Process for co-sintering of waste incineration fly ash and multi-source hazardous waste and product thereof

CN122647254APending Publication Date: 2026-08-28ZHEJIANG HELIHEIKO NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610890873.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-06-18
Publication Date
2026-08-28

AI Technical Summary

Technical Problem

该处置模式不仅大量占用土地资源,还面临填埋场库容日渐枯竭的现实压力,同时填埋产生的渗滤液易下渗,存在污染地下水的环境风险

Benefits of technology

[0032]1. This invention rationally proportions various hazardous wastes, including municipal solid waste incineration fly ash, virgin fly ash with varying chlorine content, surface treatment hazardous waste sludge, and aluminum ash, and employs an integrated sintering process for centralized harmless disposal. This effectively reduces plant area requirements, equipment investment, material transfer costs, and operation and maintenance management costs. Through pre-treatment such as chlorine content-based grading of virgin fly ash and fine screening and dehydration of raw materials, different types of hazardous waste react fully and synergistically within the sintering system, significantly improving hazardous waste disposal capacity and effectively expanding the disposal pathways and application scope of hazardous waste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_4
    Figure SMS_4
  • Figure SMS_6
    Figure SMS_6
Patent Text Reader

Abstract

The application discloses a kind of waste incineration fly ash and multi-source hazardous waste collaborative sintering process and its product, belong to garbage processing technical field, first to domestic waste incineration fly ash washing, according to the classification of chlorine content, surface treatment hazardous waste sludge filter pressing dewatering;After mixing various raw materials according to the proportion, water granulation is sprayed, in turn through preheating, high-temperature calcination, cooling to obtain lightweight aggregate.Kiln tail gas is treated by multi-stage purification, dust is used as cement admixture, and desulfurization gypsum is recycled and used as building material raw material.The application reasonably matches domestic waste incineration fly ash, different chlorine content primary fly ash, surface treatment hazardous waste sludge, aluminum ash and other hazardous wastes, and completes centralized harmless disposal by using integrated sintering process, which effectively reduces the factory area, equipment investment, material transfer and operation management cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of waste treatment technology, specifically to a co-sintering process for waste incineration fly ash and multi-source hazardous waste, and its products. Background Technology

[0002] Fly ash from municipal solid waste incineration is classified as HW18 hazardous waste, and the mainstream disposal method in the industry is currently solidification and landfilling. This disposal method not only occupies a large amount of land resources, but also faces the reality of landfill capacity being gradually depleted. In addition, the leachate generated from landfilling is prone to seepage, posing an environmental risk of groundwater pollution.

[0003] Currently, mainstream fly ash sintering technologies generally follow a single-material approach, using only municipal solid waste incineration fly ash as the core raw material for sintering. When faced with multi-source hazardous wastes with significantly different physicochemical properties, such as aluminum ash, surface treatment hazardous waste sludge, and carbon concentrate, existing processes cannot rationally blend them according to the characteristics of different hazardous waste components, making it difficult to achieve the co-feeding and simultaneous harmless treatment of multiple hazardous wastes. Each type of hazardous waste requires a separate treatment line and is processed in batches, which not only significantly increases the plant's land area, equipment investment, material transfer, and operation and maintenance costs.

[0004] Based on this, the present invention designs a co-sintering process for waste incineration fly ash and multi-source hazardous waste and its products to solve the above problems. Summary of the Invention

[0005] To address the aforementioned shortcomings of existing technologies, this invention provides a co-sintering process for waste incineration fly ash and multi-source hazardous waste, comprising the following steps:

[0006] S1: The fly ash from municipal solid waste incineration is washed 2-3 times with water at a solid-liquid mass ratio of 3-5:1 at 20-35℃. The material is then fed into a plate and frame filter press and held under pressure of 0.4-0.6MPa and diaphragm pressing pressure of 1.2-1.6MPa for 25-40 minutes for solid-liquid separation. The solid filter cake is dried with hot air at 80-110℃ for 5-12 minutes and then crushed and passed through a 120-sieve to obtain the washed fly ash from municipal solid waste incineration. The washing wastewater obtained from the separation is sent to a wastewater storage tank, where the pH is adjusted to 7-9. After flocculation and sedimentation pretreatment, part of the pretreatment supernatant is reused in the granulation water replenishment process, and the remaining tailings are transported to a comprehensive wastewater treatment plant.

[0007] After the fly ash from the incineration of raw waste is crushed, it is sieved through a 150-mesh sieve and then further divided into high-chlorine raw fly ash and low-chlorine raw fly ash according to their chlorine content, and stored in separate compartments.

[0008] The aluminum ash, carbon concentrate, lime powder, and carbon black are crushed and then passed through a 130-mesh sieve.

[0009] The surface-treated hazardous waste sludge was dewatered by chamber filter press, and the pressure was maintained for 20-35 minutes at a feed pressure of 0.35-0.5MPa and a diaphragm pressing pressure of 1.1-1.5MPa.

[0010] S2: By weight, weigh 48-54 parts of water-washed municipal solid waste incineration fly ash, 30-38 parts of surface-treated hazardous waste sludge, 2.5-3.5 parts of aluminum ash, 5.5-6.5 parts of carbon concentrate, 4.5-5.5 parts of lime powder, 0-3.5 parts of raw waste incineration fly ash, and 0-15.5 parts of carbon black, and feed them into a closed mixer to mix for 22-35 minutes to obtain a mixture;

[0011] S3: Feed the mixture into the granulator. During the granulation process, inject water at a pressure of 0.3-0.5MPa into the granulator, adding 2-6wt% of the total mass of the mixture to obtain raw material with a particle size of 6-12mm.

[0012] S4: Qualified raw materials are fed from the top of the kiln. The material enters the drying and preheating zone and is preheated for 35-55 minutes at 510-670℃ and -30Pa negative pressure inside the kiln. The flue gas from the drying and preheating zone is controlled by a pressure regulator valve from -30 to -20Pa and then connected to the downstream flue gas treatment pipeline.

[0013] S5: The material in the drying and preheating zone moves down into the high-temperature calcination zone, where it is calcined for 42-65 minutes at 1040-1340℃, with combustion air quantitatively introduced from the bottom of the calcination zone by a variable frequency fan, an air excess coefficient of 1.15-1.35, and a Pa of -90 to -60.

[0014] When the oxygen content in the kiln is below 6%, the fan air volume is increased by 10%; when the oxygen content is above 10%, the fan air volume is decreased by 20%.

[0015] S6: The calcined product descends into the cooling zone and is cooled by blowing in ambient temperature air. The cooling air volume is 1.8-3.2 times the volume of the raw material. It is cooled at 260-320℃ for 28-42 minutes, and the discharge temperature is ≤260℃ to obtain lightweight aggregate.

[0016] S7: A variable frequency induced draft fan is installed at the kiln tail. The speed of the induced draft fan is adjusted according to the negative pressure interlock between the drying preheating zone and the high temperature calcination zone. The flue gas at the kiln tail is sent to the bag filter, the regenerative thermal incinerator, the SNCR denitrification device, and the wet desulfurization tower through a closed pipeline with a pressure regulating valve.

[0017] The inlet flue gas temperature of the bag filter is 140-175℃, and the filter bag operating pressure difference is 800-1400Pa.

[0018] The furnace temperature of the regenerative thermal incineration device is 780-880℃, and the residence time of flue gas inside the device is ≥2.2s;

[0019] SNCR denitrification was carried out by atomizing 25% ammonia water at a pressure of 0.25-0.4 MPa and spraying it into the 850-980℃ temperature zone at the rear end of the calcination zone.

[0020] The wet desulfurization tower uses an 8% lime slurry, and the liquid-to-gas ratio of the desulfurization tower is 9-14 L / Nm³. 3 When the chloride ion concentration in the circulating slurry is >12000 mg / L, the desulfurization tower continuously discharges waste slurry accounting for 3-7% of the total weight, while replenishing with fresh lime slurry; the filter liquid produced by desulfurization is recycled to the fly ash washing process after being dechlorinated and demineralized of heavy metals.

[0021] S8: Dust collected by baghouse dust collectors is used as an admixture in cement production;

[0022] The desulfurized gypsum produced by the wet desulfurization tower is dried and ground, and then reused as a regenerated desulfurizing agent in the desulfurization tower of this process. After three cycles, it is used as a raw material for building gypsum.

[0023] Furthermore, the classification standard for primary fly ash is as follows: primary fly ash with a total chlorine content >15wt% is high-chlorine primary fly ash, and primary fly ash with a total chlorine content ≤15wt% is low-chlorine primary fly ash.

[0024] Furthermore, the S2 raw material ratio is as follows: 48-51 parts of water-washed municipal solid waste incineration fly ash, 32-35 parts of surface-treated hazardous waste sludge, 2.5-3.0 parts of aluminum ash, 5.5-6.0 parts of carbon concentrate, 4.5-5.0 parts of lime powder, and 0-1.0 parts of high-chlorine raw waste incineration fly ash.

[0025] Furthermore, the S2 raw material ratio is as follows: 51-54 parts of water-washed municipal solid waste incineration fly ash, 35-38 parts of surface-treated hazardous waste sludge, 3.0-3.5 parts of aluminum ash, 6.0-6.5 parts of carbon concentrate, 5.0-5.5 parts of lime powder, 2.0-3.5 parts of low-chlorine virgin waste incineration fly ash, and 8.0-15.5 parts of carbon black.

[0026] Furthermore, the calcination temperature of S5 is 1250-1340℃.

[0027] Furthermore, the calcination temperature of S5 is 1040-1220℃.

[0028] A lightweight aggregate prepared by the co-sintering process of waste incineration fly ash and multi-source hazardous waste.

[0029] A dust collector ash produced by the co-sintering process of waste incineration fly ash and multi-source hazardous waste.

[0030] A desulfurized gypsum prepared by the co-sintering process of waste incineration fly ash and multi-source hazardous waste.

[0031] Compared with the prior art, the beneficial effects of this invention are as follows:

[0032] 1. This invention rationally proportions various hazardous wastes, including municipal solid waste incineration fly ash, virgin fly ash with varying chlorine content, surface treatment hazardous waste sludge, and aluminum ash, and employs an integrated sintering process for centralized harmless disposal. This effectively reduces plant area requirements, equipment investment, material transfer costs, and operation and maintenance management costs. Through pre-treatment such as chlorine content-based grading of virgin fly ash and fine screening and dehydration of raw materials, different types of hazardous waste react fully and synergistically within the sintering system, significantly improving hazardous waste disposal capacity and effectively expanding the disposal pathways and application scope of hazardous waste.

[0033] 2. The lightweight aggregate obtained by sintering according to this invention has a dense structure and excellent mechanical properties. Depending on the mix proportions and process parameters, it can be used as building materials such as high-strength precast concrete components, roadbed fillers, and permeable brick raw materials. The dust collected by the bag filter is of stable quality and can be used as an admixture in cement production. The desulfurized gypsum produced by wet desulfurization is first recycled back into the desulfurization system, and after multiple cycles, it is further processed into building material gypsum raw materials. Each product performs its specific function and is utilized in a graded manner, forming a closed-loop resource utilization system with significant economic and environmental benefits.

[0034] 3. This invention employs technologies such as gradient temperature control preheating, high-temperature calcination, and dynamic oxygen content adjustment, combined with multi-stage flue gas purification devices including regenerative thermal combustion, SNCR denitrification, and wet desulfurization. This enables efficient decomposition of dioxins, stable solidification of heavy metals, and effective removal of harmful components such as sulfur and chlorine. The content of heavy metals, dioxins, sulfur, and chlorine in the three products—light aggregate, dust collector ash, and desulfurized gypsum—is maintained at a low level. Detailed Implementation

[0035] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.

[0036] Example 1: This example provides a co-sintering process for waste incineration fly ash and multi-source hazardous waste, including the following steps:

[0037] S1: All raw materials are sampled and tested for heavy metals and dioxins after entering the factory. Materials with excessive levels are stored separately in isolation.

[0038] Materials exceeding the following limits are considered to be substandard: Mercury > 0.1, Cadmium > 0.3, Lead > 10, Total Chromium > 15, Hexavalent Chromium > 5, Arsenic > 1.5, Nickel > 10, Copper > 50, Zinc > 100, Beryllium > 0.02, Antimony > 0.6, Selenium > 1.0, Thallium > 0.3. The total heavy metal control threshold (mg / kg) for raw materials is as follows:

[0039] Dioxins > 3 ng TEQ / kg are considered excessive.

[0040] Municipal solid waste incineration fly ash was washed three times with water at a solid-liquid mass ratio of 5:1 at 35℃. The material was then fed into a plate and frame filter press and subjected to solid-liquid separation at a feed pressure of 0.6MPa and a diaphragm pressing pressure of 1.6MPa for 40 minutes. The solid filter cake was dried with hot air at 110℃ for 12 minutes and then crushed and passed through a 120-sieve to obtain water-washed municipal solid waste incineration fly ash. The separated washing wastewater was sent to a wastewater storage tank, where the pH was adjusted to 7-9. After flocculation and sedimentation pretreatment, part of the pretreatment supernatant was reused in the granulation water replenishment process (S3), and the remaining tailings were transported to a comprehensive wastewater treatment plant.

[0041] After the fly ash from the incineration of raw waste is crushed and passed through a 150-mesh sieve, it is classified as high-chlorine raw fly ash based on the chlorine content, with a total chlorine content >15wt%.

[0042] The aluminum ash, carbon concentrate, lime powder, and carbon black are crushed and then passed through a 130-mesh sieve.

[0043] The surface-treated hazardous waste sludge (HW17 336-064-17) was dewatered by chamber filter press, and the pressure was maintained for 35 minutes at a feed pressure of 0.5 MPa and a diaphragm pressing pressure of 1.5 MPa.

[0044] All materials are stored in separate warehouses in designated areas, with physical partitions separating adjacent warehouses, and are stored in a 28°C storage environment.

[0045] S2: By weight, weigh 51 parts of fly ash from incineration of washed municipal solid waste, 35 parts of sludge from surface treatment hazardous waste, 3.0 parts of aluminum ash, 6.0 parts of carbon concentrate, 5.0 parts of lime powder, and 1.0 part of fly ash from incineration of high-chlorine primary waste.

[0046] S3: Feed the mixture into the granulator. During the granulation process, inject water at a pressure of 0.5 MPa into the granulator, adding 6 wt% of the total mass of the mixture to obtain raw material with a particle size of 6-12 mm.

[0047] S4: Qualified raw materials are fed from the top of the kiln (vertical kiln). The material enters the drying and preheating zone and is preheated for 55 minutes at 670℃ and a negative pressure of -30Pa inside the kiln. The flue gas from the drying and preheating zone is controlled by a pressure regulator valve to a pressure of -20Pa and then connected to the downstream flue gas treatment pipeline.

[0048] S5: The material in the drying preheating zone descends into the high-temperature calcination zone, and is calcined for 65 minutes at 1340℃, with combustion air quantitatively introduced from the bottom of the calcination zone by a variable frequency fan, an air excess coefficient of 1.35, and -60Pa.

[0049] When the oxygen content in the kiln is below 6%, the fan air volume is increased by 10%; when the oxygen content is above 10%, the fan air volume is decreased by 20%.

[0050] S6: The calcined product descends into the cooling zone and is cooled by blowing in ambient temperature air. The cooling air volume is 3.2 times the volume of the raw material. It is cooled at 320℃ for 42 minutes, and the discharge temperature is ≤260℃ to obtain lightweight aggregate.

[0051] The produced lightweight aggregate is a special lightweight aggregate for high-strength concrete and precast components.

[0052] S7: A variable frequency induced draft fan is installed at the kiln tail. The speed of the induced draft fan is adjusted according to the negative pressure interlock between the drying preheating zone and the high temperature calcination zone. The flue gas at the kiln tail is sent to the bag filter, the regenerative thermal incinerator, the SNCR denitrification device, and the wet desulfurization tower through a closed pipeline with a pressure regulating valve.

[0053] The inlet flue gas temperature of the bag filter is 175℃, and the filter bag operating pressure difference is 1400Pa.

[0054] The furnace temperature of the regenerative thermal incineration device is 880℃, and the residence time of flue gas inside the device is ≥2.2s;

[0055] SNCR denitrification was carried out by atomizing 25% ammonia water at a pressure of 0.4 MPa and spraying it into the 980℃ temperature zone at the rear end of the calcination zone.

[0056] The wet desulfurization tower uses 8% lime slurry with a liquid-to-gas ratio of 14 L / Nm³. 3 When the chloride ion concentration in the circulating slurry is greater than 12000 mg / L, the desulfurization tower continuously discharges waste slurry accounting for 7% of the total weight, while replenishing with fresh lime slurry. The filter liquid produced by desulfurization is recycled to the fly ash washing process (S1) after being dechlorinated and demineralized of heavy metals.

[0057] S8: Dust collected by baghouse dust collectors is used as an admixture in cement production;

[0058] The desulfurized gypsum produced by the wet desulfurization tower is dried and ground, and then reused as a regenerated desulfurizing agent in the desulfurization tower of this process. After three cycles, it is used as a raw material for building gypsum.

[0059] Example 2: This example provides a co-sintering process for waste incineration fly ash and multi-source hazardous waste, including the following steps:

[0060] S1: All raw materials are sampled and tested for heavy metals and dioxins after entering the factory. Materials with excessive levels are stored separately in isolation.

[0061] Materials exceeding the following limits are considered to be substandard: Mercury > 0.1, Cadmium > 0.3, Lead > 10, Total Chromium > 15, Hexavalent Chromium > 5, Arsenic > 1.5, Nickel > 10, Copper > 50, Zinc > 100, Beryllium > 0.02, Antimony > 0.6, Selenium > 1.0, Thallium > 0.3. The total heavy metal control threshold (mg / kg) for raw materials is as follows:

[0062] Dioxins > 3 ng TEQ / kg are considered excessive.

[0063] Municipal solid waste incineration fly ash is washed twice with water at 20℃ with a solid-liquid mass ratio of 3:1. The material is then fed into a plate and frame filter press and subjected to solid-liquid separation at a feed pressure of 0.4MPa and a diaphragm pressing pressure of 1.2MPa for 25 minutes. The solid filter cake is dried with hot air at 80℃ for 5 minutes and then crushed and passed through a 120-sieve to obtain washed municipal solid waste incineration fly ash. The separated washing wastewater is sent to a wastewater storage tank, where the pH is adjusted to 7-9. After flocculation and sedimentation pretreatment, part of the pretreatment supernatant is reused in the granulation water replenishment process (S3), and the remaining tailings are transported to a comprehensive wastewater treatment plant.

[0064] The aluminum ash, carbon concentrate, lime powder, and carbon black are crushed and then passed through a 130-mesh sieve.

[0065] The surface-treated hazardous waste sludge (HW17 336-064-17) was dewatered by chamber filter press, and the pressure was maintained for 20 minutes at a feed pressure of 0.35 MPa and a diaphragm pressing pressure of 1.1 MPa.

[0066] All materials are stored in separate warehouses in designated areas, with physical partitions separating adjacent warehouses, and are stored in a 28°C storage environment.

[0067] S2: By weight, weigh 48 parts of fly ash from water-washed municipal solid waste incineration, 32 parts of surface treatment hazardous waste sludge, 2.5 parts of aluminum ash, 5.5 parts of carbon concentrate, and 4.5 parts of lime powder;

[0068] S3: Feed the mixture into the granulator. During the granulation process, inject water at a pressure of 0.3 MPa into the granulator, adding 2 wt% of the total mass of the mixture to obtain raw material with a particle size of 6-12 mm.

[0069] S4: Qualified raw materials are fed from the top of the kiln (vertical kiln). The material enters the drying and preheating zone and is preheated for 35 minutes at 510℃ and -30Pa negative pressure inside the kiln. The flue gas from the drying and preheating zone is controlled by a pressure regulator valve to a pressure of -30Pa and then connected to the downstream flue gas treatment pipeline.

[0070] S5: The material in the drying and preheating zone descends into the high-temperature calcination zone, and is calcined for 42 minutes at 1250℃, with combustion air quantitatively introduced from the bottom of the calcination zone by a variable frequency fan, an air excess coefficient of 1.15, and a temperature of -90℃.

[0071] When the oxygen content in the kiln is below 6%, the fan air volume is increased by 10%; when the oxygen content is above 10%, the fan air volume is decreased by 20%.

[0072] S6: The calcined product descends into the cooling zone and is cooled by blowing in ambient temperature air. The cooling air volume is 1.8 times the volume of the raw material. It is cooled at 260℃ for 28 minutes, and the discharge temperature is ≤260℃ to obtain lightweight aggregate.

[0073] The produced lightweight aggregate is a special lightweight aggregate for high-strength concrete and precast components.

[0074] S7: A variable frequency induced draft fan is installed at the kiln tail. The speed of the induced draft fan is adjusted according to the negative pressure interlock between the drying preheating zone and the high temperature calcination zone. The flue gas at the kiln tail is sent to the bag filter, the regenerative thermal incinerator, the SNCR denitrification device, and the wet desulfurization tower through a closed pipeline with a pressure regulating valve.

[0075] The inlet flue gas temperature of the bag filter is 140℃, and the filter bag operating pressure difference is 800Pa.

[0076] The furnace temperature of the regenerative thermal incineration device is 780℃, and the residence time of flue gas inside the device is ≥2.2s;

[0077] SNCR denitrification was carried out by atomizing 25% ammonia water at a pressure of 0.25 MPa and spraying it into the 850℃ temperature zone at the rear end of the calcination zone.

[0078] The wet desulfurization tower uses 8% lime slurry with a liquid-to-gas ratio of 9 L / Nm³. 3 When the chloride ion concentration in the circulating slurry is greater than 12000 mg / L, the desulfurization tower continuously discharges waste slurry accounting for 3% of the total weight, while replenishing with fresh lime slurry. The filter liquid produced by desulfurization is recycled to the fly ash washing process (S1) after being dechlorinated and demineralized of heavy metals.

[0079] S8: Dust collected by baghouse dust collectors is used as an admixture in cement production;

[0080] The desulfurized gypsum produced by the wet desulfurization tower is dried and ground, and then reused as a regenerated desulfurizing agent in the desulfurization tower of this process. After three cycles, it is used as a raw material for building gypsum.

[0081] Example 3: This example provides a co-sintering process for waste incineration fly ash and multi-source hazardous waste, including the following steps:

[0082] S1: All raw materials are sampled and tested for heavy metals and dioxins after entering the factory. Materials with excessive levels are stored separately in isolation.

[0083] Materials exceeding the following limits are considered to be substandard: Mercury > 0.1, Cadmium > 0.3, Lead > 10, Total Chromium > 15, Hexavalent Chromium > 5, Arsenic > 1.5, Nickel > 10, Copper > 50, Zinc > 100, Beryllium > 0.02, Antimony > 0.6, Selenium > 1.0, Thallium > 0.3. The total heavy metal control threshold (mg / kg) for raw materials is as follows:

[0084] Dioxins > 3 ng TEQ / kg are considered excessive.

[0085] Municipal solid waste incineration fly ash is washed twice with water at 20℃ with a solid-liquid mass ratio of 3:1. The material is then fed into a plate and frame filter press and subjected to solid-liquid separation at a feed pressure of 0.4MPa and a diaphragm pressing pressure of 1.2MPa for 25 minutes. The solid filter cake is dried with hot air at 80℃ for 5 minutes and then crushed and passed through a 120-sieve to obtain washed municipal solid waste incineration fly ash. The separated washing wastewater is sent to a wastewater storage tank, where the pH is adjusted to 7-9. After flocculation and sedimentation pretreatment, part of the pretreatment supernatant is reused in the granulation water replenishment process (S3), and the remaining tailings are transported to a comprehensive wastewater treatment plant.

[0086] After the fly ash from the incineration of raw waste is crushed, it is sieved through a 150-mesh sieve. Based on the chlorine content, the raw fly ash with a total chlorine content of ≤15wt% is classified as low-chlorine raw fly ash.

[0087] The aluminum ash, carbon concentrate, lime powder, and carbon black are crushed and then passed through a 130-mesh sieve.

[0088] The surface-treated hazardous waste sludge (HW17 336-064-17) was dewatered by chamber filter press, and the pressure was maintained for 20 minutes at a feed pressure of 0.35 MPa and a diaphragm pressing pressure of 1.1 MPa.

[0089] All materials are stored in separate warehouses in designated areas, with physical partitions separating adjacent warehouses, and are stored in a 28°C storage environment.

[0090] S2: By weight, weigh 51 parts of water-washed municipal solid waste incineration fly ash, 35 parts of surface treatment hazardous waste sludge, 3.0 parts of aluminum ash, 6.0 parts of carbon concentrate, 5.0 parts of lime powder, 2.0 parts of low-chlorine virgin waste incineration fly ash, and 8.0 parts of carbon black;

[0091] S3: Feed the mixture into the granulator. During the granulation process, inject water at a pressure of 0.3 MPa into the granulator, adding 2 wt% of the total mass of the mixture to obtain raw material with a particle size of 6-12 mm.

[0092] S4: Qualified raw materials are fed from the top of the kiln (vertical kiln). The material enters the drying and preheating zone and is preheated for 35 minutes at 510℃ and -30Pa negative pressure inside the kiln. The flue gas from the drying and preheating zone is controlled by a pressure regulator valve to a pressure of -30Pa and then connected to the downstream flue gas treatment pipeline.

[0093] S5: The material in the drying and preheating zone descends into the high-temperature calcination zone, and is calcined for 42 minutes at 1040℃, with combustion air quantitatively introduced from the bottom of the calcination zone by a variable frequency fan, an air excess coefficient of 1.15, and -90Pa.

[0094] When the oxygen content in the kiln is below 6%, the fan air volume is increased by 10%; when the oxygen content is above 10%, the fan air volume is decreased by 20%.

[0095] S6: The calcined product descends into the cooling zone and is cooled by blowing in ambient temperature air. The cooling air volume is 1.8 times the volume of the raw material. It is cooled at 260℃ for 28 minutes, and the discharge temperature is ≤260℃ to obtain lightweight aggregate.

[0096] The produced lightweight aggregate is used as roadbed filler and permeable brick base material;

[0097] S7: A variable frequency induced draft fan is installed at the kiln tail. The speed of the induced draft fan is adjusted according to the negative pressure interlock between the drying preheating zone and the high temperature calcination zone. The flue gas at the kiln tail is sent to the bag filter, the regenerative thermal incinerator, the SNCR denitrification device, and the wet desulfurization tower through a closed pipeline with a pressure regulating valve.

[0098] The inlet flue gas temperature of the bag filter is 140℃, and the filter bag operating pressure difference is 800Pa.

[0099] The furnace temperature of the regenerative thermal incineration device is 780℃, and the residence time of flue gas inside the device is ≥2.2s;

[0100] SNCR denitrification was carried out by atomizing 25% ammonia water at a pressure of 0.25 MPa and spraying it into the 850℃ temperature zone at the rear end of the calcination zone.

[0101] The wet desulfurization tower uses 8% lime slurry with a liquid-to-gas ratio of 9 L / Nm³. 3 When the chloride ion concentration in the circulating slurry is greater than 12000 mg / L, the desulfurization tower continuously discharges waste slurry accounting for 3% of the total weight, while replenishing with fresh lime slurry. The filter liquid produced by desulfurization is recycled to the fly ash washing process (S1) after being dechlorinated and demineralized of heavy metals.

[0102] S8: Dust collected by baghouse dust collectors is used as an admixture in cement production;

[0103] The desulfurized gypsum produced by the wet desulfurization tower is dried and ground, and then reused as a regenerated desulfurizing agent in the desulfurization tower of this process. After three cycles, it is used as a raw material for building gypsum.

[0104] Example 4: This example provides a co-sintering process for waste incineration fly ash and multi-source hazardous waste, including the following steps:

[0105] S1: All raw materials are sampled and tested for heavy metals and dioxins after entering the factory. Materials with excessive levels are stored separately in isolation.

[0106] Materials exceeding the following limits are considered to be substandard: Mercury > 0.1, Cadmium > 0.3, Lead > 10, Total Chromium > 15, Hexavalent Chromium > 5, Arsenic > 1.5, Nickel > 10, Copper > 50, Zinc > 100, Beryllium > 0.02, Antimony > 0.6, Selenium > 1.0, Thallium > 0.3. The total heavy metal control threshold (mg / kg) for raw materials is as follows:

[0107] Dioxins > 3 ng TEQ / kg are considered excessive.

[0108] Municipal solid waste incineration fly ash is washed twice with water at 20℃ with a solid-liquid mass ratio of 3:1. The material is then fed into a plate and frame filter press and subjected to solid-liquid separation at a feed pressure of 0.4MPa and a diaphragm pressing pressure of 1.2MPa for 25 minutes. The solid filter cake is dried with hot air at 80℃ for 5 minutes and then crushed and passed through a 120-sieve to obtain washed municipal solid waste incineration fly ash. The separated washing wastewater is sent to a wastewater storage tank, where the pH is adjusted to 7-9. After flocculation and sedimentation pretreatment, part of the pretreatment supernatant is reused in the granulation water replenishment process (S3), and the remaining tailings are transported to a comprehensive wastewater treatment plant.

[0109] After the fly ash from the incineration of raw waste is crushed, it is sieved through a 150-mesh sieve. Based on the chlorine content, the raw fly ash with a total chlorine content of ≤15wt% is classified as low-chlorine raw fly ash.

[0110] The aluminum ash, carbon concentrate, lime powder, and carbon black are crushed and then passed through a 130-mesh sieve.

[0111] The surface-treated hazardous waste sludge (HW17 336-064-17) was dewatered by chamber filter press, and the pressure was maintained for 20 minutes at a feed pressure of 0.35 MPa and a diaphragm pressing pressure of 1.1 MPa.

[0112] All materials are stored in separate warehouses in designated areas, with physical partitions separating adjacent warehouses, and are stored in a 28°C storage environment.

[0113] S2: By weight, weigh 54 parts of water-washed municipal solid waste incineration fly ash, 38 parts of surface treatment hazardous waste sludge, 3.5 parts of aluminum ash, 6.5 parts of carbon concentrate, 5.5 parts of lime powder, 3.5 parts of low-chlorine raw waste incineration fly ash, and 15.5 parts of carbon black.

[0114] S3: Feed the mixture into the granulator. During the granulation process, inject water at a pressure of 0.3 MPa into the granulator, adding 2 wt% of the total mass of the mixture to obtain raw material with a particle size of 6-12 mm.

[0115] S4: Qualified raw materials are fed from the top of the kiln (vertical kiln). The material enters the drying and preheating zone and is preheated for 35 minutes at 510℃ and -30Pa negative pressure inside the kiln. The flue gas from the drying and preheating zone is controlled by a pressure regulator valve to a pressure of -30Pa and then connected to the downstream flue gas treatment pipeline.

[0116] S5: The material in the drying and preheating zone descends into the high-temperature calcination zone, and is calcined for 42 minutes at 1220℃, with combustion air quantitatively introduced from the bottom of the calcination zone by a variable frequency fan, an air excess coefficient of 1.15, and -90Pa.

[0117] When the oxygen content in the kiln is below 6%, the fan air volume is increased by 10%; when the oxygen content is above 10%, the fan air volume is decreased by 20%.

[0118] S6: The calcined product descends into the cooling zone and is cooled by blowing in ambient temperature air. The cooling air volume is 1.8 times the volume of the raw material. It is cooled at 260℃ for 28 minutes, and the discharge temperature is ≤260℃ to obtain lightweight aggregate.

[0119] The produced lightweight aggregate is used as roadbed filler and permeable brick base material;

[0120] S7: A variable frequency induced draft fan is installed at the kiln tail. The speed of the induced draft fan is adjusted according to the negative pressure interlock between the drying preheating zone and the high temperature calcination zone. The flue gas at the kiln tail is sent to the bag filter, the regenerative thermal incinerator, the SNCR denitrification device, and the wet desulfurization tower through a closed pipeline with a pressure regulating valve.

[0121] The inlet flue gas temperature of the bag filter is 140℃, and the filter bag operating pressure difference is 800Pa.

[0122] The furnace temperature of the regenerative thermal incineration device is 780℃, and the residence time of flue gas inside the device is ≥2.2s;

[0123] SNCR denitrification was carried out by atomizing 25% ammonia water at a pressure of 0.25 MPa and spraying it into the 850℃ temperature zone at the rear end of the calcination zone.

[0124] The wet desulfurization tower uses 8% lime slurry with a liquid-to-gas ratio of 9 L / Nm³. 3 When the chloride ion concentration in the circulating slurry is greater than 12000 mg / L, the desulfurization tower continuously discharges waste slurry accounting for 3% of the total weight, while replenishing with fresh lime slurry. The filter liquid produced by desulfurization is recycled to the fly ash washing process (S1) after being dechlorinated and demineralized of heavy metals.

[0125] S8: Dust collected by baghouse dust collectors is used as an admixture in cement production;

[0126] The desulfurized gypsum produced by the wet desulfurization tower is dried and ground, and then reused as a regenerated desulfurizing agent in the desulfurization tower of this process. After three cycles, it is used as a raw material for building gypsum.

[0127] Comparative Example 1: The difference between this comparative example and Example 1 is that the step of subdividing municipal solid waste incineration fly ash into high-chlorine primary fly ash and low-chlorine primary fly ash according to the chlorine content in step S1 is omitted, and primary fly ash is directly used in the batching.

[0128] Comparative Example 2: The difference between this comparative example and Example 1 is that the calcination temperature was adjusted from 1340°C to 900°C.

[0129] Comparative Example 3: The difference between this comparative example and Example 4 is that the functional core raw material lime powder is removed, while the proportions of the remaining materials remain unchanged.

[0130] Comparative Example 4: The difference between this comparative example and Example 4 is that the regenerative thermal incineration device in S7 is shut down, and the flue gas directly skips the device and enters the subsequent bag filter dust collector, SNCR denitrification and wet desulfurization.

[0131] Experiment Example 1: Safety Testing;

[0132] (1) The heavy metal content (mg / kg) of the dust collected by each group of bag filters was tested according to HJ 766, and the dioxin toxicity equivalent of the dust collected by each group of bag filters was tested according to HJ77.3. The chlorine and sulfur content (mg / kg) of the dust collected by each group of bag filters was tested according to HJ 84, and the results are shown in Table 1.

[0133] Table 1:

[0134]

[0135] As shown in the table above, the pollutant indicators of the dust prepared in the examples are all at extremely low levels. The dioxin toxicity equivalent of the dust in all examples is controlled within 1.1 ng TEQ / kg. The contents of various heavy metals such as mercury, cadmium, lead, and arsenic are far below the raw material entry control threshold. The sulfur and chlorine contents are also stable within a reasonable range. The differences in indicators between examples with different raw material ratios are small. This fully demonstrates that the entire process of raw material pretreatment, precise batching, high-temperature calcination, and multi-stage flue gas treatment of the present invention has a significant effect on the control of pollutants such as heavy metals, dioxins, chlorine, and sulfur in dust, and can stably produce dust products that meet the requirements of cement production admixtures.

[0136] Compared with the example, all pollutant indicators in Comparative Example 1 showed a slight increase. The content of heavy metals such as mercury, cadmium, and lead increased by about 5-0%, and the dioxin toxicity equivalent and sulfur and chlorine content were also slightly higher than those in the example group. This indicates that the graded control step for the chlorine content of the primary fly ash set in this invention can effectively reduce the fluctuation of chlorine content in the batching system, reduce the volatilization and migration of heavy metals and the secondary generation of dioxins during calcination, and is a key pre-process to ensure the stability of the quality of dust removal ash products.

[0137] Comparative Example 2 showed a significant increase in all pollutant indicators. The contents of core heavy metals such as mercury, cadmium, and lead increased by more than 50% compared to the previous example. The dioxin toxicity equivalent reached 1.55 ng TEQ / kg, 1.6 times that of Example 1. Sulfur and chlorine contents also increased substantially. These results demonstrate the scientific validity of the 1040-1340℃ calcination temperature range of this invention. This temperature range is the core parameter for achieving heavy metal lattice solidification and high-temperature dioxin decomposition. Insufficient calcination temperature leads to incomplete sintering of the material, significantly reducing the decomposition and solidification effects of pollutants, directly causing the dust pollutant content to exceed the standard.

[0138] Compared with Examples 3 and 4, some heavy metal indicators in Comparative Example 3 showed a slight increase, and the chlorine and sulfur contents also showed a significant increase. This indicates that lime powder, as the core functional raw material of the batching system of this invention, plays multiple roles in regulating the alkalinity of the system, fixing sulfur and chlorine, and stabilizing heavy metals during the calcination process. At the same time, it can optimize the melting effect of the sintering system. The lack of lime powder will directly lead to a decrease in the pollutant control capability of the sintering system, resulting in an increase in the chlorine, sulfur and heavy metal contents in the dust.

[0139] Comparative Example 4 showed a comprehensive and significant deterioration in all pollutant indicators. The levels of heavy metals such as mercury, cadmium, and lead were approximately twice that of Example 1, and the dioxin toxicity equivalent reached 1.85 ng TEQ / kg, 1.9 times that of Example 1. Sulfur and chlorine levels also reached 2051 mg / kg and 1050 mg / kg, respectively, far exceeding all other example groups. This demonstrates that the regenerative thermal incineration process is the core component of the flue gas treatment in this invention, effectively decomposing dioxins and unburned organic matter in the flue gas while removing most gaseous heavy metals. The absence of this process would lead to a complete collapse of the flue gas treatment effect.

[0140] (2) Detect the heavy metal content (×10) of each group of desulfurized gypsum. -3 mg / kg), dioxin toxicity equivalent The results of the chlorine and sulfur content (mg / kg) are shown in Table 2.

[0141] Table 2:

[0142]

[0143] As shown in the table above, the desulfurized gypsum prepared in Examples 1-4 exhibits excellent overall performance in terms of the content of heavy metals, dioxins, and chlorine-sulfur, fully meeting the requirements for use as a regenerated desulfurizing agent and building material gypsum raw material. The dioxin toxicity equivalent of the desulfurized gypsum in all examples was controlled below 13 ng TEQ / kg.

[0144] Compared to the examples, the pollutant indicators of the desulfurization gypsum in Comparative Example 1 showed a slight increase. The content of heavy metals such as mercury, cadmium, and lead increased by approximately 3-8%, and the dioxin toxicity equivalent and sulfur and chlorine content were also slightly higher. This indicates that graded control of the chlorine content in primary fly ash can effectively reduce the chlorine content entering the flue gas, lower the chlorine concentration in the desulfurization tower circulating slurry, and reduce the entrainment of chlorine and heavy metals in the desulfurization gypsum, which is a crucial step in ensuring the quality of desulfurization gypsum products.

[0145] In Comparative Example 2, the various pollutant indicators of the desulfurized gypsum showed a significant increase, with the lead content reaching 118.9 × 10⁻⁶. - 3The concentration of dioxins in the flue gas was 1.6 times that of Example 1, reaching a dioxin toxicity equivalent of 15.97 ng TEQ / kg. Sulfur and chlorine contents also showed a significant increase. This indicates that insufficient calcination temperature leads to a substantial increase in the content of heavy metals, dioxins, and sulfur oxides in the flue gas, directly increasing the treatment load of the desulfurization system and causing a significant increase in the pollutant content in the desulfurization gypsum.

[0146] Compared with the example, the heavy metal content of the desulfurized gypsum in Comparative Example 3 increased slightly, and the chlorine content also increased significantly. This indicates that the lack of lime powder leads to insufficient basicity in the sintering system, a significant decrease in the fixation effect of sulfur and chlorine during calcination, and a significant increase in the sulfur and chlorine content entering the flue gas.

[0147] In Comparative Example 4, the various pollutant indicators of the desulfurized gypsum showed a comprehensive and significant deterioration, with the lead content reaching 162.3 × 10⁻⁶. -3 The concentration of dioxins in the flue gas was 2.2 times that of Example 1, and the dioxin toxicity equivalent was as high as 20.54 ng TEQ / kg, which was 1.8 times that of Example 1. The chlorine and sulfur contents also reached 1578 mg / kg and 1919 mg / kg, respectively, which were far higher than those in all example groups. This proves that the lack of regenerative thermal incineration technology will lead to the ineffective decomposition of dioxins, heavy metals and organic matter in the flue gas, which will directly enter the desulfurization system and be entrained in large quantities in the desulfurization gypsum.

[0148] (3) Detect the heavy metal content (×10) in each group of lightweight aggregates. -3 (mg / kg) and dioxin toxicity equivalent The results are shown in Table 3.

[0149] Table 3:

[0150]

[0151] As shown in the table above, the lightweight aggregates prepared in Examples 1-4 have extremely low levels of heavy metals, dioxins, chlorine, and sulfur. The dioxin toxicity equivalent of the lightweight aggregates in all examples is controlled within 15 ng TEQ / kg, and the chlorine and sulfur contents are also stable within a reasonable range.

[0152] Compared to the examples, all pollutant indicators of the lightweight aggregate in Comparative Example 1 showed a slight increase. The content of heavy metals such as mercury, cadmium, and lead increased by approximately 4-9%, and the dioxin toxicity equivalent and sulfur-chlorine content were also slightly higher. This indicates that graded control of the chlorine content in virgin fly ash can effectively reduce fluctuations in the chlorine content of the batching system, prevent excessive chlorine content from causing the volatilization and migration of heavy metals during calcination, and improve the solidification effect of heavy metals in lightweight aggregates. This is a key step in ensuring the environmental safety of lightweight aggregate products.

[0153] Comparative Example 2 showed a significant increase in various pollutant indicators in the lightweight aggregate, with lead content reaching 0.7 × 10⁻⁶.-3 The concentration of dioxins reached 20.15 ng TEQ / kg, 1.75 times that of Example 1, and the dioxin toxicity equivalent reached 20.15 ng TEQ / kg, 1.5 times that of Example 1. The contents of core heavy metals such as chromium, nickel, and manganese also showed a significant increase. These results fully verify that the calcination temperature range of 1040-1340℃ is crucial for achieving sintering densification of lightweight aggregates, solidification of heavy metal lattices, and high-temperature decomposition of dioxins. Insufficient temperature leads to incomplete sintering of materials and inadequate decomposition of dioxins, ultimately resulting in a significant increase in the pollutant content of lightweight aggregates.

[0154] Compared to the example, the heavy metal content of the lightweight aggregate in Comparative Example 3 showed a slight increase compared to the example, and the chlorine and sulfur content also increased significantly. This indicates that lime powder, as the core flux and alkalinity regulator of the sintering system, can effectively reduce the melting temperature of the material, increase the amount of liquid phase generated during calcination, enhance the bonding effect between particles, and combine with elements such as sulfur and chlorine to achieve sulfur and chlorine fixation. The lack of lime powder will directly lead to a decrease in sintering effect, a poorer solidification effect of heavy metals, and an increase in the pollutant content of the lightweight aggregate.

[0155] In Comparative Example 4, all pollutant indicators of the lightweight aggregate showed a significant and comprehensive deterioration, with the lead content reaching 207.6 × 10⁻⁶. -3 The concentration of dioxins in the flue gas was 519 times that of Example 1, and the dioxin toxicity equivalent was also much higher than that of the Example group. The content of core heavy metals such as chromium, nickel, and manganese also increased significantly. This proves that the lack of regenerative thermal incineration technology will result in the ineffective decomposition and removal of dioxins and heavy metals in the kiln tail flue gas. Some pollutants will flow back into the kiln with the flue gas and re-enter the sintering products, ultimately causing the pollutant content of the lightweight aggregate to exceed the standard.

[0156] Experiment Example 2: Performance Testing;

[0157] The performance of each group of lightweight aggregates was tested according to GB / T 17431, and the specific results are shown in Table 4.

[0158] Table 4:

[0159]

[0160] As can be seen from the table above, the lightweight aggregates prepared in Examples 1-4 exhibit excellent overall performance, and all performance indicators fully meet the relevant requirements of GB / T17431 "Lightweight Aggregates and Their Test Methods".

[0161] Compared with the example, all performance indicators of the lightweight aggregate in Comparative Example 1 showed a slight decrease, with a slight decrease in cylinder compressive strength and a slight increase in mud content, mud content, and water absorption. This indicates that graded control of the chlorine content of the virgin fly ash can effectively reduce the fluctuation of chlorine content in the batching system, and avoid uneven melting of materials during calcination due to excessive chlorine content, which would affect the structural density and mechanical properties of the lightweight aggregate.

[0162] In Comparative Example 2, all performance indicators of the lightweight aggregate showed a significant decline, with the compressive strength of the cylinder only 3.2 MPa, which is 62.7% of that in Example 1, and the density grade increased to 1320 kg / m³. 3 The water absorption rate, mud content, and mud content all increased significantly, and the softening coefficient was only 0.65, far lower than the level of over 0.95 in the previous example. This indicates that the calcination temperature range of 1040-1340℃ is the core for achieving sintering and densification of lightweight aggregates and forming a stable glassy structure. Insufficient temperature will lead to insufficient melting of materials, poor bonding between particles, loose product structure, and a significant decrease in mechanical properties, water resistance, and durability.

[0163] The performance indicators of the lightweight aggregate in Comparative Example 3 showed a significant decline. The compressive strength was only 3.8 MPa, 88.4% of that in Example 4. The density grade increased, while the water absorption and mud content both increased slightly, and the softening coefficient decreased to 0.75. This indicates that lime powder, as the core flux in the sintering system, can effectively reduce the melting temperature of the material, increase the amount of liquid phase generated during calcination, enhance the bonding effect between particles, and form a denser product structure. The lack of lime powder directly leads to a decrease in sintering effect, and the mechanical properties and water resistance of the product deteriorate significantly.

[0164] The performance indicators of the lightweight aggregate in Comparative Example 4 showed a comprehensive and significant deterioration, with the compressive strength of the cylinder only 2.5 MPa, which is 49% of that in Example 1, and the density grade increased to 1450 kg / m³. 3 The mud content, mud content, and water absorption rate all reached the highest values ​​among all groups, with a softening coefficient of only 0.52, far below the national standard requirements. This proves that the lack of regenerative thermal incineration technology leads to the ineffective decomposition of unburned organic matter and dioxins in the kiln tail flue gas. Some organic matter will flow back into the kiln with the flue gas and undergo secondary combustion during calcination, causing an unstable temperature field in the kiln and uneven sintering of materials. At the same time, unburned carbon will remain in the lightweight aggregate, resulting in a loose product structure and a serious decline in mechanical properties, water resistance, and durability.

[0165] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features. Such modifications or substitutions will not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A co-sintering process for waste incineration fly ash and multi-source hazardous waste, characterized in that, Includes the following steps: S1: The fly ash from municipal solid waste incineration is washed with water and then subjected to solid-liquid separation. The filter cake is dried, crushed, and sieved to obtain washed municipal solid waste incineration fly ash. The fly ash from raw waste incineration is crushed and sieved, and then subdivided into high-chlorine raw fly ash and low-chlorine raw fly ash according to the chlorine content. The surface-treated hazardous waste sludge is dewatered by pressure filtration. S2: By weight, weigh 48-54 parts of water-washed municipal solid waste incineration fly ash, 30-38 parts of surface-treated hazardous waste sludge, 2.5-3.5 parts of aluminum ash, 5.5-6.5 parts of carbon concentrate, 4.5-5.5 parts of lime powder, 0-3.5 parts of raw waste incineration fly ash, and 0-15.5 parts of carbon black, and mix them to obtain the mixture. S3: Spray water onto the mixture and granulate it to obtain raw meal; S4: Preheat raw materials at 510-670℃ for 35-55 minutes; S5: Calcination at 1040-1340℃ for 42-65 min; S6: Cool at 260-320℃ for 28-42 minutes to obtain lightweight aggregate; S7: The kiln tail flue gas is sequentially fed into a bag filter, a regenerative thermal ignition device, an SNCR denitrification device, and a wet desulfurization tower. S8: The dust collected by the bag filter is used as an admixture in cement production; the desulfurized gypsum produced by the wet desulfurization tower is dried and ground and then recycled as a desulfurizing agent for the desulfurization tower in this process. After three cycles, it is used as a raw material for building gypsum.

2. The co-sintering process for waste incineration fly ash and multi-source hazardous waste according to claim 1, characterized in that, The classification standard for primary fly ash is as follows: primary fly ash with a total chlorine content >15wt% is high-chlorine primary fly ash, and primary fly ash with a total chlorine content ≤15wt% is low-chlorine primary fly ash.

3. The co-sintering process for waste incineration fly ash and multi-source hazardous waste according to claim 2, characterized in that, The S2 raw material ratio is: 48-51 parts of water-washed municipal solid waste incineration fly ash, 32-35 parts of surface treatment hazardous waste sludge, 2.5-3.0 parts of aluminum ash, 5.5-6.0 parts of carbon concentrate, 4.5-5.0 parts of lime powder, and 0-1.0 parts of high-chlorine raw waste incineration fly ash.

4. The co-sintering process for waste incineration fly ash and multi-source hazardous waste according to claim 3, characterized in that, The S2 raw material ratio is as follows: 51-54 parts of water-washed municipal solid waste incineration fly ash, 35-38 parts of surface treatment hazardous waste sludge, 3.0-3.5 parts of aluminum ash, 6.0-6.5 parts of carbon concentrate, 5.0-5.5 parts of lime powder, 2.0-3.5 parts of low-chlorine virgin waste incineration fly ash, and 8.0-15.5 parts of carbon black.

5. The co-sintering process for waste incineration fly ash and multi-source hazardous waste according to claim 4, characterized in that, The calcination temperature of S5 is 1250-1340℃.

6. The co-sintering process for waste incineration fly ash and multi-source hazardous waste according to claim 5, characterized in that, S5 calcination temperature: 1040-1220℃.

7. A lightweight aggregate prepared by the co-sintering process of waste incineration fly ash and multi-source hazardous waste according to any one of claims 1-6.

8. A dust collector ash obtained by the co-sintering process of waste incineration fly ash and multi-source hazardous waste according to any one of claims 1-6.

9. A desulfurized gypsum prepared by the co-sintering process of waste incineration fly ash and multi-source hazardous waste according to any one of claims 1-6.