Antibacterial and anti-algae PP (polypropylene) composite board as well as preparation method and application thereof

By introducing antibacterial masterbatch and chopped glass fiber reinforcement layer into PP sheets, combined with nano-titanium dioxide shielding and self-cleaning layer, the safety and environmental protection issues of PP sheets in aquaculture environments are solved, achieving long-lasting antibacterial and anti-algae properties and adaptive performance, and reducing the risk of environmental pollution.

CN121973523APending Publication Date: 2026-05-05JIANGSU BIOYI ENVIRONMENTAL PROTECTION TECH CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202610173743.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-02-06
Publication Date
2026-05-05

AI Technical Summary

Technical Problem

Existing PP boards pose risks of harmful substance migration in aquaculture environments, have easily diminished antibacterial and anti-algae effects, release microplastics, cause bacterial resistance, and contribute to environmental pollution. Furthermore, they are difficult to dispose of and cannot meet the safety and environmental protection requirements of aquaculture.

Method used

The core-shell structure of the antibacterial masterbatch includes a maleic anhydride-grafted polypropylene resin shell and a core of mixed filler consisting of quaternary ammonium salt-grafted chitosan and nano zinc oxide. Combined with a chopped glass fiber reinforcement layer and a nano titanium dioxide UV shielding layer, along with a self-cleaning layer and a flexible conductive sensor, a multi-layer composite structure is formed.

Benefits of technology

It achieves long-lasting antibacterial and anti-algae properties, avoids the loss of antibacterial agents, enhances the stability and durability of the board, reduces microplastic release, lowers the risk of bacterial resistance, and improves environmental adaptability and self-cleaning ability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses an antibacterial and anti-algae PP composite board and a preparation method and application thereof.The antibacterial and anti-algae PP composite board comprises a polypropylene composite material layer, a glass fiber reinforcement layer and an antibacterial layer which are sequentially stacked, the antibacterial layer comprises antibacterial master batch, the antibacterial master batch is of a core-shell structure, a maleic anhydride grafted polypropylene resin material serves as a shell layer, and the shell layer is made of a polypropylene resin material; a mixed filler formed by quaternary ammonium salt grafted chitosan and nano zinc oxide is used as an inner core. The antibacterial and anti-algae PP composite board provided by the invention has excellent antibacterial and anti-algae capabilities, and has excellent mechanical properties and weather resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of composite material technology, specifically relating to an antibacterial and anti-algae PP composite board, its preparation method, and its application. Background Technology

[0002] In the aquaculture industry, the performance of materials used in aquaculture facilities directly affects aquaculture efficiency, the aquatic environment, and the health of farmed organisms. Polypropylene (PP) sheets have excellent corrosion resistance and strong tolerance to salt, acid and alkali substances and disinfectants in water. They are not prone to corrosion and deformation under long-term immersion conditions, effectively avoiding the inherent defects of traditional materials such as wood's easy rot and metal's easy rust and leakage. At the same time, their low surface energy characteristics can, to a certain extent, prevent dirt and algae from adhering. Therefore, they are widely used in the manufacture of aquaculture ponds, tanks, and other aquaculture facilities.

[0003] However, in actual aquaculture scenarios, the excess of nutrients such as nitrogen and phosphorus in the aquaculture water provides ample nutrients for the growth of algae and bacteria. Although traditional PP boards themselves have a certain resistance to microbial corrosion, after long-term soaking, organic debris easily accumulates on their surface and forms a biofilm. These biofilms become stable attachment points for algae and bacteria, significantly aggravating surface pollution problems. In addition, when the pH value of the aquaculture water is too high, it will inhibit the growth of beneficial algae and instead promote the reproduction of harmful algae such as blue-green algae, further worsening the surface pollution of PP boards, increasing the frequency of cleaning and maintenance costs of aquaculture facilities, and may also induce diseases in aquaculture organisms.

[0004] Among existing related patent technologies, patent CN119220022B discloses a low-temperature resistant PP composite board and its preparation method. This patent prepares a low molecular weight chain amide compound by amidation reaction of phthaloyl chloride and diethylenetriamine, and then uses (3-iodopropyl)trimethoxysilane to undergo a substitution reaction with the imine structure in the molecular chain of the compound to introduce a methoxysilane structure into the side chain, thus obtaining a low-temperature resistant additive. After introducing this low-temperature resistant additive into the PP composite board, it significantly improves the low-temperature impact resistance and creep resistance of the composite board, solving the problem of poor mechanical properties of PP boards in low-temperature environments. However, when applied to aquaculture, there are still many unresolved technical defects, specifically as follows: First, there is a risk of harmful substance migration. PP boards may release toxic substances such as antimony and phthalates in high-temperature, acidic, or oily environments such as water temperature fluctuations in aquaculture ponds and contact with feed, polluting the aquaculture water and endangering the health of aquatic animals. Moreover, these harmful substances may accumulate through the food chain over a long period of time, posing a potential threat to human health. Second, the antibacterial and anti-algae effects are easily weakened, and silver ions... Commonly used antibacterial agents such as quaternary ammonium salts gradually lose their effectiveness during use due to ultraviolet radiation, water erosion, and material aging, resulting in a shortened protection period, accelerated algae attachment and bacterial growth, increased cleaning frequency of aquaculture ponds, and increased risk of disease outbreaks. Third, there are issues with microplastic release and pollution. During long-term use, PP sheets wear down or degrade, producing micron-sized plastic fragments. These microplastics easily enter the aquaculture water and are ingested by aquatic organisms, damaging their digestive systems and accumulating toxins, while also polluting the surrounding ecological environment. Fourth, it easily leads to bacterial resistance and secondary pollution. Long-term use of a single antibacterial agent may induce drug resistance in common aquaculture microorganisms such as Aeromonas hydrophila, reducing the effectiveness of disease control. Furthermore, the leaching of ineffective antibacterial agents can create chemical pollution, further deteriorating the aquatic environment and increasing aquaculture costs. Fifth, waste disposal is difficult and carries a heavy environmental burden. PP sheets are difficult to degrade naturally after their lifespan ends, and discarded sheets containing antibacterial agents may release residual toxins, polluting soil and water sources, exacerbating plastic pollution problems, violating relevant environmental regulations, and increasing waste disposal costs for enterprises.

[0005] Therefore, developing a PP board technology that is suitable for aquaculture environments and has both safety and environmental protection characteristics as well as long-lasting antibacterial and antifouling properties has become an urgent technical need to be addressed in the field of aquaculture facility materials. Summary of the Invention

[0006] In view of the shortcomings of the prior art, the purpose of this invention is to provide an antibacterial and anti-algae PP composite board, its preparation method and application.

[0007] To achieve this objective, the present invention adopts the following technical solution: In a first aspect, the present invention provides an antibacterial and anti-algae PP composite board, comprising a polypropylene composite material layer, a glass fiber reinforcement layer and an antibacterial layer stacked sequentially, wherein the antibacterial layer comprises an antibacterial masterbatch, the antibacterial masterbatch having a core-shell structure, with maleic anhydride-grafted polypropylene resin material as the shell layer and a mixed filler formed by quaternary ammonium salt-grafted chitosan and nano zinc oxide as the core.

[0008] In this invention, a composite antibacterial system composed of quaternary ammonium salt grafted chitosan and nano zinc oxide is introduced, which has both organic and inorganic antibacterial properties. At the same time, the quaternary ammonium salt and chitosan are introduced through chemical grafting, which forms a stable bond between the quaternary ammonium salt and chitosan, improving the stability of the antibacterial system during long-term immersion in water, thereby avoiding the problem of the decline in the antibacterial effect of the board due to the loss of antibacterial agent. In addition, this invention introduces maleic anhydride grafted polypropylene, which can further delay the erosion of environmental water bodies and ensure the durability and stability of the antibacterial effect of the board.

[0009] Meanwhile, the polypropylene introduced in this invention is maleic anhydride-grafted polypropylene, which can further improve the compatibility between polypropylene resin and mixed filler.

[0010] Preferably, based on the total mass of the components of the antibacterial masterbatch as 100%, the mass percentage of the maleic anhydride-grafted polypropylene resin is 60-80 wt%, such as 60 wt%, 65 wt%, 70 wt%, 75 wt%, 80 wt%, etc., preferably 70 wt%.

[0011] The method for preparing the antibacterial masterbatch includes: mixing maleic anhydride-grafted polypropylene resin and mixed fillers, melt extruding, and granulating to obtain an antibacterial masterbatch with a particle size D50 of 5-15 μm.

[0012] Maleic anhydride-grafted polypropylene resin and mixed filler are melt-extruded. During the melt extrusion process, the maleic anhydride-grafted polypropylene flows and coats the mixed filler. The anhydride groups contained therein react with the amino / hydroxyl groups of chitosan to enhance the interfacial compatibility between the two, thereby enhancing the dispersibility of the mixed filler.

[0013] Preferably, the melt extrusion is performed using a screw extruder, the parameters of which include: Zone 1 170-175℃, for example 170℃, 171℃, 172℃, 173℃, 174℃, 175℃, etc.; Zone 2 175-180℃, for example 175℃, 176℃, 177℃, 178℃, 179℃, 180℃, etc.; Zone 3 185-195℃, for example... Temperature ranges include 185℃, 186℃, 188℃, 190℃, 192℃, 193℃, and 195℃; four zones range from 195-200℃, such as 195℃, 196℃, 197℃, 198℃, 199℃, and 200℃; the machine head ranges from 190-195℃, such as 190℃, 191℃, 192℃, 193℃, 194℃, and 195℃; and the speed ranges from 200-240 rpm, such as 200 rpm, 205 rpm, 210 rpm, 215 rpm, 220 rpm, 225 rpm, 230 rpm, 235 rpm, and 240 rpm.

[0014] Preferably, the particle size D50 of the antibacterial masterbatch is 5-15 μm, such as 5 μm, 6 μm, 8 μm, 10 μm, 12 μm, 15 μm, etc.

[0015] In this invention, the test method for particle size D50 is: laser particle size analyzer method (dry method).

[0016] Preferably, the preparation method of the mixed filler includes: quaternary ammonium salt grafted chitosan and nano zinc oxide are mixed in the presence of ethanol at a mass ratio of (2-5):1 for 0.5-1 h to obtain the mixed filler.

[0017] Preferably, the mass ratio of the quaternary ammonium salt grafted chitosan to nano zinc oxide is (2-5):1, such as 2:1, 2.5:1, 3:1, 3.5:1, 4:1, 4.5:1, 5:1, etc.

[0018] Preferably, the mixing time is 0.5-1 h, for example 0.5 h, 0.6 h, 0.7 h, 0.8 h, 0.9 h, 1 h, etc.

[0019] Preferably, the amount of ethanol used is 30-50% of the total mass of the mixed filler, for example, 30%, 35%, 40%, 45%, 50%, etc.

[0020] In this invention, ethanol is added as a dispersant during the preparation of the mixed packing. Although the mixed packing is removed by vacuum drying after preparation, the surface of the mixed packing is optimized by ethanol treatment.

[0021] In the preparation method of the mixed filler provided by the present invention, the mixing is carried out in a high-speed mixer. In the high-speed mixer, the shear force can effectively break up the agglomerates of the mixed filler or maleic anhydride-grafted polypropylene resin. Under the shear force and centrifugal motion of the high-speed mixer, the polar groups (such as maleic anhydride groups) of the maleic anhydride-grafted polypropylene resin come into full contact with the mixed filler. Through interfacial interactions such as hydrogen bonding or polar adsorption, the dispersion stability is further improved and phase separation is reduced.

[0022] In this invention, ethanol is used as a volatile organic solvent. To avoid problems such as bubbles, thermal degradation, or performance decline during subsequent processing, the ethanol needs to be removed. The ethanol removal step is performed after the preparation of the mixed packing material. The method includes: placing the wet mixed packing material at 50-60°C, such as 50°C, 52°C, 55°C, 58°C, 60°C, etc., under a vacuum of 0.08-0.1 MPa, such as 0.08 MPa, 0.09 MPa, 0.1 MPa, etc., and drying for 1-2 hours, such as 1 hour, 1.2 hours, 1.5 hours, 1.8 hours, 2 hours, etc., to remove the ethanol.

[0023] The preparation method of the quaternary ammonium salt grafted chitosan includes: Chitosan solution and glycidyltrimethylammonium chloride were mixed at a mass ratio of 1:(1-3) and reacted at 60-80℃ for 2-3 h. After the reaction, the pH was adjusted to neutral to precipitate the quaternary ammonium salt-grafted chitosan, thus obtaining the quaternary ammonium salt-grafted chitosan.

[0024] Preferably, the mass ratio of chitosan to quaternary ammonium salt is 1:(1-3), such as 1:1, 1:1.5, 1:2, 1:2.5, 1:3, etc., and preferably 1:2.

[0025] Preferably, the reaction temperature is 60-80℃, such as 60℃, 65℃, 70℃, 75℃, 80℃, etc., and the time is 2-3 h, such as 2 h, 2.2 h, 2.5 h, 2.8 h, 3 h, etc.

[0026] As a preferred embodiment of the present invention, the method for preparing the antibacterial masterbatch includes: S1. Add chitosan powder to acetic acid solution and stir until completely dissolved to obtain chitosan solution with a chitosan concentration of 1-10 wt%. S2. According to the mass ratio of chitosan to quaternary ammonium salt of 1:(1-3), quaternary ammonium salt is added to chitosan solution and reacted at 60-80℃ for 2-3 h to obtain quaternary ammonium salt grafted chitosan solution. Sodium hydroxide solution is added to adjust the pH to neutral to precipitate quaternary ammonium salt grafted chitosan. Then, after filtration, washing with deionized water and vacuum drying, quaternary ammonium salt grafted chitosan solid is obtained. S3. Weigh out the quaternary ammonium salt-grafted chitosan and nano zinc oxide according to the mass ratio of quaternary ammonium salt-grafted chitosan and nano zinc oxide (2-5):1, put them into a high-speed mixer, add 30-50% ethanol and stir at high speed for 0.5-1h to mix. S4. After mixing, place the mixture in an environment of 50-60℃ and vacuum degree of 0.08-0.1 MPa to dry for 1-2 h to remove ethanol and obtain the mixed packing material; S5. Maleic anhydride-grafted polypropylene resin particles and mixed fillers are added to a high-speed mixer at a mass ratio of (6-8):(4-2) for dry mixing. The mixed material is then fed into a twin-screw extruder for melt extrusion. The melt extrusion is carried out using a screw extruder with the following parameters: Zone 1 170-175℃, Zone 2 175-180℃, Zone 3 185-195℃, Zone 4 195-200℃, Die head 190-195℃, and Rotation speed 200-240 rpm. Granulation and drying are performed to obtain antibacterial masterbatch with a particle size of 5-15μm.

[0027] This invention uses quaternary ammonium salt grafted with chitosan to form organic antibacterial agents and nano zinc oxide to form inorganic antibacterial agents in the antibacterial layer, replacing the single antibacterial agent used in the prior art. The stable bond formed by quaternary ammonium salt and chitosan reduces the dissolution rate of antibacterial agents when the board is soaked in water, thereby avoiding the problem of antibacterial effect decay caused by antibacterial agent inactivation during long-term soaking.

[0028] Meanwhile, the outer layer of the composite antibacterial system composed of quaternary ammonium salt-grafted chitosan and nano zinc oxide is coated with maleic anhydride-grafted polypropylene, which can delay the erosion of the antibacterial system by the environment, thereby improving the antibacterial effect and duration of PP composite board in water.

[0029] Furthermore, during the preparation process, the agglomeration of nanoparticles was avoided by adding ethanol and mixing with a high-speed mixer, so that the mixed filler could be uniformly dispersed in maleic anhydride-grafted polypropylene resin. Grafting maleic anhydride with polypropylene resin improved the compatibility between the resin and the mixed filler. Subsequently, gradient temperature control was used to avoid local overheating during the extrusion of antibacterial layer particles, thereby improving the stability of the extrusion of antibacterial layer particles.

[0030] Preferably, the glass fiber reinforced layer comprises chopped glass fibers and ethylene-ethyl acetate copolymer, and the chopped glass fibers have a mass percentage content of 50-80 wt%, such as 50 wt%, 55 wt%, 60 wt%, 65 wt%, 70 wt%, 75 wt%, 80 wt%, etc., based on the total mass of the components of the glass fiber modified layer as 100%.

[0031] The length of the chopped glass fiber is 1-5 mm, such as 1 mm, 2 mm, 3 mm, 4 mm, 5 mm, etc., and the vinyl acetate content in the ethylene-ethyl acetate copolymer is 18-40%, such as 18%, 20%, 25%, 30%, 35%, 40%, etc.

[0032] Compared to not introducing glass fibers or introducing long glass fibers, the present invention avoids the disadvantages of local stress concentration caused by long fibers by introducing short glass fibers into the glass fiber reinforcement layer. At the same time, the glass fibers introduced in the present invention are preferably 1-3 mm in length, which can avoid the formation of burrs on the surface of the glass fiber reinforcement layer particles.

[0033] Meanwhile, the ethylene-vinyl acetate copolymer preferred in this invention has flexible molecular chains that can effectively absorb and disperse impact energy. The composite structure constructed with rigid chopped glass fibers combines bending strength and impact toughness, overcoming the inherent defect of traditional boards where adding long fibers to increase strength leads to increased material brittleness. Furthermore, the ethylene-vinyl acetate polar groups in the ethylene-vinyl acetate copolymer of this invention can form hydrogen bonds with the silanol groups on the surface of the chopped glass fibers. Moreover, the ethylene-vinyl acetate copolymer and the maleic anhydride-grafted polypropylene resin in the antibacterial layer not only have excellent compatibility, but can also form hydrogen bonds between them. Therefore, the glass fiber reinforcement layer and the antibacterial layer of this invention have excellent bonding strength, which can prevent the subsequent multilayer boards from delamination and eliminate the risk of water leakage.

[0034] Furthermore, the chopped glass fibers have the function of blocking ultraviolet rays, and the acetate-vinyl groups in the ethylene-vinyl acetate copolymer can capture free radicals. The synergistic effect of the two can delay the oxidative aging process of the board, thereby improving the environmental adaptability and durability of the PP composite board.

[0035] As a preferred embodiment of the present invention, the method for preparing the granules for the glass fiber reinforcement layer includes: Based on the total mass of the components of the glass fiber reinforcement layer being 100%, the chopped glass fiber has a mass percentage content of 50-80 wt%. The chopped glass fiber and ethylene-vinyl acetate copolymer are mixed in a high-speed mixer at 50°C at 200-500 rpm, and then fed into a twin-screw extruder for melt extrusion and granulation. The parameters include: zone 1 temperature: 120-130°C, zone 2 temperature: 140-150°C, zone 3 temperature: 160-170°C, zone 4 temperature: 150-160°C, die head temperature: 140-150°C, and rotation speed: 100-300 rpm, to obtain granules for the glass fiber reinforcement layer.

[0036] This invention uses chopped glass fibers with a length of 1-3 mm instead of unreinforced or long glass fibers during the preparation of the glass fiber reinforcement layer. This avoids localized stress concentration caused by long fibers and prevents burrs from appearing on the surface of the glass fiber reinforcement layer particles. The ethylene-vinyl acetate copolymer used has an acetate-ethylene content of 18-40%, which absorbs impact energy through the flexibility of the molecular chains, thereby forming a composite structure of rigid fibers and a flexible network. This improves the flexural strength and impact toughness of the glass fiber reinforcement layer, avoiding the defect of adding long fibers to traditional boards to increase toughness and strength, but which also increases the brittleness of the board. The polar acetate-vinyl groups of the ethylene-vinyl acetate copolymer can form hydrogen bonds with the silanol groups on the surface of the chopped glass fibers, avoiding subsequent... In the preparation of multilayer boards, defects such as glass fiber precipitation occur. At the same time, the ethylene-vinyl acetate copolymer and the maleic anhydride-grafted polypropylene resin in the antibacterial layer can form hydrogen bonds, and have excellent compatibility with the compatibilizer of the polypropylene composite layer. Therefore, the glass fiber reinforced layer of this invention has excellent bonding strength with both the antibacterial layer and the polypropylene composite layer, which can avoid water leakage caused by delamination. By blocking ultraviolet penetration with short-cut glass fibers and capturing free radicals with the vinyl acetate groups in the ethylene-vinyl acetate copolymer to delay the oxidation of the board, the service life of the antibacterial layer in the water environment is further extended, and the adaptability and service life of the finished board in the water environment are improved.

[0037] Preferably, the polypropylene composite material layer comprises 25-50 parts polypropylene resin, 5-15 parts nano silica, 1-5 parts compatibilizer, 0.6-1 part antioxidant, and 0.2-2 parts light stabilizer. The polypropylene resin 25-50 parts can be 25 parts, 30 parts, 35 parts, 40 parts, 45 parts, 50 parts, etc.; the nano silica 5-15 parts can be 5 parts, 6 parts, 8 parts, 10 parts, 12 parts, 15 parts, etc.; the compatibilizer 1-5 parts can be 1 part, 2 parts, 3 parts, 4 parts, 5 parts, etc.; the antioxidant 0.6-1 part can be 0.6 parts, 0.7 parts, 0.8 parts, 0.9 parts, 1 part, etc.; and the light stabilizer 0.2-2 parts can be 0.2 parts, 0.5 parts, 0.8 parts, 1 part, 1.2 parts, 1.5 parts, 1.6 parts, 1.8 parts, 2 parts, etc.

[0038] The compatibilizer includes maleic anhydride-grafted polypropylene, the antioxidant includes antioxidant 1010, and the light stabilizer includes hindered amine light stabilizers.

[0039] The polypropylene composite material layer defined in this invention uses polypropylene resin and nano-titanium dioxide as the main raw materials. The nano-titanium dioxide forms a highly efficient ultraviolet shielding layer in the polypropylene composite material layer. It works synergistically with antioxidant 1010 and hindered amine light stabilizer to inhibit the oxidation and decomposition process of the board and improve the board's resistance to ultraviolet rays and water erosion in the aquatic environment. At the same time, the nano-titanium dioxide can decompose organic matter under photocatalysis, so that algae and bacteria attached to the surface of the board can be automatically removed.

[0040] Furthermore, by using maleic anhydride-grafted polypropylene as a compatibilizer, the present invention improves the dispersibility of nano-titanium dioxide in polypropylene resin and prevents the aggregation of nanoparticles.

[0041] Furthermore, the preferred resin for the polypropylene composite layer in this invention is polypropylene resin, which has weak van der Waals forces with the ethylene-vinyl acetate copolymer. At the same time, the introduction of maleic anhydride-grafted polypropylene compatibilizer enables a strong bond between the polypropylene composite layer and the glass fiber reinforcement layer, thus preventing delamination of the board during application.

[0042] As a preferred embodiment of the present invention, the method for preparing the granules for the polypropylene composite material layer includes: The polypropylene resin, nano titanium dioxide, compatibilizer, antioxidant and light stabilizer are uniformly mixed in the formula and then added to a twin-screw extruder. The parameters of the twin-screw extruder are controlled as follows: Zone 1 160-180℃, Zone 2 190-200℃, and Die head 200-210℃. Melt extrusion and granulation are carried out to obtain polypropylene composite material granules.

[0043] The polypropylene composite material layer provided by this invention uses nano-titanium dioxide and polypropylene resin as the main raw materials. Nano-titanium dioxide can not only form an ultraviolet shielding layer, but also photocatalytically decompose organic matter, enabling the automatic removal of algae and bacteria on the surface of the board, thus preventing algae and bacteria from attaching and harming aquatic organisms. At the same time, antioxidant 1010 and hindered amine light stabilizer inhibit the oxidative decomposition of the polypropylene composite material layer, thereby improving the board's resistance to ultraviolet radiation and water erosion in water. The surface smoothness of the polypropylene resin grafted with maleic anhydride is improved, making it difficult for pollutants to adhere to the board surface. Meanwhile, the maleic anhydride-grafted polypropylene acts as a compatibilizer to improve the dispersibility of nano-titanium dioxide in the polypropylene resin, preventing the agglomeration of nano-titanium dioxide, thereby improving the impact strength of the polypropylene composite material layer.

[0044] Preferably, the thickness of the antibacterial layer is 10-50 μm, such as 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, etc.; the thickness of the glass fiber reinforced layer is 100-500 μm, such as 100 μm, 150 μm, 200 μm, 250 μm, 300 μm, 350 μm, 400 μm, 450 μm, 500 μm, etc.; and the thickness of the polypropylene composite material layer is 50-200 μm, such as 50 μm, 80 μm, 100 μm, 120 μm, 150 μm, 180 μm, 200 μm, etc.

[0045] Preferably, the antibacterial and anti-algae PP composite board further includes a flexible conductive sensor, which is located between the glass fiber reinforcement layer and the antibacterial layer. The thickness of the conductive sensor is 10-100 μm, such as 10 μm, 20 μm, 30 μm, 50 μm, 60 μm, 80 μm, 90 μm, 100 μm, etc.

[0046] This invention embeds a flexible conductive sensor between the glass fiber reinforcement layer and the antibacterial layer and then performs hot pressing molding. The flexible conductive sensor monitors the algae attachment on the surface of the board in real time and issues an early warning when there is too much algae, thereby realizing intelligent management of the board.

[0047] The antibacterial and anti-algae PP composite board also includes a self-cleaning layer. The self-cleaning layer is located on the side of the polypropylene composite material layer away from the glass fiber reinforcement layer. The thickness of the self-cleaning layer is 5-10 μm, such as 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, etc. The components of the self-cleaning layer include heptadecafluorodecyltriethoxysilane, nano-silica, and polydimethylsiloxane. The mass ratio of heptadecafluorodecyltriethoxysilane, nano-silica, and polydimethylsiloxane is (12-15):(8-10):(5-8). The 12-15 can be 12, 13, 14, 15, etc., the 8-10 can be 8, 8.5, 9, 9.5, 10, etc., and the 5-8 can be 5, 5.5, 6, 6.5, 7, 7.5, 8, etc.

[0048] This invention improves the hydrophobicity of the board surface by setting a self-cleaning layer on the outermost layer. The self-cleaning layer forms a micro-nano composite structure through chemical bonding, which reduces the basis for microbial adhesion. Furthermore, the nano-silica contained in the self-cleaning layer can further increase the mechanical durability of the coating.

[0049] As a preferred embodiment of the present invention, the slurry for the self-cleaning layer comprises: Heptadecafluorodecyltriethoxysilane, nano-silica, and polydimethylsiloxane were dissolved in anhydrous ethanol at a mass ratio of (12-15):(8-10):(5-8), and 0.5 wt% acetic acid was added. The mixture was then ultrasonically dispersed at 300 W for 30 min to obtain a slurry for a self-cleaning layer.

[0050] In this invention, a flexible conductive sensor is embedded between the glass fiber reinforcement layer and the antibacterial layer to monitor algae adhering to the board surface. This allows for timely warnings when excessive algae accumulate. Furthermore, a self-cleaning layer is sprayed onto the board surface using a slurry. Through chemical bonding and the formation of a micro-nano composite structure, the hydrophobicity of the board surface is enhanced, thereby reducing microbial adhesion. The nano-silica contained in the self-cleaning layer further improves the mechanical durability of the board coated with this layer. This avoids the problem of frequent cleaning due to algae adhesion and bacterial growth on the board surface, reducing the use of human resources.

[0051] In this invention, the antibacterial layer possesses excellent antibacterial properties, while the glass fiber reinforcement layer, by introducing chopped glass fibers, enhances the tensile strength, flexural strength, and modulus of the board. This allows the board to adapt to varying water pressures and currents at different depths, making it less prone to deformation and breakage during collisions with aquatic organisms. The elastomeric properties of the ethylene-vinyl acetate copolymer absorb impact energy, preventing breakage due to impact or stress in low-temperature water environments. Furthermore, during the hot-pressing of the glass fiber reinforcement layer and the polypropylene composite layer, the ethylene-vinyl acetate copolymer and polypropylene exhibit good compatibility, preventing delamination. The nano-titanium dioxide exhibits strong photocatalytic activity under light irradiation, enabling the board to decompose organic matter and kill bacteria in the water when exposed to light. The bacteria and algae attached to the surface of the board are killed, while nano-titanium dioxide, as an ultraviolet shielding agent, can reflect and scatter UV light. Hindered amine light stabilizer captures free radicals through chemical action, and antioxidant 1010 prevents oxidation chain reaction. The synergistic effect of nano-titanium dioxide, antioxidant 1010 and hindered amine light stabilizer can improve the environmental adaptability of the board and prevent the board from degrading, yellowing and embrittlement due to ultraviolet radiation in sunlight. The maleic anhydride anhydride group of maleic anhydride grafted polypropylene can chemically react with the polar groups on the molecular chain of ethylene-vinyl acetate copolymer in glass fiber reinforcement layer. At the same time, the polypropylene resin segments of glass fiber reinforcement layer are completely compatible with the polypropylene resin matrix of polypropylene composite layer, and no delamination will occur during interlayer pressing.

[0052] In a second aspect, the present invention provides a method for preparing an antibacterial and anti-algae PP composite board as described in the first aspect, the method comprising: (1) The polypropylene composite material layer, the glass fiber reinforcement layer and the antibacterial layer are stacked in sequence and hot-pressed at 175-185℃ and 8-10MPa for 15-20 min to obtain the antibacterial and anti-algae PP composite board.

[0053] Preferably, the hot pressing temperature is 175-185℃, such as 175℃, 177℃, 178℃, 180℃, 182℃, 185℃, etc., and the pressure is preferably 8-10 MPa, such as 8 MPa, 8.2 MPa, 8.5 MPa, 9 MPa, 9.2 MPa, 9.5 MPa, 9.8 MPa, 10 MPa, etc., and the time is preferably 15-20 min, such as 15 min, 16 min, 17 min, 18 min, 19 min, 20 min, etc.

[0054] Preferably, the preparation method further includes: placing a flexible conductive sensor between the glass fiber reinforcement layer and the antibacterial layer, and then performing lamination and hot pressing; The preparation method further includes: adding 0.1-1 wt% acetic acid (e.g., 0.1 wt%, 0.2 wt%, 0.4 wt%, 0.5 wt%, 0.6 wt%, 0.8 wt%, 1 wt%, etc.) to the ethanol slurry of the self-cleaning layer, mixing it, coating it on the surface of the polypropylene composite material layer, and drying it to obtain the self-cleaning layer.

[0055] Preferably, the polypropylene composite material layer and the antibacterial layer are obtained by injection molding of granules to form a sheet, and the glass fiber reinforced layer is obtained by hot pressing of granules at high temperature to form a sheet.

[0056] Preferably, the preparation method of the polypropylene composite material layer includes: injection molding the polypropylene composite material layer using granules to obtain the polypropylene composite material layer. The injection molding parameters include: injection temperature: 190-195℃, such as 190℃, 191℃, 192℃, 193℃, 194℃, 195℃, etc.; injection pressure: 70-80 MPa, such as 70 MPa, 72 MPa, 75 MPa, 78 MPa, 80 MPa, etc.; holding pressure: 50 MPa; holding time: 8 s; mold temperature: 70-75℃, such as 70℃, 71℃, 72℃, 73℃, 74℃, 75℃, etc.; and cooling time: 25-35 s, such as 25 s, 26 s, 28 s, 30 s, 32 s, 34 s, 35 s, etc.

[0057] Preferably, the method for preparing the glass fiber reinforced layer includes: hot pressing the glass fiber reinforced layer with granules to obtain the glass fiber reinforced layer. The parameters of the hot pressing include: preheating temperature: 140-150℃ / 2min, such as 140℃, 142℃, 145℃, 146℃, 148℃, 150℃, etc.; hot pressing temperature: 140-150℃, such as 140℃, 142℃, 145℃, 146℃, 148℃, 150℃, etc.; pressure: 8-10 MPa, such as 8 MPa, 8.5 MPa, 9 MPa, 9.5 MPa, 10 MPa, etc.; holding time: 8min; and cooling method: water cooling to 50℃ for demolding.

[0058] Preferably, the method for preparing the antibacterial layer includes: injection molding an antibacterial masterbatch to obtain the antibacterial layer, wherein the injection molding parameters include: injection temperature: 165-170℃, such as 165℃, 166℃, 167℃, 168℃, 169℃, 170℃, etc.; injection pressure: 80-100 MPa, such as 80 MPa, 85 MPa, 90 MPa, 95 MPa, 100 MPa, etc.; holding pressure / time: 60MPa / 5sd; mold temperature: 50-60℃, such as 50℃, 52℃, 55℃, 56℃, 58℃, 60℃, etc.; and cooling time: 20-30 s, such as 20 s, 22 s, 24 s, 25 s, 26 s, 28 s, 30 s, etc.

[0059] Thirdly, the present invention provides an application of the antibacterial and anti-algae PP composite board as described in the first aspect in aquaculture.

[0060] Compared with the prior art, the present invention has the following beneficial effects: (1) The antibacterial masterbatch provided by the present invention has a double-layer structure, with the core being quaternary ammonium salt grafted chitosan and nano zinc oxide, which can achieve the combination of organic antibacterial and inorganic antibacterial. At the same time, maleic anhydride grafted polypropylene resin is used as the outer layer to protect the antibacterial agent, avoiding the disadvantage of rapid decay of the antibacterial effect of the board due to long-term soaking, and realizing the long-term antibacterial function of the board. (2) The present invention constructs a composite glass fiber reinforcement layer by designing short glass fibers and ethylene-vinyl acetate copolymer. The short glass fibers provide rigid support, and the ethylene-vinyl acetate copolymer provides a flexible network, thereby enhancing the interfacial bonding force and avoiding the problem of delamination and leakage of the board leading to the failure of the antibacterial agent. (3) This invention incorporates nano-titanium dioxide and nano-carbon dioxide into polypropylene to shield ultraviolet light and catalyze the decomposition of organic matter, algae and bacteria. At the same time, maleic anhydride-grafted polypropylene can improve interfacial compatibility and avoid delamination, thus realizing the function of the board adapting to the water environment and avoiding the problem of board damage and reduced antibacterial performance caused by changes in the water environment. (4) By introducing a self-cleaning layer, the present invention can further improve the environmental adaptability of the board material; (5) This invention achieves the function of intelligent monitoring of the board surface by embedding a flexible conductive sensor between the glass fiber reinforcement layer and the antibacterial layer and monitoring the adhering substances on the board surface through the flexible conductive sensor. At the same time, by introducing a self-cleaning layer, the frequent manual cleaning of the board can be avoided. Detailed Implementation

[0061] The technical solution of the present invention will be further illustrated below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely illustrative of the present invention and should not be construed as limiting the invention in any way.

[0062] Unless otherwise specified, the raw materials involved in the following specific embodiments of the present invention are all conventional materials in the art, and can be purchased from commercially available products. Some raw material information is as follows: Maleic anhydride-grafted polypropylene resin: purchased from LyondellBasell, model Y1300; Chitosan: Purchased from Qingdao Haihui Biotechnology, model CS-90; Nano zinc oxide: purchased from Evonik Germany, model number Zano@20; Chopped fiberglass: Purchased from China Jushi, model ECK13-4.5-508A; Ethylene-ethyl acetate copolymer: purchased from Formosa Plastics, model number UL00328; Polypropylene resin: purchased from CNPC, model 1100N; Nano titanium dioxide: purchased from Chemours, model P25; Light stabilizer: purchased from BASF, model Tinuvin® 770; Nano silica: purchased from Evonik, model Aerosil® 200; Polydimethylsiloxane: purchased from Dow Corning, model number SYLGARD®184; Flexible conductive sensor: 20 μm thick, purchased from Hanwei Technology, model FPS-100A.

[0063] Example 1 This embodiment provides an antibacterial and anti-algae PP composite board, comprising a self-cleaning layer (5 μm), a polypropylene composite material layer (100 μm), a glass fiber reinforcement layer (300 μm), and an antibacterial layer (30 μm) stacked sequentially. A flexible conductive sensor is disposed between the glass fiber reinforcement layer and the antibacterial layer. The preparation method is as follows: (1) Preparation of antimicrobial masterbatch for antimicrobial layer Chitosan powder was added to acetic acid solution and stirred until completely dissolved to obtain a chitosan solution (chitosan concentration 5 wt%). Quaternary ammonium salt was added to the chitosan solution at a ratio of 2:1, with continuous stirring. The reaction was carried out at 60℃ for 3 hours to obtain a quaternary ammonium salt-grafted chitosan solution. The pH of the quaternary ammonium salt-grafted chitosan solution was adjusted to neutral by adding 0.1 M sodium hydroxide aqueous solution, causing the quaternary ammonium salt-grafted chitosan to precipitate. After filtration, washing with deionized water, and vacuum drying, solid quaternary ammonium salt-grafted chitosan was obtained. Quaternary ammonium salt-grafted chitosan and nano-zinc oxide were weighed at a weight ratio of 2:1 and placed in a high-speed mixer. Ethanol (40% of the total mass of the mixed filler) was added and stirred at high speed for 1 hour to obtain a wet mixed filler. The mixed filler was then dried in an environment of 55℃ and 0.1 MPa vacuum for 1.5 hours to remove the ethanol. Maleic anhydride-grafted polypropylene resin and mixed fillers were added to a high-speed mixer at a mass ratio of 7:3 for dry mixing. The mixed material was then fed into a twin-screw extruder for melt extrusion. The melt extrusion was carried out using a screw extruder with the following parameters: zone 1 170℃, zone 2 175℃, zone 3 185℃, zone 4 195℃, die head 190℃, and rotation speed of 200 rpm. Granulation was performed to obtain antibacterial masterbatch with a particle size D50 of 10 μm.

[0064] (2) Granules for preparing glass fiber reinforced layers Short-cut glass fibers and ethylene-ethyl acetate copolymer were mixed at a mass ratio of 5:2 in a high-speed mixer at 50°C and 300 rpm. The mixture was then fed into a twin-screw extruder and melt-extruded at controlled temperatures of 120°C, 140°C, 160°C, 150°C, and 145°C, and at a speed of 200 rpm to obtain granules for glass fiber reinforcement layers.

[0065] (3) Preparation of granules for polypropylene composite layer 30 parts of polypropylene resin, 5 parts of nano titanium dioxide, 2 parts of compatibilizer, 1 part of antioxidant 1010 and 0.5 parts of light stabilizer were uniformly mixed and then added to a twin-screw extruder. The temperature of the twin-screw extruder was controlled at 160℃, 190℃ and 200℃ for melt extrusion and granulation to obtain granules for polypropylene composite material layers.

[0066] (4) Preparation of slurry for self-cleaning layer Heptadecafluorodecyltriethoxysilane, nano-silica, and polydimethylsiloxane were dissolved in anhydrous ethanol in a ratio of 12:8:5. 0.5 wt% acetic acid was added, and the mixture was ultrasonically dispersed at 300 W for 30 min to obtain a slurry for a self-cleaning layer.

[0067] (5) Preparation of antibacterial and anti-algae PP composite board The antibacterial masterbatch was vacuum dried at 60℃ for 4 h to ensure that the moisture content of the antibacterial masterbatch was less than 0.1%. The antibacterial masterbatch, which was melted at 165℃, was injected into the mold at 90 MPa pressure and held at 60 MPa pressure for 5 s. The mold temperature was then reduced to 55℃ and cooled for 25 s before demolding to obtain the antibacterial layer. The glass fiber reinforced layer is laid in a mold with granules, preheated at 145°C for 2 min to soften, the pressure is increased to 9 MPa, held for 8 min, and then cooled to 50°C by water to demold and obtain the glass fiber reinforced layer board. Polypropylene composite material granules are placed in the barrel of an injection molding machine and heated to 190°C to melt and plasticize. They are then injected into the mold at a pressure of 70 MPa, held at 50 MPa for 8 seconds, and the mold is kept at a constant temperature of 70°C. After cooling for 25 seconds, the polypropylene composite material layer is demolded to obtain the polypropylene composite material layer. Then, the polypropylene composite layer, the glass fiber reinforcement layer, and the antibacterial layer are stacked in sequence, and the flexible conductive sensor is placed between the glass fiber reinforcement layer and the antibacterial layer. The mixture is then hot-pressed at 175℃ and 10 MPa for 20 minutes and then cooled. After cooling to room temperature, the self-cleaning layer is sprayed onto the surface with a slurry to a thickness of 5 μm, and then dried to obtain the antibacterial and anti-algae PP composite board.

[0068] Example 2 This embodiment provides an antibacterial and anti-algae PP composite board, comprising a self-cleaning layer (8 μm), a polypropylene composite material layer (50 μm), a glass fiber reinforcement layer (100 μm), and an antibacterial layer (10 μm) stacked sequentially. A flexible conductive sensor is disposed between the glass fiber reinforcement layer and the antibacterial layer. The preparation method is as follows: (1) Preparation of antimicrobial masterbatch for antimicrobial layer Chitosan powder was added to acetic acid solution and stirred until completely dissolved to obtain a chitosan solution (chitosan concentration 1 wt%). Quaternary ammonium salt was added to the chitosan solution at a ratio of 1:1, with continuous stirring. The reaction was carried out at 70℃ for 2.5 h to obtain a quaternary ammonium salt-grafted chitosan solution. The pH of the quaternary ammonium salt-grafted chitosan solution was adjusted to neutral by adding 0.1 M sodium hydroxide aqueous solution, causing the quaternary ammonium salt-grafted chitosan to precipitate. After filtration, washing with deionized water, and vacuum drying, solid quaternary ammonium salt-grafted chitosan was obtained. Quaternary ammonium salt-grafted chitosan and nano-zinc oxide were weighed at a weight ratio of 4:1 and placed in a high-speed mixer. Ethanol (30% of the total mass of the mixed filler) was added and stirred at high speed for 1 h to obtain a wet mixed filler. The mixed filler was then dried in a 50℃, 0.1 MPa vacuum environment for 2 h to remove the ethanol. Maleic anhydride-grafted polypropylene resin and mixed fillers were added to a high-speed mixer at a mass ratio of 6:4 for dry mixing. The mixed material was then fed into a twin-screw extruder for melt extrusion. The melt extrusion was carried out using a screw extruder with the following parameters: Zone 1 175℃, Zone 2 180℃, Zone 3 195℃, Zone 4 200℃, Die head 195℃, and Rotation speed 240 rpm. Granulation was performed to obtain antibacterial masterbatch with a particle size D50 of 5 μm.

[0069] (2) Granules for preparing glass fiber reinforced layers Short-cut glass fibers and ethylene-ethyl acetate copolymer were mixed at a mass ratio of 8:2 in a high-speed mixer at 50°C and 200 rpm. The mixture was then fed into a twin-screw extruder and melt-extruded at temperatures of 130°C, 150°C, 170°C, 160°C, and 140°C and a speed of 300 rpm to obtain granules for glass fiber reinforcement layers.

[0070] (3) Preparation of granules for polypropylene composite layer 25 parts of polypropylene resin, 10 parts of nano titanium dioxide, 1 part of compatibilizer, 0.6 parts of antioxidant 1010 and 0.2 parts of light stabilizer were uniformly mixed and then added to a twin-screw extruder. The temperature of the twin-screw extruder was controlled at 180℃, 200℃ and 210℃ for melt extrusion and granulation to obtain granules for polypropylene composite material layers.

[0071] (4) Preparation of slurry for self-cleaning layer Heptadecafluorodecyltriethoxysilane, nano-silica, and polydimethylsiloxane were dissolved in anhydrous ethanol in a ratio of 15:10:8. 0.5 wt% acetic acid was added, and the mixture was ultrasonically dispersed at 300 W for 30 min to obtain a slurry for a self-cleaning layer.

[0072] (5) Preparation of antibacterial and anti-algae PP composite board The antibacterial masterbatch was vacuum dried at 60℃ for 4 h to ensure that the moisture content of the antibacterial masterbatch was less than 0.1%. The antibacterial masterbatch, which was melted at 165℃, was injected into the mold at 100MPa pressure. The mold was held at 60MPa pressure for 5 s, and the mold temperature was reduced to 50℃ and cooled for 20 s to demold the antibacterial layer. The glass fiber reinforced layer is laid in a mold with granules, preheated at 140°C for 2 min to soften, the pressure is increased to 10 MPa, held for 8 min, and then cooled with water to 50°C to demold and obtain the glass fiber reinforced layer board. Polypropylene composite material granules are placed in the injection molding machine barrel and heated to 195°C to melt and plasticize. They are then injected into the mold at a pressure of 70 MPa, held at 50 MPa for 8 seconds, and the mold temperature is maintained at 75°C. After cooling for 35 seconds, the polypropylene composite material layer is demolded to obtain the polypropylene composite material layer. Then, the polypropylene composite layer, the glass fiber reinforcement layer, and the antibacterial layer are stacked in sequence, and the flexible conductive sensor is placed between the glass fiber reinforcement layer and the antibacterial layer. The mixture is then hot-pressed at 185℃ and 8 MPa for 20 minutes and then cooled. After cooling to room temperature, the self-cleaning layer is sprayed onto the surface with a slurry and dried to obtain the antibacterial and anti-algae PP composite board.

[0073] Example 3 This embodiment provides an antibacterial and anti-algae PP composite board, comprising a self-cleaning layer (10 μm), a polypropylene composite material layer (200 μm), a glass fiber reinforcement layer (500 μm), and an antibacterial layer (50 μm) stacked sequentially. A flexible conductive sensor is disposed between the glass fiber reinforcement layer and the antibacterial layer. The preparation method is as follows: (1) Preparation of antimicrobial masterbatch for antimicrobial layer Chitosan powder was added to acetic acid solution and stirred until completely dissolved to obtain a chitosan solution (chitosan concentration 10 wt%). Quaternary ammonium salt was added to the chitosan solution at a ratio of 3:1, with continuous stirring. The reaction was carried out at 80℃ for 2 h to obtain a quaternary ammonium salt-grafted chitosan solution. 0.1 M sodium hydroxide aqueous solution was added to adjust the pH of the quaternary ammonium salt-grafted chitosan solution to neutral, causing the quaternary ammonium salt-grafted chitosan to precipitate. After filtration, washing with deionized water, and vacuum drying, solid quaternary ammonium salt-grafted chitosan was obtained. Quaternary ammonium salt-grafted chitosan and nano-zinc oxide were weighed at a weight ratio of 5:1 and placed in a high-speed mixer. Ethanol, accounting for 50% of the total mass of the mixed filler, was added and stirred at high speed for 1 h to obtain a wet mixed filler. The mixed filler was then placed in an environment of 60℃ and 0.08 MPa vacuum for 1 h to remove the ethanol. Maleic anhydride-grafted polypropylene resin and mixed fillers were added to a high-speed mixer at a mass ratio of 8:2 for dry mixing. The mixed material was then fed into a twin-screw extruder for melt extrusion. The melt extrusion was carried out using a screw extruder with the following parameters: Zone 1 172℃, Zone 2 178℃, Zone 3 190℃, Zone 4 198℃, Die head 192℃, and rotation speed of 220 rpm. Granulation was performed to obtain antibacterial masterbatch with a particle size D50 of 15 μm.

[0074] (2) Granules for preparing glass fiber reinforced layers Short-cut glass fibers and ethylene-ethyl acetate copolymer were mixed at a mass ratio of 5:5 in a high-speed mixer at 500 rpm at 50°C. The mixture was then fed into a twin-screw extruder and melt-extruded at controlled temperatures of 125°C, 145°C, 165°C, 155°C, and 150°C, with a rotation speed of 100 rpm. The mixture was then granulated to obtain granules for glass fiber reinforced layers.

[0075] (3) Preparation of granules for polypropylene composite layer 50 parts of polypropylene resin, 15 parts of nano titanium dioxide, 5 parts of compatibilizer, 1 part of antioxidant 1010 and 2 parts of light stabilizer are uniformly mixed and then added to a twin-screw extruder. The temperature of the twin-screw extruder is controlled at 170℃, 195℃ and 205℃ for melt extrusion and granulation to obtain granules for polypropylene composite material layers.

[0076] (4) Preparation of slurry for self-cleaning layer Heptadecafluorodecyltriethoxysilane, nano-silica, and polydimethylsiloxane were dissolved in anhydrous ethanol in a ratio of 14:9:7. 0.5 wt% acetic acid was added, and the mixture was ultrasonically dispersed at 300 W for 30 min to obtain a slurry for a self-cleaning layer.

[0077] (5) Preparation of antibacterial and anti-algae PP composite board The antibacterial masterbatch was vacuum dried at 60°C for 4 hours to ensure that the moisture content of the antibacterial masterbatch was less than 0.1%. The antibacterial masterbatch, which was melted at 170°C, was injected into the mold at 80 MPa pressure. The mold was held at 60 MPa pressure for 5 seconds. The mold temperature was then reduced to 60°C and cooled for 30 seconds to demold the antibacterial layer. The glass fiber reinforced layer is laid in a mold with granules, preheated at 150°C for 2 min to soften, the pressure is increased to 8 MPa, held for 8 min, and then cooled to 50°C by water to demold and obtain the glass fiber reinforced layer board. Polypropylene composite material granules are placed in the injection molding machine barrel and heated to 192°C to melt and plasticize. They are then injected into the mold at a pressure of 80 MPa, held at 50 MPa for 8 seconds, and the mold temperature is maintained at 70°C. After cooling for 25 seconds, the polypropylene composite material layer is demolded to obtain the polypropylene composite material layer plate. Then, the polypropylene composite layer, the glass fiber reinforcement layer, and the antibacterial layer are stacked in sequence, and the flexible conductive sensor is placed between the glass fiber reinforcement layer and the antibacterial layer. The mixture is then hot-pressed at 175℃ and 10 MPa for 20 minutes and then cooled. After cooling to room temperature, the self-cleaning layer is sprayed onto the surface with a slurry and dried to obtain the antibacterial and anti-algae PP composite board.

[0078] Example 4 This embodiment provides an antibacterial and anti-algae PP composite board.

[0079] The difference from Example 1 is that, in this example, the chopped glass fibers are replaced with 50 mm long chopped glass fibers (purchased from China Jushi, model ECK13-4.5-508A).

[0080] Example 5 This embodiment provides an antibacterial and anti-algae PP composite board.

[0081] The difference from Embodiment 1 is that, in this embodiment, a flexible conductive sensor is not included.

[0082] Comparative Example 1 This comparative example provides an antibacterial and anti-algae PP composite board.

[0083] The difference from Example 1 is that, in this comparative example, the mixed filler was replaced with nano silver (purchased from Evonik, Germany, model SilverNanoPowder-30).

[0084] Comparative Example 2 This comparative example provides an antibacterial and anti-algae PP composite board.

[0085] The difference from Example 1 is that, in this comparative example, the mixed filler is replaced with an equal mass of nano zinc oxide, i.e., no quaternary ammonium salt grafted chitosan is added.

[0086] Comparative Example 3 This comparative example provides an antibacterial and anti-algae PP composite board.

[0087] The difference from Example 1 is that, in this comparative example, the mixed filler is replaced with an equal mass of quaternary ammonium salt grafted chitosan, i.e., no nano zinc oxide is added.

[0088] Comparative Example 4 This comparative example provides an antibacterial and anti-algae PP composite board.

[0089] The difference from Example 1 is that in this comparative example, the nano-titanium dioxide in step (3) is omitted.

[0090] Comparative Example 5 This comparative example provides an antibacterial and anti-algae PP composite board.

[0091] The difference from Example 1 is that no self-cleaning layer is provided in this comparative example.

[0092] Performance testing The performance of the boards provided in the examples and comparative examples was tested using the following methods: (1) Antibacterial and anti-algae PP composite boards provided in the examples and comparative examples were tested for antibacterial properties. The samples were cut into 5cm×5cm pieces, and the surfaces were disinfected by ultraviolet irradiation for 30 min. Vibrio (ATCC 17802 / CMCC(B)21603) and Escherichia coli ( ) were selected. Escherichia coli ATCC 25922 and mold (ATCC 6227b / CMCC(F)98004) were formulated to a concentration of 1×10 6 A bacterial suspension of CFU / mL was evenly spread on the surface of the PP sample plate using a sterile cotton swab, covered with sterile filter paper, and incubated in an incubator at 30℃ and 95±3% relative humidity for 7 days. Sterile nutrient solution was sprayed daily to keep the plate moist. The diameter of the inhibition zone was measured, which is the width of the area where no bacteria grow. The inhibition rate was calculated using the formula: inhibition rate = (average colony count of control group - average colony count of experimental group) / average colony count of control group × 100%. (2) Antibacterial stability: A 5cm×5cm sample was immersed in water at 30℃ for 14 days, then removed and tested for antibacterial activity according to the above test method. The results are shown in Table 1: Table 1 As can be seen from the examples and performance tests, the antibacterial and anti-algae PP composite board provided by the present invention has excellent antibacterial properties and antibacterial stability. Its inhibition rate against Vibrio, Escherichia coli and mold is above 97%, and it can still maintain more than 95% antibacterial properties after soaking.

[0093] As can be seen from the comparison of the examples and comparative examples, the present invention, by introducing a composite antibacterial system composed of quaternary ammonium salt grafted chitosan and nano zinc oxide, enables the PP composite board to have excellent antibacterial properties, while improving the stability of the antibacterial system in long-term water immersion, thereby avoiding the problem of the board's antibacterial effect decaying due to the loss of antibacterial agents.

[0094] (2) Prepare several PP boards for the examples and comparative examples, cut them into 5cm×5cm sizes as samples, and disinfect the surface of the PP boards by ultraviolet irradiation for 30 min. Select Chlorella proteoglycans ( Chlorella pyrenoidosa ) and Microcystis aeruginosa ( Microcystis aeruginosa The preparation concentration is 1×10 6A mixed algal culture solution of CFU / mL was used. The sample PP plate was placed in the center of an Allen medium petri dish, and the algal culture solution was evenly sprayed onto the surface using a chromatographic sprayer. The plate was incubated for 21 days at 30℃, 95±3% relative humidity, and 3000 lx illumination. Algal coverage was recorded every 7 days and calculated using the formula: Coverage = (Algal Coverage Area of ​​Measured Surface / Total Surface Area of ​​Sample) × 100%. The test standard was GB / T21866-2008. The test results are shown in Table 2. Table 2 As can be seen from the examples and performance tests, the antibacterial and anti-algae PP composite board provided by the present invention has excellent anti-algae properties, and algae grow extremely slowly on its surface.

[0095] (3) Prepare several PP sheets prepared in the examples and comparative examples, cut them into 10cm×10cm sizes as samples, and disinfect the surface of the PP sheets by ultraviolet irradiation for 30 min. Perform durability tests on the PP sheets according to standard GB / T 16422.2-2022. The test results are shown in Table 3: Table 3 As can be seen from the examples and performance tests, the antibacterial and anti-algae PP composite board provided by the present invention has excellent durability. In the aging resistance test, it has a small color difference, and has a high tensile strength retention rate and impact strength. At the same time, it has a low surface crack density.

[0096] The present invention has been illustrated through the above embodiments, but the present invention is not limited to the above process steps, that is, it does not mean that the present invention must rely on the above process steps to be implemented. Those skilled in the art should understand that any improvements to the present invention, equivalent substitutions of the raw materials used in the present invention, additions of auxiliary components, and selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. An antibacterial and anti-algae PP composite board, characterized in that, It includes a polypropylene composite material layer, a glass fiber reinforcement layer and an antibacterial layer stacked in sequence. The antibacterial layer is composed of an antibacterial masterbatch, which has a core-shell structure. The shell is made of maleic anhydride-grafted polypropylene resin material, and the core is a mixed filler formed by quaternary ammonium salt-grafted chitosan and nano zinc oxide.

2. The antibacterial and anti-algae PP composite board according to claim 1, characterized in that, Based on the total mass of the components of the antibacterial masterbatch as 100%, the mass percentage of the maleic anhydride-grafted polypropylene resin is 60-80 wt%. The method for preparing the antibacterial masterbatch includes: mixing maleic anhydride-grafted polypropylene resin and mixed fillers, melt extruding, and granulating to obtain an antibacterial masterbatch with a particle size D50 of 5-15 μm. The melt extrusion is carried out using a screw extruder, the parameters of which include: zone 1 170-175℃, zone 2 175-180℃, zone 3 185-195℃, zone 4 195-200℃, die head 190-195℃, and speed 200-240 rpm.

3. The antibacterial and anti-algae PP composite board according to claim 2, characterized in that, The preparation method of the mixed filler includes: quaternary ammonium salt grafted chitosan and nano zinc oxide are mixed in the presence of ethanol at a mass ratio of (2-5):1 for 0.5-1h to obtain the mixed filler; The preparation method of the quaternary ammonium salt grafted chitosan includes: Chitosan solution and glycidyltrimethylammonium chloride were mixed at a mass ratio of 1:(1-3) and reacted at 60-80℃ for 2-3 h. After the reaction, the pH was adjusted to neutral to precipitate the quaternary ammonium salt-grafted chitosan, thus obtaining the quaternary ammonium salt-grafted chitosan.

4. The antibacterial and anti-algae PP composite board according to claim 1, characterized in that, The glass fiber reinforced layer comprises chopped glass fibers and ethylene-ethyl acetate copolymer, and the chopped glass fibers comprise 50-80 wt% of the total mass of the glass fiber modified layer, based on 100% of the total mass of the components. The chopped glass fibers have a length of 1-5 mm, and the vinyl acetate content in the ethylene-ethyl acetate copolymer is 18-40%.

5. The antibacterial and anti-algae PP composite board according to claim 1, characterized in that, The polypropylene composite material layer comprises 25-50 parts polypropylene resin, 5-15 parts nano silica, 1-5 parts compatibilizer, 0.6-1 part antioxidant, and 0.2-2 parts light stabilizer. The compatibilizer includes maleic anhydride-grafted polypropylene, the antioxidant includes antioxidant 1010, and the light stabilizer includes hindered amine light stabilizers.

6. The antibacterial and anti-algae PP composite board according to claim 1, characterized in that, The thickness of the antibacterial layer is 10-50 μm, the thickness of the glass fiber reinforced layer is 100-500 μm, and the thickness of the polypropylene composite layer is 50-200 μm.

7. The antibacterial and anti-algae PP composite board according to claim 1, characterized in that, The antibacterial and anti-algae PP composite board also includes a flexible conductive sensor, which is located between the glass fiber reinforcement layer and the antibacterial layer, and the thickness of the conductive sensor is 10-100μm. The antibacterial and anti-algae PP composite board also includes a self-cleaning layer. The self-cleaning layer is located on the side of the polypropylene composite material layer away from the glass fiber reinforcement layer. The thickness of the self-cleaning layer is 5-10 μm. The components of the self-cleaning layer include heptadecafluorodecyltriethoxysilane, nano-silica, and polydimethylsiloxane. The mass ratio of heptadecafluorodecyltriethoxysilane, nano-silica, and polydimethylsiloxane is (12-15):(8-10):(5-8).

8. A method for preparing an antibacterial and anti-algae PP composite board as described in any one of claims 1-7, characterized in that, The preparation method includes: (1) The polypropylene composite material layer, the glass fiber reinforcement layer and the antibacterial layer are stacked in sequence and hot-pressed at 175-185℃ and 8-10 MPa for 15-20 min to obtain the antibacterial and anti-algae PP composite board.

9. The preparation method according to claim 8, characterized in that, The preparation method further includes: placing a flexible conductive sensor between the glass fiber reinforcement layer and the antibacterial layer, and then performing lamination and hot pressing; The preparation method further includes: mixing the ethanol slurry of the self-cleaning layer with 0.1-1 wt% acetic acid, coating it on the surface of the polypropylene composite material layer, and drying it to obtain the self-cleaning layer.

10. The application of an antibacterial and anti-algae PP composite board as described in any one of claims 1-7 in aquaculture.

Citation Information

Patent Citations