A zinc anode, its preparation method, and a battery

By constructing a composite modification layer of polystyrene microspheres and ionic liquid on the surface of the zinc anode, the interfacial stability problem of zinc-based metal anodes in acidic aqueous zinc-manganese batteries was solved, improving coulombic efficiency and cycle life, and enabling stable operation of the battery at high current density.

CN122091469APending Publication Date: 2026-05-26TIANFU JIANGXI LAB
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610161503.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-02-04
Publication Date
2026-05-26

AI Technical Summary

Technical Problem

Zinc-based metal anodes face interfacial stability issues in acidic aqueous zinc-manganese batteries, including severe hydrogen evolution, chemical corrosion, and irregular dendrite growth, leading to reduced coulombic efficiency and shortened battery life.

Method used

A composite modification layer formed by polystyrene microspheres and ionic liquids was used to construct a porous channel structure, which was then coated on the surface of a zinc substrate to form a protective layer with a thickness of 5-30 μm, thereby regulating the interfacial reaction of the zinc anode.

Benefits of technology

It significantly improves the coulombic efficiency and cycle life of the zinc anode, suppresses hydrogen evolution reaction and chemical corrosion, and maintains the stable performance of the battery at high current density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122091469A_ABST
    Figure CN122091469A_ABST
Patent Text Reader

Abstract

This invention discloses a zinc anode, its preparation method, and a battery, belonging to the field of electrochemical technology. It solves the problem of reduced coulombic efficiency and reduced cycle life in existing batteries using zinc-based metal anodes. A zinc anode includes a zinc substrate and a composite modification layer coated on the surface of the zinc substrate; the composite modification layer is formed by combining polystyrene microspheres and an ionic liquid, and the thickness of the composite modification layer is 5-30 μm. The composite modification layer on the zinc anode of this invention does not significantly hinder Zn²⁺ deposition. + The transmission of electrons can maintain the electron conversion reaction in the strong acid electrolyte, enabling the battery system to achieve excellent cycle stability while maintaining high voltage output. The acidic aqueous zinc-manganese full cell constructed with zinc anode prepared using this composite modification layer still maintains stable rate performance at high current density.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of electrochemical technology, specifically relating to a zinc anode, its preparation method, and a battery. Background Technology

[0002] In acidic aqueous zinc-manganese batteries, the zinc-based metal anode faces a series of severe interfacial stability problems in a strongly acidic electrolyte environment. First, there is the severe hydrogen evolution caused by reactions with water and protons; second, zinc metal inevitably undergoes chemical corrosion in acidic media; and third, irregular dendrite growth forms during repeated deposition / stripping of zinc. These problems accelerate the loss of zinc active material, damage electrode interfacial stability, and significantly reduce coulombic efficiency, cycle life, and battery safety. Summary of the Invention

[0003] In view of the above problems, the purpose of this invention is to provide a zinc anode, its preparation method and battery, which solves the problem of reduced coulombic efficiency and reduced cycle life of batteries using zinc-based metal anodes.

[0004] To achieve the above objectives, the technical solution of the present invention is implemented as follows: A zinc anode includes a zinc substrate and a composite modification layer coated on the surface of the zinc substrate; the composite modification layer is formed by combining polystyrene microspheres and an ionic liquid, and the thickness of the composite modification layer is 5-30 μm.

[0005] In some embodiments, the polystyrene microspheres have a particle size of 50-500 nm.

[0006] In some embodiments, the ionic liquid is at least one of 1-ethyl-3-methylimidazolium bis[(trifluoromethyl)sulfonyl]imide, 1-methyl-3-propylimidazolium bis[(trifluoromethyl)sulfonyl]imide, 1-butyl-3-methylimidazolium bis[(trifluoromethyl)sulfonyl]imide, 1-hexyl-3-methylimidazolium bis[(trifluoromethyl)sulfonyl]imide, 1,3-dimethylimidazolium bis[(trifluoromethyl)sulfonyl]imide, 1-ethyl-3-methylimidazolium tetrafluoroborate, 1-ethyl-3-methylimidazolium hexafluorophosphate, and 1-ethyl-3-methylimidazolium trifluoromethanesulfonate.

[0007] In some embodiments, the mass ratio of the polystyrene microspheres to the ionic liquid in the composite modification layer is (0.235-0.94):(7.55-22.65).

[0008] In some embodiments, the zinc substrate is one of zinc foil or zinc alloy foil, and the thickness of the zinc substrate is 10-200 μm.

[0009] In some embodiments, the composite modification layer has a porous channel structure, wherein the pore size of the porous channel is 10-200 nm.

[0010] Another technical solution of the present invention is implemented as follows: a method for preparing a zinc negative electrode, comprising the following steps: S1. Pre-treated zinc substrate: The zinc substrate is washed in a solvent, removed and dried to obtain the pre-treated zinc substrate; S2. Preparation of polystyrene microsphere dispersion: Dissolve polystyrene microspheres in solvent, stir and disperse evenly to obtain a polystyrene microsphere dispersion with a mass concentration of 0.5-2wt%, i.e., APS dispersion; S3. Preparation of zinc anode: The APS dispersion is added to the pretreated zinc substrate to obtain APS@Zn electrode, and the ionic liquid is added to the APS@Zn electrode to obtain APS-IL@Zn electrode, i.e., zinc anode.

[0011] In some embodiments, the solvent in S1 is at least one of ethanol, acetone, isopropanol, and toluene, and the drying temperature in S1 is 50-70°C, and the drying time is 3-9 hours.

[0012] In some embodiments, the assembly amount of the polystyrene microspheres on the pretreated zinc substrate in step S3 is 0.0053-0.0106 mg / mm². 2 The APS dispersion is added to the pretreated zinc substrate at a temperature of 50-70°C for 1-20 minutes.

[0013] Another technical solution of the present invention is as follows: a battery comprising the zinc negative electrode.

[0014] Compared with the prior art, the composite modification layer on the zinc anode of the present invention does not significantly hinder Zn²⁺. + The transmission of electrons can maintain the electron conversion reaction in the strong acid electrolyte, enabling the battery system to achieve excellent cycle stability while maintaining high voltage output. The acidic aqueous zinc-manganese full cell constructed with zinc anode prepared using this composite modification layer still maintains stable rate performance at high current density. Attached Figure Description

[0015] To more clearly illustrate the technical solutions in the embodiments of this application, the accompanying drawings used in the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0016] Figure 1 Optical images of the electrodes of Example 1 and Comparative Example 1 after immersion in electrolyte for 72 hours; Figure 2 Tafel curves of the electrodes of Example 1 and Comparative Example 1; Figure 3 Coulombic efficiency diagrams of zinc half-cells prepared from the electrodes of Example 1 and Comparative Example 1; Figure 4 The graph shows the long-term constant current cycling performance of the zinc symmetric cells prepared with the electrodes of Example 1 and Comparative Example 1. Figure 5 The graph shows the performance indicators of the zinc full cells prepared by the electrodes of Example 1 and Comparative Example 1. Figure 6 Performance parameters of composite modified layers prepared from colloidal solutions of different mass concentrations; It should be noted that the accompanying drawings are not necessarily drawn to scale, but are shown only in a schematic manner without affecting the reader's understanding. Detailed Implementation

[0017] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.

[0018] In this application, the terms "upper," "lower," "left," "right," "front," "rear," "top," "bottom," "inner," "outer," "middle," "vertical," "horizontal," "lateral," and "longitudinal" indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. These terms are primarily for the purpose of better describing this application and its embodiments, and are not intended to limit the indicated device, element, or component to having a specific orientation, or to be constructed and operated in a specific orientation.

[0019] Furthermore, in addition to indicating location or positional relationship, some of the aforementioned terms may also have other meanings. For example, the term "above" may also be used in some cases to indicate a certain dependency or connection relationship. Those skilled in the art can understand the specific meaning of these terms in this application based on the specific circumstances.

[0020] Furthermore, the terms "installation," "setup," "equipped with," "connection," and "linked" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral structure; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium, or an internal connection between two devices, components, or parts. Those skilled in the art can understand the specific meaning of these terms in this application based on the specific circumstances.

[0021] Furthermore, the terms "first," "second," etc., are primarily used to distinguish different devices, components, or parts (which may be the same or different in specific type and construction), and are not intended to indicate or imply the relative importance or quantity of the indicated devices, components, or parts. Unless otherwise stated, "a plurality of" means two or more.

[0022] It should also be understood that the terminology used in this application specification is for the purpose of describing particular embodiments only and is not intended to limit the application. As used in this application specification and the appended claims, the singular forms “a,” “an,” and “the” are intended to include the plural forms unless the context clearly indicates otherwise.

[0023] It should also be further understood that the term “and / or” as used in this application specification and the appended claims means any combination of one or more of the associated listed items and all possible combinations, and includes such combinations.

[0024] Example 1 Commercial zinc foil (thickness: 100 μm) was cut into discs (diameter: 12 mm) and ultrasonically washed in water and ethanol for 15 min to remove surface impurities and contaminants. It was then transferred to an empty beaker and kept in a drying oven at 60 °C for 5 h to obtain a pretreated zinc substrate. A 1 wt% colloidal solution was prepared by using ethanol as a solvent to prepare polystyrene microspheres with a particle size of 50 nm. 60 μL of the colloidal solution was added dropwise at a volume rate of 0.5 μL / s to the surface of a pretreated zinc substrate and allowed to stand at 60°C for 5 min to self-assemble to obtain an APS@Zn electrode. 5 μL of 1-ethyl-3-methylimidazolium bis[(trifluoromethyl)sulfonyl]imide liquid was added dropwise at a volume rate of 0.5 μL / s to the surface of the APS@Zn electrode. After standing, it was allowed to fill the pores of the polystyrene colloidal crystal self-assembled array to obtain the APS-IL@Zn electrode. The thickness of the composite modification layer on the APS-IL@Zn electrode was 17 μm, the pore size of the porous channels on the composite modification layer was 15 nm, and the assembly amount of polystyrene microspheres in the composite modification layer was 0.0098 mg / mm². 2 .

[0025] Example 2 Commercial zinc foil (thickness: 100 μm) was cut into discs (diameter: 12 mm) and ultrasonically washed in water and ethanol for 20 min to remove surface impurities and contaminants. Then it was transferred to an empty beaker and kept in a drying oven at 70 °C for 7 h to obtain a pretreated zinc substrate. A 1.5 wt% colloidal solution was prepared by using ethanol as a solvent to obtain 100 nm polystyrene microspheres. 60 μL of the colloidal solution was added dropwise at a volume rate of 0.5 μL / s to the surface of a pretreated zinc substrate and allowed to stand at 70°C for 10 min to self-assemble, thus obtaining an APS@Zn electrode. 10 μL of 1-ethyl-3-methylimidazolium bis[(trifluoromethyl)sulfonyl]imide liquid was uniformly poured onto the surface of the APS@Zn electrode at a volume rate of 0.5 μL / s. After standing, the liquid was allowed to fill the pores of the polystyrene colloidal crystal self-assembled array to obtain the APS-IL@Zn electrode. The thickness of the composite modification layer on the APS-IL@Zn electrode was 20 μm, the pore size of the porous channels on the composite modification layer was 25 nm, and the assembly amount of polystyrene microspheres in the composite modification layer was 0.0067 mg / mm². 2 .

[0026] Example 3 Commercial zinc foil (thickness: 100 μm) was cut into discs (diameter: 12 mm) and ultrasonically washed in water and ethanol for 25 min to remove surface impurities and contaminants. It was then transferred to an empty beaker and kept in a drying oven at 50 °C for 7 h to obtain a pretreated zinc substrate. A 2wt% colloidal solution was prepared by using ethanol as a solvent to prepare polystyrene microspheres with a particle size of 50nm. 60μL of the colloidal solution was added dropwise at a volume rate of 0.5μL / s to the surface of a pretreated zinc substrate and allowed to stand at 60°C for 15min to self-assemble to obtain an APS@Zn electrode. 15 μL of 1-ethyl-3-methylimidazolium bis[(trifluoromethyl)sulfonyl]imide liquid was added dropwise at a volume rate of 0.5 μL / s to the surface of the APS@Zn electrode. After standing, it was allowed to fill the pores of the polystyrene colloidal crystal self-assembled array to obtain the APS-IL@Zn electrode. The thickness of the composite modification layer on the APS-IL@Zn electrode was 20 μm, the pore size of the porous channels on the composite modification layer was 15 nm, and the assembly amount of polystyrene microspheres in the composite modification layer was 0.0072 mg / mm². 2 .

[0027] Comparative Example 1 Commercial zinc foil (thickness: 100 μm) was cut into discs (diameter: 12 mm) and ultrasonically washed in water and ethanol for 15 min to remove surface impurities and contaminants. It was then transferred to an empty beaker and kept in a drying oven at 60 °C for 5 h to obtain a pretreated zinc substrate. A 1 wt% colloidal solution was prepared by using ethanol as a solvent to prepare polystyrene microspheres with a particle size of 50 nm. 60 μL of the colloidal solution was added dropwise at a volume rate of 0.5 μL / s to the surface of a pretreated zinc substrate and allowed to stand at 60°C for 5 min to self-assemble, thus obtaining the APS@Zn electrode.

[0028] Comparative Example 2 Commercial copper foil (thickness: 100 μm) was cut into discs (diameter: 12 mm) and ultrasonically washed in water and ethanol for 15 min to remove surface impurities and contaminants. Then it was transferred to an empty beaker and kept in a drying oven at 60 °C for 5 h to obtain a pretreated copper substrate. A 1 wt% colloidal solution was prepared by using ethanol as a solvent to prepare polystyrene microspheres with a particle size of 50 nm. 60 μL of the colloidal solution was added dropwise at a volume rate of 0.5 μL / s to the surface of a pretreated copper substrate and allowed to stand at 60°C for 5 min to self-assemble, thus obtaining an APS@Cu electrode. 5 μL of 1-ethyl-3-methylimidazolium bis[(trifluoromethyl)sulfonyl]imide liquid was added dropwise at a volume rate of 0.5 μL / s to the surface of the APS@Cu electrode and allowed to stand until it filled the pores of the polystyrene colloidal crystal self-assembled array to obtain the APS-IL@Cu electrode.

[0029] Zinc-based batteries were prepared using the electrodes from Examples 1-3 and Comparative Examples 1-2, with glass fiber membrane as the separator material; 1 mol L 1 Zinc sulfate solution, 1 mol L 1 Manganese sulfate solution and 0.5 mol L 1 A sulfuric acid solution was used as the electrolyte. Zinc symmetric cells were assembled in the following order: negative electrode shell, electrode, separator, electrode, gasket, spring, and positive electrode shell. A suitable amount of electrolyte was added to assemble a coin cell for electrochemical testing. Zinc half-cells were assembled in the following order: negative electrode shell, Zn electrode, separator, electrode, gasket, spring, and positive electrode shell. A suitable amount of electrolyte was added to assemble a coin cell for electrochemical testing. Zinc full cells were assembled in the following order: negative electrode shell, electrode, separator, MnO2 positive electrode, gasket, spring, and positive electrode shell. A suitable amount of electrolyte was added to assemble a coin cell for electrochemical testing. The zinc symmetric cells were tested at a current density of 2 mA cm⁻¹. - ², Capacity cutoff is 1mAh cm -Electrochemical tests were conducted under the following conditions: ². The zinc full cell test conditions were a current density of 0.2 Ag. - ¹-2Ag - ¹. The test results are shown in Table 1.

[0030] Table 1. Test results of zinc symmetric cells corresponding to the examples and comparative examples.

[0031] To evaluate the effectiveness of the zinc anode, the obtained product and untreated zinc foil were immersed together in an electrolyte solution of 1 mol zinc sulfate, 0.5 mol manganese sulfate, and 0.2 mol sulfuric acid for a seven-day immersion experiment under the same conditions. Figure 1 As shown, the APS-IL@Zn electrode exhibits the least surface corrosion and demonstrates the best protective performance.

[0032] To evaluate the effect of a colloidal solution prepared from polystyrene microspheres using ethanol as a solvent on the thickness of the composite modified layer, the thickness of the composite modified layer without the addition of ionic liquid was studied. The results show that the protective layer assembled with a 1 wt% colloidal solution exhibits the best performance, minimal polarization, and stable performance. Figure 6 As shown.

[0033] To evaluate the interfacial corrosion behavior, Tafel polarization measurements were performed on the product prepared in Example 1 using a three-electrode configuration. Figure 2 As shown, APS-IL@Zn exhibits the most positive corrosion potential and shows a low degree of corrosion, indicating a significantly enhanced corrosion resistance. The working electrode in the three-electrode configuration is the prepared product, and the reference electrode is Zn²⁺. + / Zn, with the counter electrode being a platinum sheet, graphite sheet, or glassy carbon electrode.

[0034] To systematically evaluate the interface engineering effect and electrochemical reversibility of the zinc anode, a zinc half-cell assembled based on the electrode prepared in Example 1 was tested. Figure 3 As shown, the APS-IL@Zn||Zn half-cell exhibits excellent zinc plating / stripping reversibility and cycle stability, achieving an average coulombic efficiency (CE) of up to 98.84% over more than 200 cycles. In contrast, the performance of the cell prepared using only the pretreated zinc substrate is significantly reduced, failing after only 74 cycles.

[0035] To investigate the interfacial stability of the zinc anode during long-term cycling, a zinc symmetric cell assembled in Example 1 was subjected to constant current cycling tests. Figure 4As shown, zinc symmetric cells prepared using only a pretreated zinc substrate failed rapidly after only 69 hours due to severe interfacial instability. In contrast, APS-IL@Zn zinc symmetric cells exhibited significantly improved cycle durability, operating stably for over 500 hours and maintaining smooth, reversible zinc deposition / stripping behavior throughout the test, without significant voltage fluctuations or spikes.

[0036] Rate curve of zinc full cell assembled in Example 1; as shown Figure 5 As shown, compared with the Zn||MnO2 battery under the same conditions, the full cell using APS-IL@Zn anode exhibits better performance at 0.2 Ag. - ¹ to 2Ag - ¹ It exhibits higher reversible specific capacity across the entire current density range. At 0.2 Ag - At a current density of ¹, its discharge specific capacity reaches 534.64 mAh g. - ¹, compared to Zn||MnO2 batteries, it has a higher specific capacity.

[0037] A composite modification layer on the zinc substrate surface utilizes hydrophobic ionic liquid-filled polystyrene colloidal crystals to construct a three-dimensional ordered porous interface structure on the zinc anode surface, effectively controlling the interfacial reaction of the zinc anode in strongly acidic electrolytes. Under strongly acidic conditions, this composite modification layer significantly reduces the direct contact between water molecules and protons and zinc metal through physical isolation, thereby inhibiting hydrogen evolution reaction and chemical corrosion; simultaneously, the formed three-dimensional ordered channels are Zn²⁺. + It provides a continuous and uniform transport path, regulates the zinc ion concentration distribution at the interface, induces uniform zinc deposition, and effectively inhibits dendrite growth. While achieving stable operation of the zinc anode, this protective layer does not significantly hinder Zn²⁺ deposition. + The transport of MnO2 / Mn² can maintain proton-driven MnO2 / Mn² in strong acid electrolytes. + The two-electron conversion reaction enables the battery system to achieve excellent cycle stability while maintaining high voltage output; the acidic aqueous zinc-manganese full cell constructed with zinc anode prepared using this composite modification layer still maintains stable rate performance at high current density.

[0038] It should be understood that the above are merely illustrative examples and do not constitute any limitation on the technical solution of the present invention. In specific applications, those skilled in the art can make settings as needed, and the present invention does not impose any restrictions on this.

[0039] It should be noted that the steps described above are merely illustrative and do not limit the scope of protection of this invention. In practical applications, those skilled in the art can select some or all of them to achieve the purpose of this embodiment according to actual needs, and no restrictions are imposed here. The steps of the method described in this application are not limited to being executed sequentially according to the order in the specification; without changing the core technical solution, the execution order of some steps can be adjusted, or they can be implemented in parallel, or steps can be omitted or added in different scenarios. The above modifications or equivalent substitutions do not affect the substantive content of the technical solution of this application and should all fall within the scope of protection of this application.

[0040] The above description is merely a preferred embodiment of this application and is not intended to limit this application in any way. The scope of protection of this application should be determined by the scope of the claims. Although this application has disclosed the preferred embodiment above, it is not intended to limit this application. Any person skilled in the art can make some modifications or alterations to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the technical solution of this application. Any simple modifications, equivalent changes, and alterations made to the above embodiments based on the technical essence of this application without departing from the content of the technical solution of this application shall fall within the scope of the technical solution of this application.

Claims

1. A zinc negative electrode, characterized in that, It includes a zinc substrate and a composite modification layer coated on the surface of the zinc substrate; the composite modification layer is formed by combining polystyrene microspheres and an ionic liquid, and the thickness of the composite modification layer is 5-30 μm.

2. The zinc negative electrode according to claim 1, characterized in that, The polystyrene microspheres have a particle size of 50-500 nm.

3. The zinc negative electrode according to claim 1, characterized in that, The ionic liquid is at least one of 1-ethyl-3-methylimidazolium bis[(trifluoromethyl)sulfonyl]imide, 1-methyl-3-propylimidazolium bis[(trifluoromethyl)sulfonyl]imide, 1-butyl-3-methylimidazolium bis[(trifluoromethyl)sulfonyl]imide, 1-hexyl-3-methylimidazolium bis[(trifluoromethyl)sulfonyl]imide, 1,3-dimethylimidazolium bis[(trifluoromethyl)sulfonyl]imide, 1-ethyl-3-methylimidazolium tetrafluoroborate, 1-ethyl-3-methylimidazolium hexafluorophosphate, and 1-ethyl-3-methylimidazolium trifluoromethanesulfonate.

4. The zinc negative electrode according to claim 1, characterized in that, In the composite modification layer, the mass ratio of the polystyrene microspheres to the ionic liquid is (0.235-0.94):(7.55-22.65).

5. The zinc negative electrode according to claim 1, characterized in that, The zinc substrate is one of zinc foil or zinc alloy foil, and the thickness of the zinc substrate is 10-200μm.

6. The zinc negative electrode according to claim 1, characterized in that, The composite modification layer has a porous channel structure with a pore size of 10-200 nm.

7. A method for preparing a zinc negative electrode as described in any one of claims 1-6, characterized in that, Includes the following steps: S1. Pre-treated zinc substrate: The zinc substrate is washed in a solvent, removed and dried to obtain the pre-treated zinc substrate; S2. Preparation of polystyrene microsphere dispersion: Dissolve polystyrene microspheres in solvent, stir and disperse evenly to obtain a polystyrene microsphere dispersion with a mass concentration of 0.5-2wt%, i.e., APS dispersion; S3. Preparation of zinc anode: The APS dispersion is added to the pretreated zinc substrate to obtain APS@Zn electrode, and the ionic liquid is added to the APS@Zn electrode to obtain APS-IL@Zn electrode, i.e., zinc anode.

8. The method for preparing the zinc negative electrode according to claim 7, characterized in that, The solvent in S1 is at least one of ethanol, acetone, isopropanol, and toluene, and the drying temperature in S1 is 50-70℃, and the drying time is 3-9h.

9. The method for preparing the zinc negative electrode according to claim 7, characterized in that, In step S3, the assembly amount of the polystyrene microspheres on the pretreated zinc substrate is 0.0053-0.0106 mg / mm². 2 The APS dispersion is added to the pretreated zinc substrate at a temperature of 50-70°C for 1-20 minutes.

10. A battery, characterized in that, Including the zinc anode as described in any one of 1-6.