Steel fiber reinforced metakaolin-based recycled concrete and preparation method thereof

By optimizing the composition and preparation process of steel fiber reinforced metakaolin-based recycled concrete, the problem of insufficient dynamic impact resistance in existing technologies has been solved, achieving high toughness, green and low carbon emissions, and uniform fiber dispersion, making it suitable for harsh engineering environments.

CN121651825APending Publication Date: 2026-03-13山东航空学院

Patent Information

Application Number
CN202512018926.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-12-30
Publication Date
2026-03-13

AI Technical Summary

Technical Problem

Existing concrete materials have insufficient impact resistance under dynamic loads and it is difficult to achieve synergistic optimization of high toughness and green low carbon emissions. Existing technologies have failed to effectively solve the problems of brittle failure and energy dissipation of materials under high strain rates.

Method used

Steel fiber reinforced metakaolin-based recycled concrete is used. By optimizing the composition ratio of recycled aggregate, cementitious materials, steel fibers and admixtures, combined with nano-silica coating and step-by-step mixing process, a uniform three-dimensional fiber network is formed, which improves the energy absorption and toughness of the material under dynamic load.

Benefits of technology

It realizes the ductile failure mode of concrete under high strain rate, improves dynamic impact resistance by 30%, reduces carbon emissions and costs, and improves fiber dispersion uniformity and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses steel fiber reinforced metakaolin-based recycled concrete and a preparation method thereof, and belongs to the technical field of civil engineering materials. The concrete is prepared from the following components in percentage by mass: 60wt%-80wt% of recycled aggregate, 20wt%-40wt% of a cementing material, 0.5 wt%-1.4 wt% of steel fibers and 0.1 wt%-0.7 wt% of an additive, wherein the cementing material comprises cement and metakaolin, and the mass ratio of the metakaolin to the cement is (1-3): (7-9). A nano silicon dioxide coating is arranged on the surface of the steel fiber. The preparation method adopts a step-by-step stirring process. The problem that dynamic impact resistance and green low carbon are difficult to cooperate in the prior art is solved, through component optimization and process control, the dynamic compressive strength of the concrete is improved, the energy absorption capacity is improved, the damage mode is converted into ductility from brittleness, fiber distribution is uniform, and the concrete is suitable for impact-resistant projects such as airport runways and protective structures.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] A steel fiber reinforced metakaolin-based recycled concrete and its preparation method belong to the field of civil engineering materials technology. Background Technology

[0002] Currently, in the field of protective and transportation engineering, improving the impact resistance of concrete mainly relies on single improvement paths such as traditional high-performance concrete, fiber reinforcement, and the use of recycled aggregates or geopolymers. These solutions either focus on improving strength and toughness through optimized gradation and fiber addition, or aim to achieve environmental protection by utilizing solid waste and low-carbon cementitious materials, but none of them systematically and synergistically address the high toughness requirements of materials under dynamic loads and the green and low-carbon requirements throughout their entire life cycle.

[0003] In the area of ​​resource utilization of construction waste, existing technologies have made some progress. For example, Chinese patent CN121135195A discloses a process for preparing recycled concrete from construction waste. This technology achieves efficient and environmentally friendly treatment and utilization of construction waste through ten steps: demolition and primary sorting, pretreatment and primary crushing, secondary crushing and shaping, screening and grading, deep impurity removal and purification, aggregate strengthening, finished product storage, mix design and adjustment, batching and mixing, transportation, pouring and curing. This process improves the quality stability of recycled concrete through precise mix design and adjustment, as well as scientific batching and mixing, laying the foundation for its application in construction engineering. However, this technology mainly focuses on improving the basic physical and mechanical properties of recycled aggregates, without addressing the optimization of the material's special properties under dynamic impact loads, particularly lacking a systematic solution for improving toughness under high strain rate conditions.

[0004] Another Chinese patent, CN121017202A, focuses on a method for producing high-quality recycled aggregates from construction solid waste. It employs advanced processes such as AI vision and near-infrared spectroscopy-based collaborative sorting, dynamic closed-loop control of crushing parameters, gradient spraying and negative pressure desliming, multi-stage crushing and shaping, and deep purification. The recycled aggregates produced by this technology exhibit excellent properties, including a crushing value ≤23%, mud content ≤0.3%, needle-like and flaky content ≤12%, roundness coefficient ≥0.75, and moisture content of 3-5%, meeting the requirements for C30 and higher grade recycled concrete. While this high-quality aggregate production technology provides an important foundation for improving the performance of recycled concrete, it also fails to address the dynamic response of materials under impact loads, particularly by failing to synergistically optimize the impact resistance of recycled aggregates with specific cementitious material systems and fiber reinforcement.

[0005] Specifically, existing technologies include traditional high-performance concrete, fiber-reinforced concrete, recycled concrete, and geopolymer concrete, but each has its limitations. For example, traditional high-performance concrete relies on energy-intensive cement and natural aggregates, and although it has high strength, it is not environmentally friendly and has limited dynamic toughness. Fiber-reinforced concrete improves tensile strength by incorporating steel fibers, but often neglects the optimization of the matrix itself, resulting in weak interfaces that are prone to brittle failure under high-speed impact. Recycled concrete uses construction waste concrete as aggregate to achieve resource recycling, but due to the interface defects of recycled aggregates, its dynamic strength and toughness are significantly lower than those of natural aggregate concrete. Geopolymer concrete uses metakaolin and other materials to replace cement, reducing carbon emissions, but the matrix is ​​brittle and has insufficient impact resistance.

[0006] These existing technologies present a fundamental contradiction: materials emphasizing impact resistance typically rely on energy-intensive cement and natural aggregates, resulting in insufficient environmental friendliness; while materials emphasizing sustainability suffer from significant shortcomings in dynamic strength and toughness due to brittle matrices or weak interfaces. This makes it difficult to obtain new concrete materials that simultaneously meet stringent impact resistance requirements and green, low-carbon goals in engineering practice. Furthermore, the lack of research on dynamic performance further highlights the deficiencies of existing technologies. Split Hopkinson bar tests have revealed that traditional concrete or single-modified materials exhibit brittle failure under high strain rates, with limited dynamic strength enhancement factors and insufficient energy dissipation capacity. For example, ordinary recycled concrete is prone to pulverization under impact loads, resulting in fragmentation and a lack of toughness. Systematic research on recycled concrete synergistically modified with steel fibers and metakaolin is still relatively lacking, and complete experimental data and unified conclusions have not yet been formed, limiting its widespread application in engineering.

[0007] In summary, while existing advanced recycled concrete technologies have made breakthroughs in aggregate processing and basic properties, they have failed to achieve synergistic optimization of materials in terms of dynamic impact resistance, green and low-carbon properties, and economic efficiency. Based on research findings, this invention resolves these contradictions through a composite design of steel fibers, metakaolin, and recycled aggregates, providing an innovative solution for projects such as airport pavements. Summary of the Invention

[0008] The technical problem to be solved by the present invention is to overcome the shortcomings of the prior art and provide a steel fiber reinforced metakaolin-based recycled concrete with high dynamic impact resistance, green and low carbon content and uniform fiber dispersion, as well as its preparation method.

[0009] The technical solution adopted by the present invention to solve its technical problem is: a steel fiber reinforced metakaolin-based recycled concrete, which is composed of the following components in the following mass ratio: recycled aggregate accounting for 60wt%~80wt%, cementitious material accounting for 20wt%~40wt%, steel fiber accounting for 0.5wt%~1.4wt%, and admixture accounting for 0.1wt%~0.7wt%; wherein the cementitious material includes cement and metakaolin, and the mass ratio of metakaolin to cement is 1~3:7~9.

[0010] Through the above-described component ratio, the concrete of this invention achieves an optimized balance of material properties. The extensive use of recycled aggregates effectively utilizes construction waste, reduces natural stone mining and carbon emissions, meets the requirements of resource recycling and green building materials, and simultaneously lowers costs. The partial replacement of cement with metakaolin in the cementitious material generates dense hydration products through a volcanic ash reaction, improving matrix strength and durability, and reducing cement usage, directly lowering the carbon footprint. The incorporation of steel fibers forms a three-dimensional network, enhancing toughness and impact resistance, increasing the material's energy absorption capacity under dynamic loads by more than 30%. The addition of admixtures improves workability and density. This synergistic effect of the proportions allows the concrete to exhibit a ductile failure mode under high strain rate impact, avoiding brittle fracture, making it suitable for harsh engineering environments.

[0011] Preferably, the steel fiber surface is provided with a functional coating, and the admixture includes a fiber dispersant and a viscosity modifier to synergistically improve the uniformity of steel fiber dispersion in concrete. The functional coating on the steel fiber surface and the special admixture components significantly improve fiber dispersion uniformity, thereby enhancing the overall material integrity. The coating reduces the coefficient of friction between fibers, prevents fiber agglomeration during mixing, and ensures uniform fiber distribution in the matrix, forming an effective bridging network. The fiber dispersant and viscosity modifier further optimize the fiber suspension state through steric hindrance effect and slurry consistency control, reducing settlement and local stress concentration. This synergistic effect improves the consistency of the mechanical properties of concrete, makes crack development more uniform, improves dynamic impact resistance by approximately 20%, and extends service life.

[0012] Preferably, the steel fiber is copper-plated steel fiber with a length of 25mm~35mm, a diameter of 0.4mm~0.6mm, and an aspect ratio of 50~80; the functional coating is a nano-silica coating with a thickness of 10nm~100nm and a nano-silica particle size of 5nm~20nm; the coating is formed on the surface of the copper-plated steel fiber by a sol-gel method to reduce the coefficient of friction between fibers and prevent agglomeration. The specific geometric parameters of the copper-plated steel fiber ensure optimal anchorage and stress transfer efficiency of the fiber in the matrix. The nano-silica coating of specific thickness and particle size forms a uniform coverage by a sol-gel method, reducing the fiber surface energy and reducing mutual adsorption, thereby avoiding agglomeration. The coating also enhances the interfacial bonding strength between the fiber and the matrix, improves pull-out energy consumption, and makes the fiber bridging effect of the material more durable under impact. This design increases the peak strain of concrete by 15%~25% and improves post-failure integrity.

[0013] Preferably, the preparation process of the nano-silica coating includes: immersing copper-plated steel fibers in nano-silica sol for 5-15 minutes, followed by drying and curing at 60-80°C for 30-60 minutes to form a uniform coating. This specific preparation process ensures the uniformity and adhesion of the nano-silica coating. Controlled immersion time allows the sol to fully penetrate the fiber surface, and optimized curing temperature and time improve coating density and stability, preventing cracking or peeling. This process is simple and easy to implement, suitable for industrial production, and the coating effectively maintains fiber dispersion and resists environmental erosion during long-term use, improving the durability and fatigue resistance of concrete.

[0014] Preferably, the fiber dispersant is an anionic polyelectrolyte dispersant, its component being either sodium polyacrylate or sodium polystyrene sulfonate, and its dosage is 0.1% to 0.3% of the cementitious material mass. This dispersant prevents fiber aggregation through steric hindrance and electrostatic repulsion. The anionic polyelectrolyte dispersant effectively prevents fiber aggregation through steric hindrance and electrostatic repulsion. The dispersant forms a double electric layer in the slurry, reducing van der Waals forces between fibers and ensuring uniform fiber suspension. This effect not only improves dispersion uniformity but also reduces mixing energy consumption, improves concrete workability, maximizes fiber reinforcement, and increases tensile strength by 10% to 15%.

[0015] Preferably, the viscosity adjusting component is micronized silica fume with a specific surface area of ​​15000 m². 2 / kg~25000m 2 / kg, with an admixture dosage of 5%~8% of the cementitious material mass; this component slows down the fiber settling rate by filling slurry pores and increasing slurry consistency, ensuring uniform suspension distribution. Micronized silica fume, as a viscosity modifier, enhances slurry consistency and slows down fiber settling rate through a micro-filling effect. The high specific surface area of ​​silica fume optimizes particle size distribution, fills pores, enhances matrix density, and provides nanoscale reinforcement. This ensures that the fibers remain uniformly distributed during casting, avoiding segregation and resulting in more stable static and dynamic properties of the concrete.

[0016] Preferably, the recycled aggregate is continuously graded particles obtained from crushed and screened construction waste concrete, with a particle size range of 5mm to 20mm, wherein particles of 5mm to 10mm account for 30wt% to 40wt%, and particles of 10mm to 20mm account for 60wt% to 70wt%. The continuous gradation design of the recycled aggregate provides an optimized skeletal structure, enhancing the aggregate-paste interface transition zone. This gradation reduces porosity, increases density, provides a uniform support framework for fiber distribution, and avoids stress concentration. Simultaneously, the high quality of the aggregate ensures consistent concrete strength, increasing the dynamic compressive strength to over 45MPa.

[0017] Preferably, the admixture comprises a polycarboxylate superplasticizer and an air-entraining agent, wherein the dosage of the polycarboxylate superplasticizer is 0.5% to 1.0% of the cementitious material mass, and the dosage of the air-entraining agent is 0.01% to 0.03% of the cementitious material mass. The combined use of the polycarboxylate superplasticizer and the air-entraining agent significantly improves the rheological properties and durability of concrete. The superplasticizer reduces the water-cement ratio, improving strength and workability; the air-entraining agent introduces microbubbles, enhancing freeze-thaw resistance and fiber dispersibility. This admixture combination enables concrete to maintain stable performance under harsh environments and reduces defect formation.

[0018] A method for preparing the aforementioned steel fiber reinforced metakaolin-based recycled concrete includes the following steps: first, premixing recycled aggregate, admixtures, and 40%–50% mixing water for 20–40 seconds; then adding cementitious materials and the remaining mixing water and main mixing for 60–120 seconds; finally, adding steel fibers and mixing for 30–90 seconds; followed by vibration molding and curing. The step-by-step mixing process optimizes fiber dispersion through time-series control. Premixing ensures aggregate wetting, main mixing forms a uniform paste, and the subsequent addition of fibers avoids early agglomeration. This process is simple and efficient, suitable for large-scale production, improving the uniformity of concrete fiber distribution by 25% and ensuring batch consistency.

[0019] Preferably, the fiber dispersant is added by premixing it with 40%~50% of mixing water to form a homogeneous solution before stirring, ensuring full contact between the dispersant and the fiber. This premixing method ensures uniform dissolution and full contact between the dispersant and the fiber, improving dispersion efficiency. This method avoids excessively high local concentrations, optimizes electrostatic repulsion, and effectively isolates the fiber in the initial stages of stirring, reducing the risk of agglomeration.

[0020] Preferably, the viscosity-modifying component, micronized silica fume, is incorporated during the dry mixing stage of the cementitious materials, mixing with cement and metakaolin for 60-120 seconds to achieve particle size matching and uniform dispersion. Incorporating the viscosity-modifying component during the dry mixing stage ensures particle size matching, guarantees uniform mixing of silica fume and cementitious materials, and prevents clumping. This timing optimizes the homogeneity of the paste, provides a stable foundation for fiber dispersion, and improves the overall performance of the concrete.

[0021] Preferably, the mixing water temperature in the premixing step is 15℃~25℃, and the premixing speed is controlled at 100rpm~150rpm; the stirring step uses a forced mixer, with the main stirring speed controlled at 200rpm~300rpm, and the stirring speed reduced to 100rpm~150rpm after the steel fibers are added. Precise control of the premixing and stirring parameters optimizes fluid shear force through temperature and time management, avoiding fiber damage. Variable speed stirring reduces energy consumption and ensures uniform fiber orientation, improving material toughness.

[0022] Preferably, the curing is carried out at a temperature of 20±2℃ and a relative humidity of ≥95% for 25-30 days, with water spraying every 24 hours during the curing period to keep the specimen surface moist. Standard curing conditions (temperature 20±2℃, humidity ≥95%, curing time 25-30 days) ensure sufficient hydration reaction, improving interfacial bond strength and fiber anchoring effect. Regular water spraying prevents shrinkage cracks, ensuring long-term stable concrete performance and improving durability by more than 30%.

[0023] Compared with existing technologies, the beneficial effects of this invention are as follows: By optimizing material proportions and preparation processes, this invention achieves a synergistic improvement in the high dynamic impact resistance, green and low-carbon properties, and uniform fiber dispersion of steel fiber-reinforced metakaolin-based recycled concrete. Specifically, the extensive use of recycled aggregates promotes the resource utilization of construction waste, reducing carbon emissions and costs; the partial replacement of cement with metakaolin in the cementitious material enhances matrix density and durability through volcanic ash reaction, reducing cement usage; the incorporation of steel fibers forms a three-dimensional network, increasing energy absorption capacity by more than 30% and preventing brittle fracture. Simultaneously, the nano-silica coating and special admixtures reduce fiber friction, optimize slurry consistency, ensure uniform fiber dispersion, reduce stress concentration, and improve dynamic impact resistance by approximately 20%. Stepwise mixing processes and precise parameter control further ensure fiber orientation and distribution uniformity, while standard curing conditions enhance interfacial bonding, improving durability by more than 30%. Overall, this invention solves the problems of insufficient dynamic toughness, poor environmental performance, and fiber agglomeration in existing technologies, making it suitable for demanding projects such as airport runways. Detailed Implementation

[0024] The invention will be further described below with reference to specific embodiments. All embodiments use recycled aggregate (particle size range 5mm~20mm, of which 5mm~10mm particles account for 30wt%~40%, and 10mm~20mm particles account for 60wt%~70%) obtained from crushed and screened construction waste concrete. The cementing materials are P.O42.5 grade cement and metakaolin (purity ≥95%). The steel fibers are copper-plated steel fibers (length 25mm~35mm, diameter 0.4mm~0.6mm). The admixtures include polycarboxylate superplasticizer (solid content 40%), air-entraining agent (alkyl sulfonate), fiber dispersant (sodium polyacrylate), and viscosity modifier (micronized silica fume, specific surface area 15000m²). 2 / kg~25000m 2 / kg). The preparation method follows the stepwise mixing process and uses a forced mixer. Curing is carried out in a standard curing room (temperature 20±2℃, relative humidity ≥95%). Example 1

[0025] The proportions and process parameters used were as follows: recycled aggregate 70 wt%, cementitious material 30 wt% (of which cement accounted for 27 wt% and metakaolin for 3 wt%, i.e., the mass ratio of metakaolin to cement was 1:9), steel fiber 1.1 wt%, and admixtures 0.4 wt% (including polycarboxylate superplasticizer at 0.8% of the cementitious material mass, air-entraining agent at 0.02%, fiber dispersant at 0.2%, and viscosity modifier at 6% of the cementitious material mass). A nano-silica coating (coating thickness 50 nm, nano-silica particle size 10 nm) was prepared on the surface of the steel fiber using the sol-gel method. The impregnation time was 10 min, and the drying and curing temperature was 70℃ for 45 min. In preparation, recycled aggregate, admixtures, and 45% mixing water (20℃) were premixed for 30 seconds (120 rpm). Then, cementitious materials and the remaining mixing water were added and stirred for 90 seconds (250 rpm). Finally, steel fibers were added and stirred for 60 seconds (speed reduced to 120 rpm). The mixture was then vibrated and molded, and cured for 28 days at a temperature of 20±2℃ and a relative humidity of ≥95%, with water spraying every 24 hours during the curing period. The concrete in this embodiment exhibited excellent performance: dynamic compressive strength reached 65 MPa, energy absorption capacity was increased by 35% compared to ordinary recycled concrete, fiber dispersion was highly uniform, and the failure mode showed ductile characteristics. Example 2

[0026] The proportions and process parameters used are as follows: 60 wt% recycled aggregate and 40 wt% cementitious material (of which cement accounts for 28 wt% and metakaolin accounts for 12 wt%, i.e., a mass ratio of 3:7), 0.5 wt% steel fiber, and 0.1 wt% admixtures (containing only 0.5% polycarboxylate superplasticizer and 0.01% air-entraining agent, without fiber dispersant or viscosity modifier). The steel fiber has no coating. Other ingredients and preparation processes are the same as in Example 1, but the premixing time is shortened to 20 s, the main mixing time is extended to 120 s, and the steel fiber mixing time is set to 30 s; the curing conditions are the same. Example 3

[0027] The mix proportions and process parameters used were: 80 wt% recycled aggregate and 20 wt% cementitious material (of which cement accounted for 18 wt% and metakaolin for 2 wt%, i.e., a mass ratio of 1:9), 1.4 wt% steel fiber, and 0.7 wt% admixtures (including 0.3% fiber dispersant, 8% viscosity modifier, water-reducing agent, and air-entraining agent). The steel fiber coating thickness was set to 100 nm, the impregnation time was 15 min, and the curing temperature was 80℃ for 60 min. Other ingredients and preparation processes were the same as in Example 1, but the premixing time was 40 s, the main mixing time was 60 s, and the steel fiber mixing time was 90 s; the curing time was extended to 30 days. The concrete in this example maximizes resources by utilizing high aggregate content, but the lower cementitious material content results in a slightly lower matrix density. The high fiber content, combined with the coating and dispersant, ensures uniform fiber distribution and improves dynamic impact resistance by 25%, but the excessive fiber slightly agglomerates, increasing the peak strain by 20%, which is not as balanced as in Example 1. This example demonstrates the need for a balance between high fiber content and matrix optimization. Example 4

[0028] The formulation in this embodiment is the same as in Example 1, but the preparation process is changed: the pre-mixing step is omitted, and all components are directly stirred for 120 seconds (250 rpm) at one time; the curing conditions are the same. The dynamic strength enhancement factor is only 1.2 (1.8 in Example 1), and the failure mode is mainly brittle. Example 5

[0029] The formulation and preparation process are the same as in Example 1, except that the viscosity adjusting component has a specific surface area of ​​25000 m². 2 The silica fume content is 8% per kg, and the fiber dispersant is replaced with sodium polystyrene sulfonate at a dosage of 0.3%. In the preparation process, the fiber dispersant is first premixed with 50% mixing water to form a solution, and then added to the stirring; the silica fume is added during the dry mixing stage of the cementitious materials and mixed for 120 seconds. The fibers are uniformly suspended, resulting in high concrete density, a 40% increase in dynamic energy dissipation, and excellent long-term durability. Example 6

[0030] The proportions and preparation process are the same as in Example 1, except that: 75wt% recycled aggregate, 25wt% cementitious material (of which cement accounts for 24.75wt% and metakaolin accounts for 0.25wt%, i.e., a mass ratio of 1:99), 1.4wt% steel fiber, and 0.3wt% admixtures (including 0.6% water-reducing agent, 0.02% air-entraining agent, 0.1% fiber dispersant, and 5% silica fume) are used. The steel fiber coating thickness is 10nm, the impregnation time is 5min, and the curing temperature is 60℃ for 30min. During preparation, pre-mixing is performed for 25s (water temperature 15℃, speed 100rpm), main stirring for 120s (speed 200rpm), and fiber stirring for 90s (speed 100rpm); curing is carried out for 30 days. The fiber dispersion uniformity is good, and the energy absorption is increased by 22%. Example 7

[0031] The composition consists of 60 wt% recycled aggregate, 40 wt% cementitious material (10 wt% cement and 30 wt% metakaolin, i.e., a mass ratio of 3:7), 0.5 wt% steel fiber, and 0.7 wt% admixtures (including 1.0% water-reducing agent, 0.03% air-entraining agent, 0.3% fiber dispersant, and 8% silica fume). The steel fiber is uncoated. The preparation process is the same as in Example 1, but the curing time is shortened to 25 days. It exhibits high static strength (compressive strength 48 MPa) and a 12% increase in energy absorption. Example 8

[0032] The mixing ratio is the same as in Example 1, but the process time is optimized: premixing for 20 seconds, main mixing for 60 seconds, and fiber mixing for 30 seconds. The curing time is reduced to 25 days, and the curing temperature is maintained at 20±2℃, but the humidity is reduced to 90%. Simultaneously, the fiber coating adopts a rapid curing process (immersion for 5 minutes, curing at 80℃ for 30 minutes). The fiber dispersibility and workability meet the requirements for rapid construction, energy absorption is increased by 28%, and costs are reduced. Example 9

[0033] The mixing ratio is the same as in Example 1, but the parameters are adjusted: the mixing water temperature is increased to 25°C, the curing temperature is set to 22°C and the humidity to 98%, and water is sprayed once every 12 hours during the curing period. The amount of air-entraining agent in the admixture is increased to 0.03% to improve impermeability. The thickness of the steel fiber coating is increased to 100nm to enhance corrosion resistance.

[0034] Comparative Example 1 The proportions were the same as in Example 1, with 70 wt% recycled aggregate and 30 wt% cementitious materials (27 wt% cement and 3 wt% metakaolin). The steel fiber content was reduced to 0.2 wt% (far below the 0.5 wt% lower limit of claim 1), and the admixture composition was the same as in Example 1. The preparation process followed the stepwise mixing and standard curing procedures of Example 1. Due to the excessively low fiber content, an effective three-dimensional fiber network could not be formed.

[0035] Comparative Example 2 The formulation is the same as in Example 1 (1.1 wt% steel fiber), but the nano-silica coating on the surface of the steel fiber is completely omitted, and no fiber dispersant is added to the additives (only the water-reducing agent and air-entraining agent are retained). In the preparation process, the steel fiber is directly incorporated without coating treatment; the stirring steps remain unchanged. The coefficient of friction between fibers is high, and severe agglomeration occurs during stirring, resulting in uneven fiber distribution after molding.

[0036] Comparative Example 3 The proportions were the same as in Example 1, but the preparation process was changed: all components (aggregate, cementitious materials, fiber, admixtures, and water) were added to the mixer at once and continuously mixed at 250 rpm for 180 seconds, followed by vibration molding and standard curing. The concrete had poor workability and bleeding occurred.

[0037] Comparative Example 4 The traditional concrete formula was used: 70 wt% natural aggregate, 30 wt% pure cementitious material (without metakaolin), 1.1 wt% steel fiber, and the admixture composition was the same as in Example 1. The preparation process was the same as in Example 1. The matrix was brittle and cracks propagated rapidly.

[0038] The following are the key performance test results of the embodiments and comparative examples of this invention. All tests were conducted in accordance with relevant national standards, including the "Standard for Test Methods of Mechanical Properties of Ordinary Concrete" (GB / T 50081-2019) for static performance testing, and the Split Hopkinson Bar (SHPB) test for dynamic impact performance evaluation. The test results are shown in Table 1.

[0039] Table 1 Performance Test Results

[0040] Test method description: Dynamic compressive strength: determined by SHPB testing at high strain rates (45-110 s⁻¹). -1 The measurement reflects the peak bearing capacity of the material under impact load.

[0041] Energy absorption enhancement: Using ordinary recycled concrete as a baseline (set to 0%), calculate the energy dissipation increment of the material of the present invention under dynamic impact.

[0042] Failure modes: Ductile failure refers to "cracks without breaking", while brittle failure refers to pulverization and fragmentation.

[0043] Fiber dispersion uniformity: fiber distribution index (range 0-1, ≥0.8 is excellent), the higher the index, the more uniform the dispersion.

[0044] Example 1 showed the best performance in terms of dynamic compressive strength (65 MPa) and energy absorption improvement (35%), with a ductile failure mode and high fiber dispersion uniformity, meeting the requirements for high impact resistance. Comparative Example 1 showed only an 8% increase in energy absorption, demonstrating insufficient performance when the steel fiber content is below 0.5 wt%. Comparative Example 2, lacking coating and dispersant, showed that fiber agglomeration led to a deterioration in the failure mode. These performance test results demonstrate that the present invention achieves a balance between dynamic performance, environmental friendliness, and economy through component synergy and process optimization.

[0045] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention in any other way. Any person skilled in the art may make changes or modifications to the above-disclosed technical content to create equivalent embodiments. However, any simple modifications, equivalent changes, and modifications made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the protection scope of the present invention.

Claims

1. A steel fiber reinforced metakaolin-based recycled concrete, characterized in that, It is composed of the following components in the following mass ratio: recycled aggregate accounting for 60wt%~80wt%, cementitious material accounting for 20wt%~40wt%, steel fiber accounting for 0.5wt%~1.4wt%, and admixture accounting for 0.1wt%~0.7wt%; wherein the cementitious material includes cement and metakaolin, and the mass ratio of metakaolin to cement is 1~3:7~9.

2. The steel fiber reinforced metakaolin-based recycled concrete according to claim 1, characterized in that: The surface of the steel fiber is provided with a functional coating, and the additives include fiber dispersants and viscosity modifiers.

3. The steel fiber reinforced metakaolin-based recycled concrete according to claim 1, characterized in that: The steel fiber is a copper-plated steel fiber with a length of 25mm~35mm, a diameter of 0.4mm~0.6mm, and an aspect ratio of 50~80; the functional coating is a nano-silica coating with a thickness of 10nm~100nm and a nano-silica particle size of 5nm~20nm; the coating is formed on the surface of the copper-plated steel fiber by a sol-gel method.

4. The steel fiber reinforced metakaolin-based recycled concrete according to claim 3, characterized in that: The preparation process of the nano-silica coating includes: immersing copper-plated steel fibers in nano-silica sol for 5 min to 15 min, and then drying and curing them at 60℃ to 80℃ for 30 min to 60 min to form a uniform coating.

5. The steel fiber reinforced metakaolin-based recycled concrete according to claim 2, characterized in that: The fiber dispersant is an anionic polyelectrolyte dispersant, and its component is either sodium polyacrylate or sodium polystyrene sulfonate, with a dosage of 0.1% to 0.3% of the mass of the cementitious material.

6. The steel fiber reinforced metakaolin-based recycled concrete according to claim 2, characterized in that: The viscosity-adjusting component is micronized silica fume with a specific surface area of ​​15000 m². 2 / kg~25000m 2 / kg, with an admixture dosage of 5% to 8% of the mass of the cementitious material.

7. The steel fiber reinforced metakaolin-based recycled concrete according to claim 1, characterized in that: The recycled aggregate is a continuously graded particle obtained by crushing and screening construction waste concrete, with a particle size range of 5mm to 20mm, of which 5mm to 10mm particles account for 30wt% to 40wt% and 10mm to 20mm particles account for 60wt% to 70wt%.

8. The steel fiber reinforced metakaolin-based recycled concrete according to claim 1, characterized in that: The admixture includes a polycarboxylate superplasticizer and an air-entraining agent. The dosage of the polycarboxylate superplasticizer is 0.5% to 1.0% of the mass of the cementitious material, and the dosage of the air-entraining agent is 0.01% to 0.03% of the mass of the cementitious material.

9. A method for preparing steel fiber reinforced metakaolin-based recycled concrete according to any one of claims 1 to 8, characterized in that, Includes the following steps: First, premix the recycled aggregate, admixtures, and 40%~50% mixing water for 20s~40s. Then, add the cementitious material and the remaining mixing water and stir for 60s~120s. Finally, add the steel fiber and stir for 30s~90s. Then, vibrate and mold the mixture and cure it.

10. The method for preparing steel fiber reinforced metakaolin-based recycled concrete according to claim 9, characterized in that: The curing process involves curing at a temperature of 20±2℃ and a relative humidity of ≥95% for 25 to 30 days, with water sprayed every 24 hours during the curing period to keep the surface of the specimen moist.

Citation Information

Patent Citations

  • Building solid waste high-quality recycled aggregate regeneration method

    CN121017202A

  • Construction waste resource recycled concrete preparation process

    CN121135195A

Cited By

  • High-strength concrete and preparation method and application thereof

    CN122277192A

  • A high-strength concrete, its preparation method and application

    CN122277192B