanism 821A and a first grinding belt moving system 822A disposed on one side for clamping the laminate 11, and a second grinding belt pressing mechanism 821B and a second grinding belt moving system 822B disposed on the other side.

[0109] The first grinding belt moving system 822A includes a supply roller and a winding roller (not shown), and first guide rollers 823A-1 to 823A-4 arranged below the supply roller and the winding roller, which move the grinding belt 20A in the direction of arrow Ra.

[0110] The second grinding belt moving system 822B includes a supply roller and a winding roller (not shown), and a second guide roller 823B-1 to 823B-4 arranged below the supply roller and the winding roller, which moves the grinding belt 20B in the direction of arrow Rb.

[0111] [Removal process]

[0112] Next, Figure 2 As shown, the second lubricant 122 is removed from the laminate 11 (removal process).

[0113] The removal process includes at least one of the following steps: an ultraviolet irradiation step of irradiating the laminate 11 coated with the first lubricant 121 and the second lubricant 122 with ultraviolet light, and a heat treatment step of heating the laminate 11 coated with the first lubricant 121 and the second lubricant 122. The second lubricant 122 on the laminate 11 is removed by at least one of ultraviolet irradiation treatment 31 and heat treatment 32. As a result, the first lubricant 121 remains on the surface of the protective layer 113 of the laminate 11, and the remaining first lubricant 121 becomes the lubricating layer 12 of the magnetic recording medium 1.

[0114] In addition, preferably in the removal process, the second lubricant 122 is completely removed by ultraviolet irradiation treatment 31 or heat treatment 32, and a portion of it may remain.

[0115] In the ultraviolet irradiation process, known irradiation sources can be used, such as ultraviolet lamps or LED lamps. The emission wavelength, emission output, and irradiation time of these lamps can be appropriately selected to remove the second lubricant 122 under processing conditions. Furthermore, processing conditions that improve the adhesion of the first lubricant 121 to the protective layer 113 are also preferred. Specifically, the ultraviolet lamp is preferably selected with a peak wavelength appropriately selected from any one of 100–280 nm, 280–315 nm, or 315–400 nm. For LED lamps, to facilitate control of the emission wavelength, the LED lamp is preferably designed according to the type of lubricant used.

[0116] From the perspective of the productivity of magnetic recording medium 1, the irradiation time of ultraviolet light is preferably less than 1 minute, and the light output is adjusted so that the processing is completed within 1 minute.

[0117] Furthermore, if the ultraviolet irradiation process is carried out in the atmosphere, ozone may be generated, which can adversely affect the manufacture of the magnetic recording medium 1. Therefore, in order to suppress ozone generation, the ultraviolet irradiation process is preferably carried out in an inert gas atmosphere or in a vacuum.

[0118] The heat treatment process can utilize known heat sources. Examples of known heat sources include halogen lamp heaters, ceramic heaters, resistance heaters, and LED lamp heaters. The heating temperature and heating time using these heat sources can be appropriately selected to remove the second lubricant 122. Furthermore, processing conditions that improve the adhesion of the first lubricant 121 to the protective layer 113 are also preferred.

[0119] From the perspective of the productivity of magnetic recording media, the heating time is preferably within 15 minutes, and preferably adjusted so that the processing is completed within 15 minutes.

[0120] From the perspective of ease of design of the heating device, the heating temperature is preferably below 120°C.

[0121] Furthermore, the degassing released by the heat source, which is absorbed into the laminate 11, may adversely affect the manufacturing of the magnetic recording medium 1. To suppress the effects caused by degassing, the heat treatment process is preferably carried out in an inert gas atmosphere.

[0122] Thus, the method for manufacturing the magnetic recording medium according to this embodiment includes a coating process, a polishing process, and a removal process. In the coating process, the second lubricant 122 is coated using a spin coating method. The polishing process includes pressing an abrasive belt 20 onto the surface of the laminate 11 and rubbing it. The removal process includes either an ultraviolet irradiation process that irradiates the laminate 11 coated with the first lubricant 121 and the second lubricant 122 with ultraviolet light, or a heat treatment process that heats the laminate 11 coated with the first lubricant 121 and the second lubricant 122. The removal process can remove the second lubricant 122 through ultraviolet irradiation treatment 31 or heat treatment 32 while simultaneously forming the first lubricant 121 as a lubricating layer 12, thereby increasing the coverage of the lubricating layer 12 on the laminate 11 while reducing the amount of foreign matter generated on the surface of the lubricating layer 12. Therefore, according to the method for manufacturing a magnetic recording medium according to this embodiment, foreign matter on the surface of the magnetic recording medium 1 can be removed efficiently and effectively, and a magnetic recording medium with a high coverage of the lubricating layer 12 can be manufactured.

[0123] As described above, the magnetic recording medium 1 manufactured using the manufacturing method of the magnetic recording medium according to this embodiment has fewer foreign matter on its surface and a high coverage of the lubricating layer 12, thus suppressing wear damage caused by contact sliding with the magnetic head and improving durability. The magnetic recording medium 1 maintains excellent electromagnetic conversion characteristics and can stably have a high recording density, therefore it is suitable for use in magnetic recording playback devices. If a magnetic recording playback device includes a magnetic recording medium manufactured using the manufacturing method of the magnetic recording medium according to this embodiment, its form is not particularly limited, and it can be a magnetic recording playback device that uses a heat-assisted recording method to record magnetic information onto the magnetic recording medium, etc.

[0124] As described above, embodiments have been presented as examples and are not intended to limit the invention. These embodiments can be implemented in various other forms, and various combinations, omissions, substitutions, and modifications can be made without departing from the spirit of the invention. These embodiments and their variations are included within the scope and spirit of the invention, and are also included within the scope of the invention as described in the claims and their equivalents.

[0125] Example

[0126] The following describes this embodiment in detail based on the examples, but this embodiment is not limited to these examples.

[0127] <Example 1>

[0128] [Manufacturing of magnetic recording media]

[0129] The washed glass substrate (HOYA, 2.5-inch) was placed in the film deposition chamber of a DC magnetron sputtering apparatus (ANELVA C-3040), and the film deposition chamber was evacuated until a vacuum of 1×10⁻⁶ was achieved. -5 Pa. Then, a 10 nm thick adhesive layer was formed on the glass substrate using a Cr target by sputtering.

[0130] Next, a soft magnetic substrate layer is formed on the bonding layer by sputtering. As the soft magnetic substrate layer, a first soft magnetic recording layer, an intermediate layer, and a second soft magnetic recording layer are formed sequentially. First, using a target of Co-20Fe-5Zr-5Ta {Fe content 20 atomic%, Zr content 5 atomic%, Ta content 5 atomic%, with the remainder Co}, a first soft magnetic recording layer with a thickness of 25 nm is formed at a substrate temperature below 100 °C. Next, an intermediate layer of Ru with a thickness of 0.7 nm is formed. Then, a second soft magnetic recording layer of Co-20Fe-5Zr-5Ta with a thickness of 25 nm is formed.

[0131] Next, a seed layer with a thickness of 5 nm is formed on the soft magnetic substrate by sputtering using a Ni-6W target (W content 6 atomic%, the remainder Ni).

[0132] Then, on the seed layer, a Ru layer with a thickness of 10 nm is formed by sputtering at a sputtering pressure of 0.8 Pa as the first orientation control layer. Next, on the first orientation control layer, a Ru layer with a thickness of 10 nm is formed by sputtering at a sputtering pressure of 1.5 Pa as the second orientation control layer.

[0133] Next, by sputtering, a first magnetic recording layer containing an alloy of 91(Co15Cr16Pt)-6(SiO2)-3(TiO2) {Cr content 15 atomic%, Pt content 16 atomic%, and the remaining portion of Co 91 mol%, SiO2 6 mol%, TiO2 3 mol%} is formed on the second orientation control layer with a layer thickness of 9 nm. The sputtering pressure at this time is 2 Pa.

[0134] Next, a non-magnetic recording layer containing 88(Co30Cr)-12(TiO2){Cr content 30 atomic%, the remaining portion of Co 88 mol%, TiO2 12 mol%} is formed on the first magnetic recording layer with a layer thickness of 0.3 nm by sputtering.

[0135] Then, by sputtering, a second magnetic recording layer containing an alloy of 92(Co11Cr18Pt)-5(SiO2)-3(TiO2) {Cr content 11 atom%, Pt content 18 atom%, the remaining portion being 92 mol% Co, 5 mol% SiO2, and 3 mol% TiO2} is formed on the non-magnetic recording layer with a layer thickness of 6 nm. The sputtering pressure at this time is 2 Pa.

[0136] Then, a non-magnetic recording layer of Ru was formed on the second magnetic recording layer by sputtering with a layer thickness of 0.3 nm.

[0137] Next, a third magnetic recording layer was formed on the non-magnetic recording layer by sputtering, using a target containing Co-20Cr-14Pt-3B {Cr content 20 atomic%, Pt content 14 atomic%, B content 3 atomic%, and the remainder Co}, with a sputtering pressure of 0.6 Pa and a layer thickness of 7 nm.

[0138] Toluene, vaporized as a feed gas, was used on the surface of the third magnetic recording layer to form a carbon hydride film via ion beam deposition. During the carbon hydride film formation, the feed gas flow rate supplied to the deposition chamber was initially set to 2.9 SCCM, and the reaction pressure to 0.2 Pa. Furthermore, the cathode power serving as the excitation source for the feed gas was 225 W (AC 22.5 V, 10 A). The voltage between the cathode electrode and the anode covering it was set to 75 V, the current to 1650 mA, the ion acceleration voltage to 200 V, and the current to 180 mA. The deposition time was 1.5 seconds, resulting in a carbon hydride film with a thickness of 3.5 nm. After the carbon hydride film was formed, the feed gas supply was stopped, and the deposition chamber was vented for 2 seconds.

[0139] Next, nitrogen gas was supplied to the film-forming chamber at a flow rate of 2 SCCM and a reaction pressure of 5 Pa. Furthermore, the cathode power was set to 128 W (AC 16 V, 8 A), the voltage between the cathode and anode electrodes was 75 V, the current was 1000 mA, the ion acceleration voltage was 200 V, the current was 90 mA, and the processing time was 1 second. Nitrogen ions formed from nitrogen gas were then irradiated onto the surface of the carbon hydride film, exposing it to nitrogen plasma. This process dehydrogenated and nitrided the surface of the carbon hydride film, forming a carbon nitride film as a protective layer.

[0140] Next, D5OH(XS) (trade name: MORESCO Co., Ltd.), which is the first lubricant, was dissolved in Vertrel XF (trade name: Mitsui-DuPont Fluorochemicals Co., Ltd.) to obtain a solution for forming the first lubricating layer. The concentration of the compound contained in the solution for forming the first lubricating layer was 0.3% by mass.

[0141] [Chemistry 1]

[0142]

[0143] (m in structure (i) is a positive integer.)

[0144] Next, the solution for forming the first lubricating layer is applied to the protective layer using an immersion method. Specifically, the protective layer is immersed in the solution for forming the first lubricating layer in an immersion tank placed in the immersion coating apparatus until a laminate of each layer is formed. Then, the laminate is lifted from the immersion tank at a controlled speed. This operation is performed to make the thickness of the first lubricating layer reach a certain value. In this way, the solution for forming the first lubricating layer is applied to the surface of the protective layer. Then, the surface coated with the solution for forming the first lubricating layer is dried, thereby forming the first lubricating layer on the surface of the laminate.

[0145] Next, the second lubricant of the following structural formula (ii) was dissolved in HFE7200 (trade name, manufactured by 3M) to obtain a solution for forming a second lubricating layer. The concentration of the compound contained in the solution for forming the second lubricating layer is 0.3% by mass. In addition, HFE7200 can dissolve the second lubricant of the following structural formula, but the first lubricant D5OH(XS) cannot be dissolved.

[0146] [Chemistry 2]

[0147]

[0148] (In structure (ii), m is a positive integer.)

[0149] Next, using a spin coating method, the second lubricant is applied to the surface of the laminate on which the first lubricating layer is formed, so that the thickness of the second lubricating layer becomes... Then, the surface coated with the solution for forming the second lubricating layer is dried to form the second lubricating layer on the surface of the laminate in which the first lubricating layer is formed.

[0150] Next, the surface of the laminate with the first and second lubricating layers is polished using an abrasive belt. The abrasive belt used is manufactured by Sumitomo 3M Corporation, model DQ3, and uses Al2O3 with a particle size of 0.3 μm as the abrasive material. The polishing conditions are a lamination rotation speed of 1000 rpm and a processing time of 3 seconds.

[0151] Next, the surface of the laminate with the first and second lubricating layers formed was subjected to ultraviolet (UV) irradiation. UV irradiation was performed using a UV lamp manufactured by USHIO Electric Corporation, in a nitrogen atmosphere, for 10 seconds.

[0152] Next, a heat treatment is performed on the surface of the laminate with the first and second lubricating layers formed. The heat treatment is carried out at 120°C for 1200 seconds in a nitrogen atmosphere. By heat treating the surface of the laminate with the first and second lubricating layers formed, the second lubricating layer is removed from the surface of the first lubricating layer, and a lubricating layer is formed from the first lubricating layer.

[0153] Thus, a magnetic recording medium is manufactured in which a sealing layer, a soft magnetic substrate layer, a seed layer, a first orientation control layer, a second orientation control layer, a first magnetic recording layer, a non-magnetic recording layer, a second magnetic recording layer, a third magnetic recording layer, a carbon nitride film (protective layer), and a lubricating layer are sequentially stacked on both sides of a glass substrate.

[0154] [Evaluation of the lubrication layer]

[0155] The laminate after ultraviolet irradiation and heat treatment was analyzed using ESCA, confirming that the remaining layer thickness was [missing information]. The first lubricating layer was removed, and the second lubricating layer was removed.

[0156] (Lubricant layer coverage)

[0157] The coverage ratio of the lubricating layer on the fabricated magnetic recording medium was determined. The coverage ratio was calculated by immersing the magnetic recording medium, after the lubricating layer was formed, in a fluorocarbon solvent for 5 minutes, and then measuring the absorbance at approximately 1270 cm⁻¹ at the same location on the same medium before and after immersion using ESCA. This absorbance was then expressed as a percentage of the lubricating layer ((absorbance after immersion / absorbance before immersion) × 100). Vertrel XF (trade name, manufactured by Mitsui-DuPont Fluorochemicals) was used as the fluorocarbon solvent. The coverage ratio of the lubricating layer on the fabricated magnetic recording medium was 80%.

[0158] (TA (Thermosensitive) Sliding Evaluation)

[0159] The thermal slip (TA) evaluation of the fabricated magnetic recording media was performed. The TA slip evaluation used an MR head (manufactured by TDK) as the inspection head. The TA slip evaluation detects the phenomenon where the regenerated signal waveform changes due to frictional heat generated when the MR head collides with protrusions on the surface of the magnetic recording medium; this is known as thermal TA. The smoothness of the magnetic recording medium's surface is evaluated by the number of these signal occurrences (TA count). A lower TA count indicates a smoother surface. The average TA count for each side of 100 fabricated magnetic recording media was 7.

[0160] The manufacturing conditions for the first and second lubricants are shown in Table 1, and the processing conditions for the first and second lubricants and the evaluation results of the lubricating layer are shown in Table 2.

[0161] <Examples 2-11, Comparative Examples 1-11>

[0162] The manufacturing conditions and processing conditions of the first and second lubricants were changed to the values ​​in Tables 1 and 2. Otherwise, the magnetic recording medium was manufactured in the same manner as in Example 1, and the lubrication layer was evaluated. The manufacturing conditions of the first and second lubricants are shown in Table 1, and the processing conditions and evaluation results of the lubrication layer are shown in Table 2.

[0163] Furthermore, in any of Examples 2-11 and Comparative Examples 1-11, the D4OH and D4OH(s) (both trade names, manufactured by MORESCO Co., Ltd.) used as the first and second lubricants respectively have the following structural formula (iii) and structural formula (iv) as follows. Adjustments were made so that the average molecular weight of D4OH was 2000 and the average molecular weight of D4OH(s) was 1600. As in Example 1, HFE7200 (trade name, manufactured by 3M) was used as the solvent for the second lubricant. HFE7200 can dissolve the second lubricant, but the first lubricant cannot.

[0164] The structural formulas of D4OH and D4OH(s) are as follows:

[0165] CH2(OH)CH(OH)CH2OCH2CF2CF2(OCF2CF2CF2) m OCF2CF2CH2OCH2CH(OH)CH2OH···(iii)

[0166] (In structure (iii), m is a positive integer.)

[0167] Structural formula (iv):

[0168] [Chemistry 3]

[0169]

[0170] [Table 1]

[0171]

[0172] [Table 2]

[0173]

[0174] As can be seen from Tables 1 and 2, compared with Comparative Examples 1 to 11 corresponding to Examples 1 to 11, the coverage of the lubricating layer in Examples 1 to 11 is increased and the TA count is decreased. Therefore, using the manufacturing method of the magnetic recording medium according to this embodiment, the second lubricant is coated using a spin coating method, and the second lubricant is subjected to at least one of ultraviolet irradiation treatment and heat treatment to remove the second lubricant and form a lubricating layer formed by the first lubricant. This efficiently removes foreign matter from the surface of the magnetic recording medium while obtaining a magnetic recording medium with a high coverage of the lubricating layer.

[0175] Explanation of symbols

[0176] 1 Magnetic recording medium

[0177] 11-layer stack (the stacked body)

[0178] 12 lubrication layers

[0179] 20, 20A, and 20B are belts containing abrasive materials (abrasive belts).

[0180] 21 Supporting bodies

[0181] 22 Abrasive Layers

[0182] 31. Ultraviolet irradiation treatment

[0183] 32 Heat treatment

[0184] 51 Solution tank

[0185] 52 solution

[0186] 53 arms

[0187] 54 pillars

[0188] 60. Lubricant coating apparatus using spin coating method

[0189] 61. Tank containing a solution of lubricant.

[0190] 62 spindle

[0191] 63 Nozzles

[0192] 64 Electric motors

[0193] 70. Lubricant coating apparatus using steam method

[0194] 71 Processing Room

[0195] 72 Setting Platform

[0196] 73 Vacuum Pump

[0197] 74 Lubricant

[0198] 80 Polishing equipment

[0199] 111 substrate

[0200] 112 Magnetic Recording Layer

[0201] 113 Protective Layer

[0202] 121 First Lubricant

[0203] 122 Second Lubricant

[0204] 221 abrasive grains

[0205] 222 Adhesive

[0206] 821 A pair of grinding belt pushing mechanisms

[0207] 822 A pair of grinding belt moving systems

[0208] 821A First Grinding Belt Pushing Mechanism

[0209] 821B Second Grinding Belt Pushing Mechanism

[0210] 822A First Grinding Belt Moving System

[0211] 822B Second Grinding Belt Moving System

[0212] S grinding surface

Claims

1. A manufacturing method of a magnetic recording medium, which is a manufacturing method of a magnetic recording medium in which a lubricating layer is formed on a laminate in which a magnetic recording layer and a protective layer are sequentially stacked on a substrate, comprising: a step of applying a first lubricant and a second lubricant on the laminate, a step of polishing a surface of the laminate on which the first lubricant and the second lubricant are applied by an abrasive, and a step of removing the second lubricant on the laminate. The application of the second lubricant uses a spin coating method. The polishing step includes a step of pressing a belt including the abrasive against the surface of the laminate and rubbing. The step of removing the second lubricant includes at least one of a step of irradiating ultraviolet rays to the laminate on which the first lubricant and the second lubricant are applied and a step of performing a heat treatment of the laminate on which the first lubricant and the second lubricant are applied.

2. The manufacturing method of a magnetic recording medium according to claim 1, The average molecular weight of the first lubricant is higher than that of the second lubricant. The polarity of the first lubricant is higher than that of the second lubricant.

3. The manufacturing method of a magnetic recording medium according to claim 1 or 2, The average molecular weight of the second lubricant is 300 to 1000, and the number of polar groups is 2 or less, or the second lubricant does not contain a polar group.

4. The manufacturing method of a magnetic recording medium according to claim 1 or 2, The average molecular weight of the first lubricant is 900 to 3000, and the number of polar groups is in a range of 4 to 8.

5. The manufacturing method of a magnetic recording medium according to claim 1 or 2, 6. The manufacturing method of a magnetic recording medium according to claim 1 or 2, The step of irradiating the ultraviolet rays is performed in an atmosphere of an inactive gas or in a vacuum.

7. The manufacturing method of a magnetic recording medium according to claim 1 or 2, The film thickness of the first lubricant applied on the laminate is The film thickness of the second lubricant is The step of performing the heat treatment is performed in an atmosphere of an inactive gas. ​ ​ ​

Citation Information

Patent Citations

  • Manufacturing method of magnetic recording medium

    JP1999025452A

  • Method for manufacturing magnetic recording medium

    JP2002222519A