Binuclear copper modified molybdenum germanic acid crystalline material and preparation method and application thereof

By preparing a binuclear copper-modified molybdenum germanate crystalline material, and utilizing its Cu(II)/Cu(I) redox couple and the regular porous structure of the organic ligand L, the problems of high energy consumption and severe pollution in ammonia synthesis were solved, achieving a highly efficient and green reduction of nitrate to ammonia.

CN121736302APending Publication Date: 2026-03-27BOHAI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202511903332.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-12-17
Publication Date
2026-03-27

AI Technical Summary

Technical Problem

In existing technologies, the synthesis of ammonia is energy-intensive and polluting, and traditional biological nitrification-denitrification and physicochemical separation technologies are time-consuming and costly, making it difficult to effectively treat nitrate pollution in water bodies.

Method used

A binuclear copper-modified molybdenum germanate crystalline material was used as an electrocatalyst to promote the reduction of NO3- through electron transfer and the Cu(II)/Cu(I) redox couple. The preparation method included the synthesis of [Cu2(L)2(HL)4(H2O)2(GeMo12O40)2]·3H2O crystalline material at high temperature, which was combined with organic ligand L to form a regular porous structure.

Benefits of technology

It significantly improves the electrocatalytic NO3- reduction performance, efficiently converts nitrate to ammonia, and has high ammonia yield and Faraday efficiency. It solves the problems of high energy consumption and pollution, and realizes a green and sustainable ammonia synthesis pathway.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121736302A_ABST
    Figure CN121736302A_ABST
Patent Text Reader

Abstract

The invention discloses a binuclear copper modified molybdenum germanic acid crystalline material as well as a preparation method and application thereof. The molecular formula of the material is [Cu2 (L) 2 (HL) 4 (H2O) 2 (GeMo12O40) 2]. 3H2O; l is 1-(4-carboxyl benzyl)-[4, 4 '] bipyridine chloride; the crystal system is monoclinic; the space group is P21 / n; the cell parameters are as follows: a is equal to 18.0008 (6), b is equal to 20.8877 (6), c is equal to 20.5829 (7), alpha is equal to 90 degrees, beta is equal to 90.2370 (10) degrees, gamma is equal to 90 degrees, and Z is equal to 2. The preparation method comprises the following steps: 1, dissolving germanium oxide, ammonium molybdate, a copper salt and a ligand L in water, and regulating the pH value of the solution by using an acid regulator to obtain a reaction solution; and step 2, reacting the reaction solution in the step 1 in a high-temperature closed environment, and cooling to room temperature after the reaction is finished to obtain the binuclear copper modified molybdenum germanic acid crystalline material. According to the crystalline material synthesized by the invention, Keggin type polyacid GeMo12 and a binuclear copper site are integrated in a single framework, and electrons are directly transferred into the copper site from the polyacid through weak interaction after the polyacid obtains the electrons, so that the catalytic performance is greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present application relates to the field of crystalline catalyst material preparation, and particularly relates to a binuclear copper modified molybdenum germanate crystalline material, a preparation method and application thereof. BACKGROUND

[0002] Ammonia, as a high-value chemical raw material, is widely used in fertilizer production and chemical manufacturing (dye, textile, etc.), and is currently mainly synthesized by the Haber-Bosch process. This process is a high-energy industrial method that requires the activation of inert nitrogen and hydrogen derived from fossil fuels under high temperature and high pressure. Current industrial data shows that this process consumes 1-2% of the world's energy and produces 1.4% of annual carbon dioxide emissions over the past century, which is fundamentally in conflict with the sustainable development goals. In addition, the overuse of nitrogen-based fertilizers and the improper discharge of industrial wastewater have led to a continuous increase in nitrate concentration in water bodies, and the accumulation of excessive nitrate poses a serious threat to the stability of the ecosystem and human health, including water eutrophication, soil degradation, and an increased risk of diseases such as methemoglobinemia. Traditional biological nitrification-denitrification and physical-chemical separation technologies are often limited by time-consuming, high cost, and harsh operating conditions.

[0003] To overcome these shortcomings, electrocatalytic nitrate reduction reaction (e-NO3RR) has become a promising alternative. This method uses electrons and water as clean reducing agents and proton sources, and takes advantage of the high reactivity of the electrode-electrolyte interface to reduce NO3 - , which is a key chemical raw material and carbon-free energy carrier, represents a green and sustainable conversion path from both environmental and energy perspectives.

[0004] As a class of well-defined, soluble d-block high-oxidation-state transition metal (usually W 6+ , V 4+ , V 5+ , Mo 5+ , and Mo 6 + ) nanometer oxygen cluster compounds, POMs (Polyoxometalates, polyoxometalates) have a wide range of applications in energy storage, catalysis, and other fields due to their electronic delocalization characteristics and reversible redox properties. However, their practical applications are often limited by insufficient stability, limited specific surface area, and easy aggregation. Combining electron-rich POMs with transition metal complexes with well-defined active catalytic sites to construct polyacid-based transition metal complex composites may be an important means to promote electron transfer and improve the performance of electrocatalytic NO3 - reduction.

[0005] This strategy not only maintains the structural integrity and reversible redox activity of POMs in energy storage, but also introduces specific metal active sites, thereby significantly improving the electrocatalytic performance. This composite material combines the dual advantages of POMs and transition metal complexes: it provides transition metal active elements (iron, cobalt, copper, tungsten, molybdenum, etc.), and constructs a regular porous structure through organic ligands. In addition, based on the synergistic effect between POMs and transition metal complexes, this composite material is expected to exhibit better electrocatalytic activity than single transition metal complexes in the reduction of NO3 - reduction reaction. On the one hand, POMs provide electron-rich centers and enhance electron transfer ability; on the other hand, transition metal complexes improve the stability of the reduced electron-rich POMs, thereby constructing an efficient and long-acting electrocatalytic NO3 - reduction reaction catalyst. SUMMARY

[0006] In view of the deficiencies of the prior art, the present application provides a binuclear copper modified molybdenum germanate crystalline material, a preparation method and application thereof.

[0007] The technical solution of the present application to solve the technical problem of the material is to provide a binuclear copper modified molybdenum germanate crystalline material, characterized in that the molecular formula of the material is [Cu2(L)2(HL)4(H2O)2(GeMo 12 O 40 )2]·3H2O; L = 1-(4-carboxybenzyl)-[4,4']bipyridine chloride; the crystal system is monoclinic; the space group is P21 / n; the unit cell parameters are a = 18.0008(6) Å, b = 20.8877(6) Å, c = 20.5829(7) Å, α = 90°, β = 90.2370(10) °, γ = 90°, Z = 2.

[0008] The technical solution of the present application to solve the technical problem of the method is to provide a preparation method of a binuclear copper modified molybdenum germanate crystalline material, characterized in that the method comprises the following steps: Step 1, dissolve germanium oxide, ammonium molybdate, copper salt and ligand L in water, and then adjust the pH of the solution with an acid regulator to obtain a reaction solution; Step 2, react the reaction solution of step 1 in a high-temperature sealed environment, and then cool to room temperature to obtain the binuclear copper modified molybdenum germanate crystalline material.

[0009] Compared with the prior art, the present application has the following advantages: (1) The crystalline material synthesized by the present application has a Keggin-type polyacid GeMo 12The polyanion, integrated with the dinuclear copper site in a single framework, transfers the electron directly from the polyanion to the copper site through weak interaction after obtaining the electron, thereby greatly improving the catalytic performance. In addition, the Cu(II) / Cu(I) redox couple of the dinuclear copper in the structure can also greatly improve the catalytic performance in the electrocatalytic NO3-reduction process. Based on the above effects, the material has high catalytic performance and excellent selectivity, excellent NO3RR performance, high ammonia yield and Faraday efficiency, and has very good application value in the field of nitrate reduction.

[0010] (2) The crystalline material of the application is prepared by one-step hydrothermal reaction of germanium molybdate (synthesized by germanium oxide and ammonium molybdate), copper salt and ligand L, and is a crystalline material with a novel cuboid structure. In the structure, each Cu center forms a six-coordinated geometry through three N atoms and one O atom of the organic ligand L and two water molecules. Two Cu 2+ ions, two L ligands and two water molecules form a quadrilateral [Cu(L)(H2O)]2 4+ unit with a size of 15.804 Å x 11.312 Å. Subsequently, four protonated L ligands are coordinated through Cu-N bonds to generate a dinuclear subunit [Cu2(L)2(HL)4(H2O)2] 8+ . These [Cu2(L)2(HL)4(H2O)2] 8+ units are connected by hydrogen bonds to form a one-dimensional chain structure. Discrete GeMo 12 polyacid anions are anchored on the chains through strong hydrogen bonds, which facilitates the transfer of electrons from GeMo 12 polyacid to the dinuclear copper site. Subsequently, these one-dimensional chains are expanded into a two-dimensional layered structure through hydrogen bond interactions, and further connected to each other through additional hydrogen bonds to form a three-dimensional supramolecular framework.

[0011] (3) In the structure of the compound, there is a Cu(II) / Cu(I) redox couple. Specifically, during the electrocatalytic reduction of NO3 - , the application of potential initiates the immediate transfer of electrons from the polyanion to the Cu 2+ active site, in which Cu 2+ is reduced to Cu + . Subsequently, the adsorbed NO3 - captures electrons from the Cu + site and is reduced to NO2 - , while causing Cu + to be re-oxidized to Cu 2+ . Copper acts as an electron shuttle between Cu 2+ and Cu +The redox cycle is continuously carried out between the two to promote the step-by-step reduction of the nitrogen-containing intermediate, so as to maintain the dynamic valence cycle thereof. BRIEF DESCRIPTION OF DRAWINGS

[0012] Figure 1 A basic structural unit diagram of the binuclear copper modified molybdenum germanate crystalline material of the present application; Figure 2 A one-dimensional structural diagram of the binuclear copper modified molybdenum germanate crystalline material of the present application; Figure 3 An X-ray diffraction diagram of the binuclear copper modified molybdenum germanate crystalline material prepared in Example 1 of the present application; Figure 4 A photoelectron spectrum diagram of Cu in the binuclear copper modified molybdenum germanate crystalline material prepared in Example 1 of the present application; Figure 5 A photoelectron spectrum diagram of Mo in the binuclear copper modified molybdenum germanate crystalline material prepared in Example 1 of the present application; Figure 6 An infrared spectrum diagram of the binuclear copper modified molybdenum germanate crystalline material prepared in Example 1 of the present application; Figure 7 A UV-Vis absorption spectrum diagram of ammonia detected at different voltages in a 0.5M Na2SO4 and 0.1M KNO3 solution of the binuclear copper modified molybdenum germanate crystalline material prepared in Example 1 of the present application; Figure 8 A diagram of ammonia yield and Faraday efficiency at different voltages drawn according to Figure 7 Example 1 of the present application; Figure 9 A UV-Vis absorption spectrum diagram of hydrazine hydrate detected at different voltages of the binuclear copper modified molybdenum germanate crystalline material prepared in Example 1 of the present application.

[0013] Figure 1 And Figure 2 In the formula, 1 is Cu, 2 is O, 3 is N, 4 is Ge, 5 is Mo, and 6 is C. DETAILED DESCRIPTION

[0014] The following gives specific embodiments of the present application. The specific embodiments are only used to further illustrate the present application and do not limit the protection scope of the present application.

[0015] The present application provides a binuclear copper modified molybdenum germanate crystalline material (referred to as material for short), characterized in that the molecular formula of the material is [Cu2(L)2(HL)4(H2O)2(GeMo 12 O 40)2]·3H2O; L = 1-(4-carboxybenzyl)-[4,4']bipyridinium chloride; the crystal system is monoclinic; the space group is P21 / n; the cell parameters are a = 18.0008(6) Å, b = 20.8877(6) Å, c = 20.5829(7) Å, α = 90°, β = 90.2370(10) °, γ = 90°, Z = 2.

[0016] The application also provides a kind of binuclear copper modified molybdenum germanic acid crystal state material (referred to as method), it is characterized in that, the method comprises the following steps: Step 1, preparation of reaction solution: germanium oxide, ammonium molybdate, copper salt and ligand L are dissolved in water, and then the pH of the solution is adjusted by an acid regulator to obtain a reaction solution; Preferably, in step 1, the copper salt is copper acetate, copper sulfate or copper chloride; the ligand L is 1-(4-carboxybenzyl)-[4,4']bipyridinium chloride; and the water is deionized water or distilled water.

[0017] Preferably, in step 1, the molar ratio of ammonium molybdate to germanium oxide is 1:0.25-0.28; the molar ratio of ammonium molybdate to copper salt is 1:9-11; the molar ratio of ammonium molybdate to ligand L is 1:0.03-0.05; and the amount-of-substance ratio of ammonium molybdate to water is 1 mmol:40-60 mL.

[0018] Preferably, in step 1, the dissolution process is as follows: the stirring method is used, the temperature is normal temperature, the stirring speed is 900-1500 rpm, and the stirring time is 4-8 h.

[0019] Preferably, in step 1, the acid regulator is sulfuric acid, nitric acid or hydrochloric acid.

[0020] Preferably, in step 1, the pH of the solution is adjusted to 2.8-5.0.

[0021] Step 2, the reaction solution of step 1 is reacted in a high-temperature sealed environment, and then cooled to room temperature after the reaction is completed to obtain brown-yellow block-shaped crystals, which are binuclear copper modified molybdenum germanic acid crystal state materials.

[0022] Preferably, in step 2, the high-temperature sealed environment is a polytetrafluoroethylene reaction kettle.

[0023] Preferably, in step 2, the reaction temperature is 120-150°C, and the reaction time is 6-8 days.

[0024] Preferably, in step 2, the cooling rate is 8-10°C / h.

[0025] The application also provides an application of the binuclear copper modified molybdenum germanic acid crystal state material, characterized in that the material is used as a raw material to prepare a modified electrode.

[0026] Preferably, the preparation method of the binuclear copper modified molybdenum germanate crystal state material modified electrode comprises the following steps: (1) 450 μL of water, 25 μL of isopropyl alcohol and 25 μL of Nafion solution are measured and dropped into a plastic tube, and mixed uniformly to obtain a colorless transparent solution; (2) 10 mg of binuclear copper modified molybdenum germanate crystal state material and 10 mg of acetylene black are put into an agate mortar and ground for 30 min to obtain a mixture; 10 mg of the mixture is weighed and put into the colorless transparent solution of step (1), and ultrasonic treatment is performed for 30 min under the condition of 80 Hz, and manual shaking is performed simultaneously to avoid material precipitation; (3) 10 μL of liquid in the middle of the plastic tube is measured by a pipette and dropped on a 1×2 cm 2 size conductive carbon cloth, a total of 5 times, a total of 50 μL, and natural air drying to obtain a binuclear copper modified molybdenum germanate crystal state material modified electrode (referred to as a modified electrode).

[0027] Example 1: (1) 0.011 g of germanium oxide, 0.5 g of ammonium molybdate, 0.479 g of copper sulfate and 0.0022 g of 1-(4-carboxybenzyl)-[4,4']bipyridine chloride are dissolved in 50 mL of water, and stirred at room temperature at 1200 rpm for 4 h; then the pH of the solution is adjusted to 4.0 with nitric acid to obtain a reaction solution; (2) The reaction solution is added to a polytetrafluoroethylene reaction kettle, and after reaction in the polytetrafluoroethylene reaction kettle at a temperature of 130℃ for 6 days, the temperature is lowered to room temperature at a rate of 10℃ / h to obtain green block crystals, which are binuclear copper modified molybdenum germanate crystal state materials.

[0028] In the example, the specific process of crystal structure determination is as follows: the single crystal is placed on a Bruker SMART CCD 1000 type X-ray single crystal diffractometer, monochromatic Mo Ka (λ=0.71073 Å) is used as incident radiation at a temperature of 273 K. The absorption correction of the data is carried out by using SADABS software, the structure is analyzed by using SHELXTL software package, the method used is direct method, and all non-hydrogen atom coordinates are corrected by using anisotropic thermal parameters. The hydrogen atom coordinates on the organic group are obtained by using the method of geometric hydrogenation. The X-ray crystallographic parameters are shown in Table 1.

[0029] Table 1

[0030] a R 1 = ∑║ F o │─│ Fc ║ / ∑│ F o │, b wR 2 = ∑[ w ( F o 2 — F c 2 ) 2 ] / ∑[ w ( F o 2 ) 2 ] 1 / 2 X-ray crystal structure description: X-ray single-crystal diffraction analysis shows that the dinuclear copper-modified molybdate germanate crystalline material prepared in Example 1 has the molecular formula [Cu2(L)2(HL)4(H2O)2(GeMo] 12 O 40 [GeMo2]·3H2O. The unit cell of this material consists of two free [GeMo2] atoms. 12 O 40 ] 4- Polyacid, Two Cu II It consists of ions, two L ligands, four protonated L ligands (HL), two coordinated water molecules, and three free water molecules, as follows: Figure 1 As shown.

[0031] Depend on Figure 2 It can be seen that the two Cu 2+ The ion, two L ligands, and two water molecules form a quadrilateral [Cu(L)(H₂O)]₂ with dimensions of 15.804 Å × 11.312 Å. 4+ The unit is then formed by coordinating four protonated L ligands via Cu–N bonds to generate a binuclear subunit [Cu2(L)2(HL)4(H2O)2]. 8+ .

[0032] Figure 3 In the figure, 1 represents the simulated peak of the crystalline material, and 2 represents the actual peak of the crystalline material. The simulated peak and the actual peak are completely consistent, indicating that the binuclear copper-modified molybdenum germanate crystalline material has been successfully synthesized.

[0033] Figure 4 In the figure, two peaks appear at 935.16 eV and 954.52 eV, which belong to Cu, respectively. 2+ Co 2p 3 / 2 and Co 2p 1 / 2 Yes. Meanwhile, the binding energies of 941.85 eV, 944.18 eV, and 962.48 eV belong to Co. 2+The satellite peak.

[0034] Figure 5 In the figure, the characteristic peaks at 232.4 eV and 235.59 eV are attributed to Mo. 6+ 3d5 / 2 and Mo 6+ 3d3 / 2.

[0035] Figure 6 In the middle, 773, 805, 993 and 984cm –1 The characteristic spectral bands at this location are attributed to ν(Mo-Oc-Mo), ν(Mo-Od), and ν(Ge-Oa). (1010-1765 cm⁻¹) -1 The characteristic peaks in the region are attributed to L-ligands.

[0036] Figure 7 In this study, the material prepared in Example 1 was drop-coated onto conductive carbon cloth as an electrocatalyst for reducing nitrate ions in 0.5 M Na₂SO₄ and 0.1 M KNO₃ solutions. Figure 7 As can be seen, within the voltage range of -0.8V to -1.4V, the solution reaches its maximum absorbance at -1.2V and its maximum Faraday efficiency at -1.1V. Therefore, the binuclear copper-modified molybdate germanate crystalline material has excellent application value in the field of nitrate reduction.

[0037] Depend on Figure 8 It can be seen that its maximum NH3 production is 14.56 mg·h⁻¹. -1 mg cat -1 Faraday efficiency FE NH3 It is 94.06%.

[0038] Figure 9 To investigate whether the binuclear copper-modified molybdenum germanate crystalline material prepared in Example 1 of this invention will produce the byproduct hydrazine hydrate when used as an electrocatalyst. Figure 9 It can be seen that within a voltage range of -0.8V to -1.4V, the UV-Vis absorbance of the solution and the blank solution are basically the same, indicating that there is no hydrated hydrazine in the solution. This further proves that the product of NO3- reduction by the dinuclear copper-modified molybdenum germanate crystalline material prepared in Example 1 is ammonia, and no byproducts are generated. This shows that the dinuclear copper-modified molybdenum germanate crystalline material prepared in Example 1 has excellent selectivity.

[0039] In summary: The binuclear copper-modified molybdenum germanate crystalline material prepared in Example 1, when drop-coated onto conductive carbon cloth, serves as an electrocatalyst for NO3-. - It has a strong reducing ability and excellent selectivity, making it a high-performance electrocatalyst for catalyzing NO3-. - It has great application potential as ammonia.

[0040] Example 2: This example is identical to Example 1, except that in step (1), the copper metal salt is copper acetate.

[0041] The tested ammonia production is 14.01 mg·h -1 mg cat -1 , and the faradic efficiency is 92.15%.

[0042] Example 3: This example is identical to Example 1, except that in step (1), the molar ratio of ammonium molybdate to germanium oxide is 1:0.26.

[0043] The tested ammonia production is 13.55 mg·h -1 mg cat -1 , and the faradic efficiency is 91.23%.

[0044] Example 4: This example is identical to Example 1, except that in step (1), the molar ratio of ammonium molybdate to ligand L is 1:0.04.

[0045] The tested ammonia production is 12.99 mg·h -1 mg cat -1 , and the faradic efficiency is 90.02%.

[0046] Example 5: This example is identical to Example 1, except that in step (1), the volume ratio of ammonium molybdate to distilled water is 0.1 mmol:40 mL.

[0047] The tested ammonia production is 13.98 mg·h -1 mg cat -1 , and the faradic efficiency is 93.56%.

[0048] The present application is applicable to the prior art.

Claims

1. A binuclear copper-modified molybdogermanate crystalline material, characterized in that, The molecular formula of the material is [Cu2(L)2(HL)4(H2O)2(GeMo 12 O 40 )2]·3H2O; L = 1 -(4-carboxybenzyl)-[4,4']bipyridinium chloride; the crystal system is monoclinic; the space group is P21 / n; the cell parameters are a = 18.0008(6) A, b = 20.8877(6) A, c = 20.5829(7) A, α = 90°, β = 90.2370(10)°, γ = 90°, Z = 2.

2. A method of preparing the binuclear copper-modified molybdogermanate crystalline material of claim 1, characterized in that, The method comprises the following steps: Step 1, dissolving germanium oxide, ammonium molybdate, copper salt and ligand L in water, and then adjusting the pH of the solution by using an acid regulator to obtain a reaction solution; Step 2, reacting the reaction solution in step 1 in a high-temperature sealed environment, and then cooling to room temperature after the reaction to obtain a binuclear copper-modified molybdenum germanate crystalline material.

3. The method of claim 2, wherein the method further comprises the step of: In step 1, the copper salt is copper acetate, copper sulfate or copper chloride; the ligand L is 1-(4-carboxylbenzyl)-[4,4']bipyridine chloride; and the water is deionized water or distilled water.

4. The method of claim 2, wherein the method is characterized by, In step 1, the molar ratio of ammonium molybdate to germanium oxide is 1:0.25-0.28; the molar ratio of ammonium molybdate to copper salt is 1:9-11; the molar ratio of ammonium molybdate to ligand L is 1:0.03-0.05; and the amount-of-substance ratio of ammonium molybdate to water is 1 mmol:40-60 mL.

5. The method for preparing the dual-core copper-modified molybdenum germanate crystalline material according to claim 2, characterized in that, In step 1, the dissolving process is as follows: using stirring, the temperature is normal temperature, the stirring speed is 900-1500 rpm, and the stirring time is 4-8 h.

6. The method for preparing the dinuclear copper-modified molybdenum germanate crystalline material according to claim 2, characterized in that, In step 1, the acid regulator is sulfuric acid, nitric acid or hydrochloric acid.

7. The method of claim 2, wherein the method is characterized by: In step 1, the pH of the solution is adjusted to 2.8-5.

0.

8. The method for preparing the dual-core copper-modified molybdenum germanate crystalline material according to claim 2, characterized in that, In step 2, the reaction temperature is 120-150 DEG C, and the reaction time is 6-8 days.

9. The method for preparing the dual-core copper-modified molybdenum germanate crystalline material according to claim 2, characterized in that, In step 2, the cooling rate is 8-10 DEG C / h.

10. Use of the binuclear copper-modified molybdogermanic acid crystalline material according to claim 1, characterized in that, The material is used as a raw material to prepare a modified electrode.