A heat treatment process for welded seams of wind turbine tower portal frames

By optimizing the microstructure of the wind turbine tower frame welds through gradient heat treatment, residual stress is eliminated and impact toughness is improved. This solves the problems of brittle fracture and fatigue resistance of the wind turbine tower frame welds, thereby improving the safety and service life of the tower.

CN122081635APending Publication Date: 2026-05-26CHINA POWER COMPLETE EQUIP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610334476.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-03-18
Publication Date
2026-05-26

AI Technical Summary

Technical Problem

Existing technologies lack effective post-weld heat treatment processes for the welds of wind turbine tower frames, resulting in the inability to effectively eliminate residual stress. This affects the resistance to brittle fracture and fatigue in the weld area, posing a risk of cracking and impacting the safety and service life of the tower.

Method used

A gradient heat treatment process is adopted, including pretreatment, gradient heating, and slow cooling. By setting multiple holding temperatures and slow cooling rates, the microstructure of the weld metal is optimized, residual stress is eliminated, and impact toughness is improved.

Benefits of technology

It significantly reduces the risk of delayed cracking and fatigue cracking, increases the impact toughness of weld metal by more than double, enhances the safety and service life of the tower, and avoids the risk of cracking.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122081635A_ABST
    Figure CN122081635A_ABST
Patent Text Reader

Abstract

This invention provides a heat treatment process for the weld seam of a wind turbine tower frame, relating to the field of metal material heat treatment technology, including the following steps: S1: Pre-treatment of the fillet weld seam area of ​​the wind turbine tower frame; S2: Gradient heating treatment at the same heating rate: first heating the fillet weld seam area to 280±20°C for a first heat preservation, then continuing heating to 450°C±20°C for a second heat preservation, and finally continuing heating to 580°C±20°C for a third heat preservation; S3: After the heat preservation is completed, the workpiece is cooled. This invention can not only eliminate welding residual stress and prevent the initiation of delayed cracks and fatigue cracks, but also significantly improve the microstructure of the weld metal, increasing its low-temperature impact toughness by more than double, thereby greatly improving the operational reliability of wind turbine towers and solving the problem of tower frame cracking in winter.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of heat treatment technology for metallic materials, and in particular to a heat treatment process for welded seams of wind turbine tower frames. Background Technology

[0002] As a critical supporting structure for wind turbine generators, the safety of the wind turbine tower is paramount. The portal frame is a weak point in the tower; its openings cause stress concentration, and the frame itself is typically welded from thick plates, generating significant residual stress in the weld area (such as at fillet welds) during the welding process. This residual stress, combined with the alternating stress generated by wind loads, greatly increases the risk of delayed and fatigue cracks in the weld area (especially the heat-affected zone). In severe cases, this could lead to tower tearing or even collapse, with potentially disastrous consequences.

[0003] Currently, while Q355 material is widely used in wind power tower manufacturing, there are no clear process requirements for post-weld heat treatment of the portal frame of in-service wind turbine towers, nor are there specific stress-relieving heat treatment procedures. This situation makes it difficult to effectively improve the residual welding stress in the weld area of ​​the tower portal frame under harsh operating conditions, thus failing to fully address the problems of insufficient resistance to brittle fracture and fatigue, which may affect the long-term safety and reliable operation of the structure.

[0004] Therefore, there is an urgent need in this field for a dedicated heat treatment method for the door frame weld of Q355 material wind turbine towers, which can not only efficiently eliminate residual stress, but also simultaneously and significantly improve the impact toughness of the weld material, thereby fundamentally enhancing the safety and service life of the tower. Summary of the Invention

[0005] The purpose of this invention is to provide a heat treatment process for the weld seam of the door frame of a wind turbine tower. By setting up a gradient heat treatment and slow cooling technical solution, it can not only eliminate residual welding stress and prevent the initiation of delayed cracks and fatigue cracks, but also significantly improve the microstructure of the weld metal, making its impact toughness more than double, thereby greatly improving the operational reliability of the wind turbine tower.

[0006] To achieve the above objectives, the present invention adopts the following technical solution: The present invention provides a heat treatment process for welded seams of wind turbine tower frame, comprising the following steps: S1: Pre-treatment of the corner weld area of ​​the door frame of the wind turbine tower; S2: Perform gradient heating treatment at the same heating rate: first heat the corner weld area of ​​the door frame to 280±20°C for the first heat preservation, then continue heating to 450°C±20°C for the second heat preservation, and finally continue heating to 580°C±20°C for the third heat preservation. S3: After the heat preservation is completed, the workpiece is cooled.

[0007] Furthermore, based on the above technical solution, the material of the wind turbine tower is low-alloy high-strength steel of model Q355.

[0008] Furthermore, based on the above technical solution, in step S1, the preprocessing includes: Evenly wrap the door frame corner weld area with rope-type heating pads, ensuring that the coverage area on both sides of the weld is no less than 50mm wide, and then evenly apply insulation cotton to the surface of the heating pads.

[0009] Furthermore, based on the above technical solution, in step S2, the heating rate is 10-100°C / h.

[0010] Furthermore, based on the above technical solution, in step S2, the insulation time for both the first insulation and the second insulation is 45-70 minutes.

[0011] Furthermore, based on the above technical solution, in step S2, the heat preservation time of the third heat preservation is T1, where T1 > plate thickness × (3.5-4) min / mm, and T1 ≥ 3h; The plate thickness refers to the thickness of the wind turbine tower section where it connects with the door frame, and the unit is mm.

[0012] Furthermore, based on the above technical solution, in step S3, the cooling rate is ≤100°C / h.

[0013] Furthermore, based on the above technical solution, in step S3, the workpiece is cooled to ≤50°C.

[0014] Furthermore, based on the above technical solution, the solder used at the corners of the door frame is selected according to the different welding methods: For manual arc welding, use solder of type E5015; For gas shielded welding, the ER50-6 solid welding wire is selected.

[0015] Furthermore, based on the above technical solutions, the rated output power of a single wind turbine generator set in a wind power tower is between 6MW and 8MW.

[0016] The heat treatment process for the weld seam of the wind turbine tower frame provided by this invention has the following beneficial effects: 1. The heat treatment process provided by the present invention, by setting the temperature, holding time, heating rate and final cooling rate of the gradient heating treatment, can ensure the strength of the material while fully releasing the residual stress in the weld area, fundamentally avoiding the delayed crack generation caused by excessive residual stress, and significantly reducing the driving force for fatigue crack initiation.

[0017] 2. This invention optimizes and reconstructs the microstructure of the weld metal through a specific "high-temperature tempering + slow cooling" heat treatment process. Specifically, unstable structures such as supersaturated solid solutions and lamellar pearlite in the weld precipitate dispersed carbides (such as cementite) at 580°C±20°C, and lamellar pearlite transforms into spheroidized pearlite, resulting in a more uniform microstructure and improved toughness. Simultaneously, coarse structures such as Widmanstätten in the weld are refined, improving the strength-toughness balance and mitigating lattice distortion in the weld microstructure, thus reducing the risk of cracking caused by stress concentration. This optimized microstructure results in the Charpy V-notch impact energy (CVN) of the weld metal being more than doubled at low temperatures compared to the post-weld state, significantly enhancing the door frame's resistance to low-temperature impact and brittle fracture.

[0018] 3. The heat treatment process provided by this invention simultaneously achieves the two major goals of "stress relief" and "toughening" of the Q355 base material tower and its welded door frame structure. This not only solves the risk of cracking, but also improves the safety margin of the structure for long-term service from the perspective of material performance, effectively preventing the serious accident of "tower collapse" caused by crack propagation.

[0019] 4. The heat treatment process parameters provided by this invention are clear and easy to implement and control in industrial settings (such as large annealing furnaces or local heat treatment equipment), and are applicable to wind turbine tower frame assemblies of different specifications. Attached Figure Description

[0020] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.

[0021] Figure 1 This is a schematic diagram of gradient heating treatment provided in Embodiment 1 of the present invention; Figure 2 This is a comparison diagram of the impact performance of the sample in Example 1 of the present invention before and after heat treatment; Figure 3 This is a comparison diagram of the residual stress of the sample in Example 1 of the present invention before and after heat treatment. Detailed Implementation

[0022] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions in the embodiments of this invention will be clearly and completely described below in conjunction with the embodiments of this invention. Those skilled in the art should understand that the embodiments described are merely illustrative of the invention and should not be considered as specific limitations thereof. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention. Process parameters not specifically specified in the following embodiments are generally performed under conventional conditions.

[0023] The endpoints and any values ​​of the ranges disclosed in this invention are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this invention.

[0024] According to a first aspect of the present invention, a heat treatment process for welded seams of wind turbine tower portal frames is provided, comprising the following steps: S1: Pre-treatment of the corner weld area of ​​the door frame of the wind turbine tower; S2: Perform gradient heating treatment at the same heating rate: first heat the corner weld area of ​​the door frame to 280±20°C (e.g., 265°C, 270°C, 280°C, 285°C, 290°C, 295°C, etc.) for the first heat preservation, then heat to 450°C±20°C (e.g., 435°C, 440°C, 450°C, 455°C, 460°C, 465°C, etc.) for the second heat preservation, and finally heat to 580°C±20°C (e.g., 565°C, 570°C, 580°C, 585°C, 590°C, 595°C, etc.) for the third heat preservation; Specifically, in the first heat preservation stage, heating to 280±20°C can alleviate the lattice distortion of the weld microstructure and reduce residual welding stress. At this temperature, excess carbon in the bainite microstructure of the weld precipitates out and forms carbides. At the same time, dislocations in the microstructure undergo partial rearrangement and annihilation, significantly reducing micro-stress, but macro-stress removal is not obvious. In the second holding stage, heating to 450°C ± 20°C refines the coarse Widmanstätten structure in the weld. Widmanstätten is a coarse, acicular ferrite structure formed during welding. At around 450°C, the ferrite matrix undergoes recovery and recrystallization, dislocations rearrange, and the substructure is refined, thereby improving the strength and toughness balance of the microstructure. Simultaneously, the supersaturated solid solution further decomposes, and cementite begins to precipitate, although its morphology is not yet spheroidized. This causes more cementite to precipitate from the bainite in the weld and the cementite in the troostite to grow, thus partially transforming both into tempered sorbite, improving the toughness of the material.

[0025] In the third holding stage, heating to 580°C ± 20°C allows the supersaturated solid solution to precipitate dispersed carbides (such as cementite) and promotes the transformation of pearlite into spheroidized pearlite. At this temperature, atomic diffusion is significantly enhanced, allowing carbides to fully precipitate, aggregate, and spheroidize, while cementite lamellars in the pearlite spheroidize, resulting in a more uniform microstructure and improved toughness. Simultaneously, at this temperature, the coarse ferrite structure in the weld undergoes grain boundary migration and recrystallization, greatly alleviating lattice distortion, multiplying the toughness, and significantly reducing residual stress.

[0026] S3: After the heat preservation is completed, the workpiece is cooled.

[0027] As an optional embodiment of the present invention, the material of the wind turbine tower is low-alloy high-strength steel of type Q355; typically, without limitation, Q420 steel can also be subjected to residual stress relief treatment with reference to the heat treatment process provided by the present invention. The door frame is made of S355NE steel.

[0028] As an optional embodiment of the present invention, in step S1, the door frame fillet weld area of ​​the wind turbine tower includes the fillet weld of the door frame itself and the wind turbine tower at the junction of the fillet weld and the door frame. In step S1, the preprocessing includes: Use rope-type heating elements to evenly wrap around the corner weld area of ​​the door frame to achieve full coverage of the corner weld. Also cover part of the wind turbine tower where it connects to the door frame. The coverage area on both sides of the weld should not be less than 50mm. Insert thermocouples at the interface between the heating elements and the corner weld, and then evenly apply insulation cotton to the surface of the heating elements.

[0029] As an optional embodiment of the present invention, a temperature controller is used to control the heating temperature. In step S2, the heating rate is 10-100°C / h (e.g., 30°C / h, 50°C / h, 70°C / h, 90°C / h, etc.). A heating rate of 10-100°C / h can avoid cracking caused by large temperature differences in different areas of the workpiece due to heat transfer problems. If it is greater than 100°C / h, it may cause new residual stress in the material due to excessively rapid heating and uneven temperature analysis, which may even lead to cracks in the material.

[0030] Specifically, the present invention addresses the problem of a wind turbine tower made of Q355 steel, which is sensitive to welding. The welded joints on its door frame are fillet welds with severe stress concentration, and the door frame opening is a flattened ellipse with uneven stress distribution. The material properties, joint type, and geometry work together to inevitably result in high residual welding stress in this area after welding. If the heating rate in step S2 is too fast (≥100°C / h) or directly raised to above 400°C, the sudden change in internal stress may cause deformation or cracking of the tower door frame. The present invention, by limiting the heating rate to ≤100°C / h to 280±20°C and then holding the temperature, can significantly reduce the risk of deformation or cracking. However, if the heating temperature is too low, such as 200°C, since the mechanical properties of Q355 material are not significantly different between room temperature and 200°C, directly heating to 200°C and holding the temperature is inefficient in field implementation.

[0031] Furthermore, this invention employs a second heat preservation process by heating from 280±20°C to 450°C±20°C at the same rate. This is because insufficient heating, such as only reaching around 350°C, results in a small temperature difference with minimal impact, limited improvement on steel performance, and low process efficiency. Conversely, directly heating to around 550°C is excessively high, and drastic temperature changes can easily induce significant thermal stress in the door frame structure, increasing the risk of cracking. Therefore, choosing to heat to around 450°C effectively reduces the additional stress caused by the temperature gradient, preventing door frame deformation and cracking. The subsequent second heat preservation is necessary because the door frame structure is large, the weld walls are thick, and heat transfer from the surface to the interior is slow. Additionally, wind farms often experience strong winds, which can easily lead to uneven temperatures in different parts. The second heat preservation process ensures uniform temperature across the entire structure, providing a stable foundation for subsequent processes.

[0032] Furthermore, this invention heats the material from 450°C±20°C to 580°C±20°C at the same rate and then holds it at that temperature for the third time. This allows for the full release of residual stress in the door frame, and also allows carbon atoms dissolved in the steel to gradually precipitate from the matrix, thereby reducing the material's hardness and increasing its toughness, effectively enhancing its crack-arresting performance. If the temperature is only raised to around 500°C, the residual stress release is incomplete, the improvement in toughness is limited, and delayed cracking may still be induced by residual stress during subsequent service. If the temperature is held at around 700°C, the temperature exceeds the phase transformation point, causing a transformation from pearlite to austenite, resulting in significant changes in the material's microstructure and properties, large fluctuations in strength and toughness, and a significant decrease in performance stability. Therefore, to balance residual stress elimination, toughness improvement, and strength maintenance, 560–600°C is a more ideal heat treatment range. In addition, the heating rate from 450°C to 600°C should be controlled within 100°C / hour to avoid generating new residual stress due to excessively rapid heating and uneven temperature distribution, thereby preventing the risk of material cracking.

[0033] Furthermore, this invention chooses to perform gradient heating treatment at the same heating rate because the door frame structure is large in size, has thick walls containing fillet welds, and the wind turbine tower at the junction with the door frame is made of Q355 material, which is extremely sensitive to temperature gradients. Whether heating from a low-temperature range (e.g., from 280±20°C to 450°C±20°C) or a medium-temperature range (e.g., from 280±20°C to 450°C±20°C), an excessively rapid heating rate will generate drastic temperature differences between the internal structure and the surface, and between thick and thin areas, thus triggering new thermal stresses. These newly generated stresses may superimpose with the original residual stresses in the material, easily leading to workpiece deformation or even cracking. Therefore, using the same, relatively slow, and controlled heating rate (e.g., ≤100°C / h) can minimize the structural risks caused by uneven heating at any stage.

[0034] As an optional embodiment of the present invention, in step S2, the heat preservation time for both the first heat preservation and the second heat preservation is 45-70 minutes. The insulation time for the third insulation is T1, where T1 > plate thickness × (3.5-4) min / mm, and T1 ≥ 3h; The plate thickness refers to the thickness of the wind turbine tower section where it connects with the door frame, and the unit is mm.

[0035] Specifically, the residual stress in the corner weld area of ​​the door frame of the wind turbine tower is relatively large, and sufficient insulation time is required to remove some of the residual stress. This invention limits the insulation time of the third insulation to T1 > plate thickness × (3.5-4) min / mm (e.g., 3.6 min / mm, 3.7 min / mm, 3.8 min / mm, 3.9 min / mm, etc.), which realizes the quantifiable control of the insulation time. If the time is too short (e.g., < plate thickness × (3.5-4) min / mm), the stress will not be completely released; if the time is too long (e.g., much longer than plate thickness × (3.5-4) min / mm), although the effect is better, the energy and labor costs will increase significantly, and the benefits will decrease.

[0036] Furthermore, the present invention also limits the insulation time of the third insulation to T1≥3h, because the overall heat capacity of the door frame fillet weld area of ​​the wind turbine tower is large and the temperature uniformity is poor. By limiting the third insulation time to ≥3h, it can be ensured that the door frame fillet weld area of ​​the wind turbine tower (including the wind turbine tower, door frame, fillet weld, and heat-affected zone) fully reaches the target temperature and completes the microstructure transformation.

[0037] As an optional embodiment of the present invention, in step S3, the cooling rate is ≤100°C / h (e.g., 30°C / h, 50°C / h, 70°C / h, 90°C / h, etc.).

[0038] Specifically, slow cooling at a rate ≤100°C / h aims to maintain the properties gained from gradient heat treatment while avoiding the introduction of new defects during the final cooling stage. Slow cooling minimizes temperature gradients between the internal and external parts of the component and between different regions, preventing the generation of new thermal stresses due to rapid shrinkage and avoiding deformation or cracking caused by superposition with residual stresses. Simultaneously, the slower cooling rate allows the microstructure to approach an equilibrium state, preventing the formation of brittle phases and ensuring that the good toughness, crack arrest performance, and moderate strength acquired during the high-temperature holding stage are stably maintained until room temperature. Furthermore, for large, thick-walled door frame structures of wind turbine towers made of Q355 material, this controlled slow cooling process allows sufficient time for uniform shrinkage, thus fully extending the stress relief effect to the final state and ensuring the dimensional stability of the component during subsequent service.

[0039] As an optional embodiment of the present invention, in step S3, the workpiece is cooled to ≤50°C (e.g., 10°C, 20°C, 30°C, 40°C, etc.).

[0040] Specifically, if the slow cooling is removed after reaching 100°C, the workpiece will be in an uncontrolled state during the subsequent cooling phase from 100°C to room temperature. Due to the difficulty in achieving uniform heat dissipation, especially in areas with varying structural thicknesses or under ventilated conditions, significant temperature gradients can easily form between the workpiece surface and core, and between different parts. This uneven cooling leads to localized shrinkage differences, generating internal tensile stress. For door frame weld structures that have already undergone heating cycles, cracks are highly likely to form. Furthermore, while the risk of phase transformation is lower in the 100°C to room temperature range, rapid cooling can still place the material in a high-stress state, weakening the stress relief effect achieved through previous heat treatment. Therefore, extending the controlled cooling endpoint to ≤50°C is equivalent to bringing the entire cooling process completely under control, minimizing stress concentration caused by non-uniform cooling, and providing a more reliable guarantee for the dimensional stability and structural integrity of the workpiece at room temperature.

[0041] As an optional embodiment of the present invention, the heating and cooling methods in the present invention are both controlled by a temperature control box (model: ZWK-I-60kW, manufacturer: Wujiang Xunda Electric Heating Appliance Technology Co., Ltd.) to control the heating or cooling rate.

[0042] As an optional embodiment of the present invention, the solder present at the corner of the door frame is selected according to the different welding methods: For manual arc welding, use solder of type E5015; For gas shielded welding, the ER50-6 solid welding wire is selected.

[0043] As an optional embodiment of the present invention, the rated output power of a single wind turbine generator set is between 6MW and 8MW.

[0044] The present invention will now be described in further detail with reference to specific embodiments and comparative examples. Unless otherwise specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply.

[0045] Example 1 Taking the tower frame of a certain in-service wind turbine as an example, the tower material is Q355NE steel, the frame material is S355NE steel, the rated output power of a single wind turbine is 6.7MW, the welding method is manual arc welding, the welding material is E5015, and the thickness of the wind turbine tower plate at the connection with the frame is 47 mm.

[0046] Three samples were selected from the tower's door frame and subjected to the following heat treatment process, including the following steps: S1: Pre-treatment of the fillet weld area of ​​the door frame: Wrap the fillet weld with a rope-type heating tape to achieve full coverage of the fillet weld, and also cover part of the wind turbine tower where it connects to the door frame. The coverage width on both sides of the weld should not be less than 50mm. Insert a thermocouple at the interface between the heating tape and the fillet weld, and then lay insulation cotton on the heating tape. Considering the relatively strong wind at the site, two layers of insulation cotton can be laid. Secure the insulation cotton with steel wire, welding nails, or brackets. S2: Turn on the temperature controller and perform gradient heating treatment at the same heating rate (100°C / h), such as... Figure 1 As shown: (1) First heat the corner weld area of ​​the door frame to 300°C and perform the first heat preservation for 60 minutes. (2) Reheat to 450°C and maintain the temperature for a second time for 60 minutes. (3) Finally, heat to 600°C and keep warm for 3 hours; S3: After the heat preservation is completed, the workpiece is cooled to 50°C at a cooling rate of 100°C / h.

[0047] like Figure 2 and Figure 3 As shown, the average impact energy (27J) and average residual stress (437MPa) of the three samples (after heat treatment) and the sample before heat treatment in Example 1 are compared. This shows that the Charpy V-notch impact energy of the door frame weld metal after heat treatment of the present invention at -40℃ is increased by more than 115% compared with the untreated sample, which fully achieves the goal of more than doubling the improvement, and the welding residual stress is effectively reduced.

[0048] Example 2 The difference between Example 2 and Example 1 is as follows: S2: Turn on the temperature controller and perform gradient heating treatment at the same heating rate (100°C / h): (1) First heat the corner weld area of ​​the door frame to 280°C and perform the first heat preservation for 70 minutes. (2) Reheat to 430°C and maintain the temperature for a second time for 70 minutes. (3) Finally, heat to 580°C and keep warm for 3.5 hours; S3: After the heat preservation is completed, the cooling rate is controlled by a temperature control box, and the workpiece is cooled to 30°C at a cooling rate of 50°C / h.

[0049] The remaining steps and technical parameters are the same as in Example 1.

[0050] Example 3 The difference between Example 3 and Example 1 is as follows: S2: Turn on the temperature controller and perform gradient heating treatment at the same heating rate (100°C / h): (1) First heat the corner weld area of ​​the door frame to 260°C and perform the first heat preservation for 70 minutes. (2) Reheat to 470°C and maintain the temperature for a second time for 60 minutes. (3) Finally, heat to 560°C and keep warm for 4 hours; S3: After the heat preservation is completed, the cooling rate is controlled by a temperature control box, and the workpiece is cooled to 40°C at a cooling rate of 80°C / h.

[0051] The remaining steps and technical parameters are the same as in Example 1.

[0052] The process conditions for Comparative Examples 1-10 are shown in Table 1: Table 1 Except for the conditions mentioned above, which are different from those in Example 1, all other steps and process parameters are the same as in Example 1.

[0053] Performance testing Residual stress test: The stress at the weld toe was measured using the blind hole method according to GB / T 31310-2014; Impact toughness test: Charpy V-notch impact test (-40°C) was conducted by taking samples from the center of the weld in accordance with GB / T 229-2020.

[0054] Ultrasonic flaw detection defects: Perform ultrasonic flaw detection on the heat-treated door frame in accordance with NB / T47013.3 to check for any new defects (defects will be generated if the cooling is too fast or the heating is too fast).

[0055] Results data The workpieces treated in Examples 1-3 and Comparative Examples 1-10 were subjected to residual stress and impact toughness tests. The average values ​​of the measured residual stress and impact toughness were taken, and the performance comparison is shown in Table 2. Table 2 As shown in Table 2, compared with Example 1, Comparative Example 1 has a heating temperature of 400°C in step (1), which is too high. This causes a sudden change in the thermal stress in the corner weld area of ​​the wind turbine tower frame, resulting in cracks inside the tower frame and defects. The impact toughness of the workpiece is also reduced.

[0056] As shown in Table 2, compared with Example 1, Comparative Example 2 has a larger temperature difference because the heating temperature in step (1) of Comparative Example 2 is 200°C, the initial heating temperature is too low, and the second heating is directly raised to 450°C, which causes a large thermal stress. Therefore, the residual stress of the workpiece is large and the impact toughness is significantly reduced.

[0057] As shown in Table 2, compared with Example 1, Comparative Example 3 has a larger residual stress and lower impact toughness because the heating temperature in step (2) of Comparative Example 3 is 350°C. The temperature difference from 300°C to 350°C is small, and the effect on improving the performance of steel is limited.

[0058] As shown in Table 2, compared with Example 1, Comparative Example 4 has a heating temperature of 550°C in step (2). The temperature difference from 300°C to 550°C is large. The drastic temperature change causes large thermal stress in the door frame structure, which leads to cracking inside the tower door frame and defects. Therefore, the impact toughness of the workpiece is also slightly reduced.

[0059] As shown in Table 2, compared with Example 1, Comparative Example 5 has a larger residual stress and can also lead to internal defects. The heating temperature in step (3) of Comparative Example 5 is 500°C. The temperature difference from 450°C to 500°C is small, the residual stress is not completely released, and the toughness improvement is limited.

[0060] As shown in Table 2, compared with Example 1, Comparative Example 6 has a heating temperature of 700°C in step (3). The temperature difference from 450°C to 700°C is large, which causes the temperature to exceed the phase transformation point. This leads to the transformation of pearlite into austenite, resulting in large fluctuations in toughness, reduced strength, and more serious defects in the interior of the workpiece, significantly reducing stability.

[0061] As shown in Table 2, compared with Example 1, Comparative Example 7 has a shorter heat preservation time of 2.5h, which results in incomplete release of thermal stress. Therefore, the residual stress of the workpiece is larger and the impact toughness is lower, which may also lead to new internal defects.

[0062] As shown in Table 2, compared with Example 1, Comparative Example 8 has a heating rate of 150℃ / h, which is too fast. This causes a sudden change in the thermal stress in the corner weld area of ​​the wind turbine tower frame, resulting in cracks and defects inside the tower frame. The impact toughness of the workpiece is also slightly reduced.

[0063] As shown in Table 2, compared with Example 1, Comparative Example 9 has a cooling rate of 150℃ / h, which is too fast. This rapid cooling will cause the workpiece to cool down quickly and generate new thermal stress. This stress, combined with the residual stress, will cause defects inside the workpiece. Furthermore, the residual stress of the workpiece is large and the impact toughness is low, resulting in new internal defects.

[0064] As shown in Table 2, compared with Example 1, Comparative Example 10 has a final cooling temperature of 100°C. The subsequent cooling stage of the workpiece from 100°C to room temperature is air cooling, resulting in uneven heat dissipation. This leads to defects inside the workpiece, and the workpiece has large residual stress and low impact toughness, resulting in new internal defects.

[0065] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A heat treatment process for wind turbine tower section door frame welds, characterized by, The method comprises the following steps: S1: Pretreating the door frame fillet weld area of the wind power tower; S2: Gradient heating treatment at the same heating rate: first heating the door frame fillet weld area to 280±20°C, first holding, then continuing to heat to 450°C±20°C, second holding, and finally continuing to heat to 580°C±20°C, third holding; S3: After the holding, cooling the workpiece.

2. The heat treatment process for wind turbine tower section door frame welds of claim 1, wherein, The material of the wind power tower is low-alloy high-strength steel of type Q355.

3. The heat treatment process for wind turbine tower section door frame welds of claim 1, wherein, In step S1, the pretreatment comprises: Uniformly winding the door frame fillet weld area with a rope-type heating sheet, and the coverage width on both sides of the weld shall not be less than 50mm, and then uniformly applying heat insulation cotton on the surface of the heating sheet.

4. The heat treatment process for wind turbine tower section door frame welds of claim 1, wherein, In step S2, the heating rate is 10-100°C / h.

5. The heat treatment process for wind turbine tower section door frame welds of claim 1, wherein, In step S2, the holding time of the first holding and the second holding is 45-70min.

6. The heat treatment process for wind turbine tower section door frame welds of claim 1, wherein, In step S2, the holding time of the third holding is T1, T1>plate thickness×(3.5-4)min / mm, and T1≥3h; Wherein, the plate thickness refers to the plate thickness of the wind power tower at the joint with the door frame, and the unit is mm.

7. The heat treatment process for wind turbine tower section door frame welds of claim 1, wherein, In step S3, the cooling rate is ≤100°C / h.

8. The heat treatment process for wind turbine tower section door frame welds of claim 1, wherein, In step S3, the workpiece is cooled to ≤50°C.

9. The heat treatment process for wind turbine tower section door frame welds of claim 1, wherein, The welding material existing in the door frame corner is selected according to the different welding methods: The welding material for manual electric arc welding is of type E5015; The welding material for gas shielded welding is of type ER50-6 solid wire.

10. The heat treatment process for wind turbine tower section door frame welds of claim 1, wherein, The single-machine rated output power of the wind turbine generator unit of the wind power tower is between 6MW and 8MW.