Method for determining rhodium content in high-impurity material
By using low-concentration sodium chloride activation and hydrochloric acid leaching, the stability and accuracy issues in the determination of rhodium content in complex materials were resolved, enabling accurate determination of rhodium content in complex materials. This method is suitable for standardized batch determination of complex materials.
Patent Information
- Application Number
- CN202611587284.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-14
- Publication Date
- 2026-11-10
AI Technical Summary
Existing technologies cannot effectively solve the problem of determining the rhodium content in high-impurity materials, especially the measurement failure and data distortion caused by the failure of nickel buckles in water crushing, and the lack of stability and accuracy.
A low-concentration sodium chloride system was used to activate and break down the film and etch the grain boundaries of the nickel matte. Combined with hydrochloric acid leaching and aqua regia digestion, the rhodium content was determined by ICP-MS to ensure accurate determination.
It enables accurate and stable determination of rhodium content in complex materials, avoids measurement failure caused by nickel foil failure due to water breakage, improves measurement efficiency and data accuracy, and is suitable for batch standardized determination of complex materials.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention relates to the field of metal analysis and detection technology, specifically to a method for determining the rhodium content in highly impure materials. Background Technology
[0002] Currently, nickel matte assay enrichment-inductively coupled plasma mass spectrometry (ICP-MS) is the mainstream core technology for rhodium content determination. Relying on the ultra-high selective trapping ability of nickel matte relative to rhodium, rhodium can be effectively separated and enriched from high-impurity materials, greatly eliminating matrix interference and meeting the instrumental requirements for accurate determination of trace and ultra-low rhodium. However, high-impurity materials generally have the characteristics of complex impurity composition and large content fluctuations, with high contents of impurities such as sulfur, copper, iron, and organic matter. During the high-temperature melting process of nickel matte assay, it is very easy to cause an imbalance in the sulfur-nickel ratio of the assay system and abnormal reduction potential of the system. Coupled with process fluctuations such as excessively high melting temperature, excessive holding time, and excessively slow cooling rate, a large amount of metallic nickel phase and copper-nickel tough solid solution will be generated inside the nickel matte, resulting in a dense and coarse grain structure and the formation of a dense inert oxide passivation film on the surface, ultimately forming a metallized hardened failed nickel matte.
[0003] Current mainstream methods for determining platinum group elements mostly focus on the determination of multiple elements such as platinum, palladium, rhodium, and iridium. They have not established a dedicated non-destructive recovery and complete determination system for the frequent failure of nickel clips due to water breakage in high-impurity materials. Nickel clip failure occurs frequently during the determination of high-impurity materials, which can easily lead to rhodium determination failure and data invalidation. Existing methods have poor stability and insufficient targeting, and cannot meet the needs of accurate batch determination of trace rhodium in high-impurity materials.
[0004] In view of this, it is necessary to design a method for determining the rhodium content in high-impurity materials in order to solve the above problems. Summary of the Invention
[0005] In view of the technical problems existing in the background art, the present invention provides a method for determining the rhodium content in high-impurity materials. The method uses a low-concentration sodium chloride system to activate and break the film and induce grain boundary corrosion. There is no large amount of salt residue and the rhodium element occurrence state is not changed. It is fully compatible with subsequent hydrochloric acid leaching, aqua regia digestion and ICP-MS accurate determination process. It completely solves the problem of rhodium determination failure and data distortion caused by the failure of nickel buckle water in high-impurity materials, and ensures the accuracy and stability of trace rhodium content determination in high-impurity materials.
[0006] This invention provides a method for determining the rhodium content in high-impurity materials, comprising: Weigh the sample of high-impurity material into a crucible, add the molten ingredients, and obtain the crucible with the prepared ingredients; The prepared crucible is melted and then subjected to a first cooling treatment to obtain nickel matte. The nickel matte was immersed in a sodium chloride aqueous solution and soaked at a constant temperature to obtain loose nickel matte; the mass fraction of sodium chloride in the sodium chloride aqueous solution was 1%~3%, and the constant temperature soaking temperature was 80℃~100℃; Loose nickel matte was immersed in hydrochloric acid solution for leaching, and then subjected to a second cooling treatment to obtain rhodium-enriched residue. The rhodium enrichment residue was digested by heating with aqua regia, and after a third cooling treatment, the rhodium content in the high-impurity material sample was determined by ICP-MS.
[0007] As a further improvement of the present invention, the impurities in the high-impurity material sample include at least one of sulfur, copper, iron, and organic matter; and / or, The mass of the high-impurity material sample is 5.00g~10.00g.
[0008] As a further improvement of the present invention, the addition of molten materials includes: adding basic nickel carbonate, sublimed sulfur, sodium carbonate, borax, ferrous sulfide, and silicon dioxide, mixing thoroughly, and then covering the surface with a covering agent; wherein the mass of basic nickel carbonate is 10g~20g; and / or, The mass of sublimed sulfur is 1g to 2g; and / or, The mass of sodium carbonate is 30g~40g; and / or, The mass of borax is 10g~15g; and / or, The mass of ferrous sulfide is 0 g to 12 g; and / or, The mass of silicon dioxide is 0g~10g; and / or, The covering agent contains sodium carbonate and borax, with a sodium carbonate to borax mass ratio of 1.8-2.2:1; and / or, The thickness of the covering agent is 8mm~12mm.
[0009] As a further improvement of the present invention, the melting process includes: placing the prepared refractory clay crucible in a fire assay furnace and heating it to a constant temperature for melting. The initial temperature of the fire assay furnace is 940℃~960℃; and / or, The heating rate is 5℃ / min to 10℃ / min; and / or, The constant temperature is 1050℃~1100℃; and / or, The melting time is 20-30 minutes.
[0010] As a further improvement of the present invention, the first cooling process includes: after melting, pouring into a cast iron mold, cooling, and separating.
[0011] As a further improvement of the present invention, the constant temperature soaking time is 2h~4h.
[0012] As a further improvement of the present invention, the concentration of the hydrochloric acid solution is 11.5 mol / L to 12.5 mol / L; and / or, The immersion temperature is 145℃~155℃; and / or, The temperature for heat digestion is 110℃~130℃; and / or, The heating and digestion time is 2 to 4 hours.
[0013] As a further improvement of the present invention, the second cooling process includes: after leaching, cooling and filtering to remove the filtrate to obtain rhodium-enriched residue; the third cooling process includes: after heating and digestion, cooling to room temperature and making up to volume with ultrapure water.
[0014] As a further improvement of the present invention, the ICP-MS determination includes: after heating and digestion, transferring the solution to a volumetric flask and making up to volume to obtain a test solution; taking a rhodium standard solution and determining and plotting a standard curve; adding an indium internal standard solution to the blank solution, standard solution and test solution, determining the rhodium element intensity in the test solution and blank solution, and determining the mass concentration of rhodium on the standard curve.
[0015] As a further improvement of the present invention, the formula for calculating the rhodium content in a high-impurity material sample is as follows: in, w i This refers to the rhodium content; r 1 The mass concentration of rhodium in the test solution is determined from the standard solution. r 2 The mass concentration of rhodium in the blank solution is determined by comparing it with the standard solution. V 1 This represents the volume of the solution after heating and digestion. V 2 This refers to the total volume of the test solution; V 3 m1 represents the volume of the test solution after dilution; m2 represents the mass of the sample containing high levels of impurities.
[0016] The beneficial technical effects of this invention are as follows: First, this invention innovatively constructs a method for determining rhodium content in highly impure materials. It is the first to integrate a wet sodium chloride thermal activation process into the rhodium determination procedure for nickel matte, specifically addressing the industry pain point of water-induced failure of nickel ingots smelted from highly impure materials such as high sulfur, high copper, high iron, and high organic matter. It achieves non-destructive loosening of water-damaged hard nickel ingots, eliminating the need for mechanical crushing and completely resolving the issues of poor precision and accuracy in traditional methods. Simultaneously, it significantly improves the efficiency of rhodium determination in highly impure materials and reduces testing costs. Furthermore, it completely avoids mechanical striking operations, fundamentally preventing cross-contamination of samples, loss of fine rhodium particles, and matrix encapsulation residues, thus significantly improving the rhodium content determination efficiency in highly impure materials. The method offers several advantages: firstly, it ensures stability and data accuracy; secondly, it employs a low-concentration sodium chloride activation system, which only activates and loosens the material, leaving no harmful impurities and not interfering with subsequent acid leaching, digestion, and precise ICP-MS determination processes. The method boasts strong compatibility and high stability. Finally, this invention is adaptable to various complex and highly impure materials, overcoming the limitations of traditional methods which are only suitable for low-impurity conventional ores and exhibit poor stability in rhodium determination for highly impure materials. This significantly broadens the applicability of rhodium determination methods without requiring modifications to existing equipment. The method is simple to operate, highly stable, and suitable for standardized batch determination of samples such as highly impure ores from mines and highly impure intermediate materials from metallurgy, making it easy to promote and apply in the industry.
[0017] The above description is only an overview of the technical solution of this application. In order to better understand the technical means of this application and to implement it in accordance with the contents of the specification, and to make the above and other objects, features and advantages of this application more obvious and understandable, the following are specific embodiments of this application. Detailed Implementation
[0018] The embodiments of the technical solution of this application will be described in detail below. The following embodiments are only used to illustrate the technical solution of this application more clearly, and are therefore only examples, and should not be used to limit the scope of protection of this application.
[0019] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains; the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the application; the terms “comprising” and “having”, and any variations thereof, in the specification and claims of this application are intended to cover non-exclusive inclusion.
[0020] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments.
[0021] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also included. Furthermore, if minimum range values of 1 and 2 are listed, and if maximum range values of 3, 4, and 5 are listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0022] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.
[0023] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions.
[0024] Unless otherwise specified, the terms "comprising" and "including" as used in this application are open-ended. For example, "comprising" and "including" may mean that other components not listed may also be included or contained.
[0025] In the description of the embodiments in this application, the term "and / or" is merely a description of the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, and B existing alone. Additionally, the character " / " in this document generally indicates that the preceding and following related objects have an "or" relationship.
[0026] The embodiments of this application will be described in further detail below with reference to the examples. The detailed description of the following embodiments is used to illustrate the principles of this application, but should not be used to limit the scope of this application, that is, this application is not limited to the described embodiments.
[0027] Current mainstream methods for determining platinum group elements mostly focus on the determination of multiple elements such as platinum, palladium, rhodium, and iridium. They lack a dedicated non-destructive repair and complete determination system to address the frequent nickel clip failure caused by water breakage in highly impure materials. The frequent nickel clip failure during the determination of highly impure materials easily leads to rhodium determination failure. Existing methods suffer from poor stability and insufficient targeting, failing to meet the demand for accurate batch determination of trace rhodium in highly impure materials. Therefore, it is necessary to design a method for determining the rhodium content in highly impure materials to solve the above problems.
[0028] This invention provides a method for determining the rhodium content in high-impurity materials, comprising: Weigh the sample of high-impurity material into a crucible, add the molten ingredients, and obtain the crucible with the prepared ingredients; The prepared crucible is melted and then subjected to a first cooling treatment to obtain nickel matte. The nickel matte was immersed in a sodium chloride aqueous solution and soaked at a constant temperature to obtain loose nickel matte; the mass fraction of sodium chloride in the sodium chloride aqueous solution was 1%~3%, and the constant temperature soaking temperature was 80℃~100℃; Loose nickel matte was immersed in hydrochloric acid solution for leaching, and then subjected to a second cooling treatment to obtain rhodium-enriched residue. The rhodium enrichment residue was digested by heating with aqua regia, and after a third cooling treatment, the rhodium content in the high-impurity material sample was determined by ICP-MS.
[0029] The method of this invention first mixes the sample of the high-impurity material to be tested with basic nickel carbonate, sublimed sulfur, sodium carbonate, borax, ferrous sulfide, and silicon dioxide, and melts it at high temperature in a refractory crucible to obtain nickel matte. Due to the high impurity content, metallized hard nickel sulfide will form. This nickel sulfide cannot be hydrolyzed normally. Therefore, the nickel matte is completely immersed in a 1% to 3% sodium chloride aqueous solution and soaked at a constant temperature of 80°C to 100°C for 2 to 4 hours. The hard nickel matte cracks and loosens from the inside out due to the synergistic effect of chloride ion film breaking, grain boundary micro-cell pitting corrosion, and nickel sulfide hydration expansion. The dispersed nickel matte is then leached with hydrochloric acid to remove the base metal matrix such as nickel, copper, and iron. The residue is filtered to obtain rhodium-enriched residue. Finally, the residue is digested with aqua regia, cooled and brought to a constant volume, and the rhodium content in the sample is determined by ICP-MS.
[0030] As a further improvement of the present invention, the impurities in the high-impurity material sample include at least one of sulfur, copper, iron, and organic matter; and / or, The mass of the high-impurity material sample is 5.00g~10.00g.
[0031] In this embodiment, the object of the method of the present invention is a high-impurity material, whose impurities include at least one of sulfur, copper, iron and organic matter. The mass of the sample to be measured is between 5.00g and 10.00g, which is convenient for detection.
[0032] As a further improvement of the present invention, the addition of molten materials includes: adding basic nickel carbonate, sublimed sulfur, sodium carbonate, borax, ferrous sulfide, and silicon dioxide, mixing thoroughly, and then covering the surface with a covering agent; wherein the mass of basic nickel carbonate is 10g~20g; and / or, The mass of sublimed sulfur is 1g to 2g; and / or, The mass of sodium carbonate is 30g~40g; and / or, The mass of borax is 10g~15g; and / or, The mass of ferrous sulfide is 0 g to 12 g; and / or, The mass of silicon dioxide is 0g~10g; and / or, The covering agent contains sodium carbonate and borax, with a sodium carbonate to borax mass ratio of 1.8-2.2:1; and / or, The thickness of the covering agent is 8mm~12mm.
[0033] In this embodiment, molten ingredients are added to the sample, stirred evenly, and then covered with a layer of covering agent. The covering agent is a mixture of sodium carbonate and borax. By controlling the content of each substance in the molten ingredients and the thickness of the covering agent, the melting effect is better, which facilitates subsequent operations.
[0034] As a further improvement of the present invention, the melting process includes: placing the prepared refractory clay crucible in a fire assay furnace and heating it to a constant temperature for melting. The initial temperature of the fire assay furnace is 940℃~960℃; and / or, The heating rate is 5℃ / min to 10℃ / min; and / or, The constant temperature is 1050℃~1100℃; and / or, The melting time is 20-30 minutes.
[0035] In this embodiment, the heating rate is controlled between 5°C / min and 10°C / min during the melting process to slow down the release of carbonate decomposition gases, prevent the melt from overflowing, and reduce the thermal shock of the crucible; the melting temperature is controlled between 1050°C and 1100°C and held for 20 min to 30 min to ensure thorough melting and complete enrichment of rhodium in the nickel matte phase.
[0036] As a further improvement of the present invention, the first cooling process includes: after melting, pouring into a cast iron mold, cooling, and separating.
[0037] In this embodiment, after melting is completed, a first cooling process is performed to separate the nickel matte.
[0038] As a further improvement of the present invention, the constant temperature soaking time is 2h~4h.
[0039] In this embodiment, controlling the soaking time at a constant temperature is to better facilitate the breaking of the buckle.
[0040] As a further improvement of the present invention, the concentration of the hydrochloric acid solution is 11.5 mol / L to 12.5 mol / L; and / or, The immersion temperature is 145℃~155℃; and / or, The temperature for heat digestion is 110℃~130℃; and / or, The heating and digestion time is 2 to 4 hours.
[0041] In this embodiment, the concentration of hydrochloric acid solution is controlled between 11.5 mol / L and 12.5 mol / L, and the leaching temperature is 145℃ to 155℃ to fully remove base metal impurities such as nickel, copper, and iron; the heating digestion temperature is 110℃ to 130℃, and the time is between 2h and 4h to ensure that the rhodium enrichment residue is completely dissolved.
[0042] As a further improvement of the present invention, the second cooling process includes: after leaching, cooling and filtering to remove the filtrate to obtain rhodium-enriched residue; the third cooling process includes: after heating and digestion, cooling to room temperature and making up to volume with ultrapure water.
[0043] In this embodiment, after leaching, the solution is cooled and filtered to remove residual hydrochloric acid solution; after heating and digestion, the solution is cooled to room temperature and diluted with ultrapure water to facilitate subsequent ICP-MS determination.
[0044] As a further improvement of the present invention, the ICP-MS determination includes: after heating and digestion, transferring the solution to a volumetric flask and making up to volume to obtain a test solution; taking a rhodium standard solution and determining and plotting a standard curve; adding an indium internal standard solution to the blank solution, standard solution and test solution, determining the rhodium element intensity in the test solution and blank solution, and determining the mass concentration of rhodium on the standard curve.
[0045] In this embodiment, after heating and digestion, the solution was cooled and transferred to a 100mL volumetric flask, diluted to the mark with water, and shaken well to obtain the test solution. The standard curve was plotted by transferring 0mL, 0.50mL, 1.00mL, 5.00mL, 10.00mL, and 20.00mL of rhodium standard solution to 100mL volumetric flasks, adding 5mL of aqua regia, diluting to the mark with water, and shaking well. The rhodium content in these standard curve solutions was 0.00ng / mL, 5.00ng / mL, 10.00ng / mL, 50.00ng / mL, 100.00ng / mL, and 200.00ng, respectively. / mL, and a standard curve was obtained after the determination. The process of determining the mass concentration of rhodium was as follows: on the inductively coupled plasma mass spectrometer, the instrument parameters were adjusted using the instrument tuning solution so that the sensitivity, oxide interference, double charge interference, resolution and other indices met the determination requirements. Indium internal standard solution was directly added to the blank solution, standard solution and test solution. A standard curve was established using the blank solution and standard solution, with the relative intensity of rhodium as the ordinate and the mass concentration of rhodium as the abscissa. The linear correlation coefficient of the standard curve was r≥0.999. The intensity of rhodium in the test solution and blank solution was measured, and the mass concentration of rhodium was determined from the standard curve.
[0046] It is worth mentioning that when the content of platinum group elements in the test solution is greater than 2000 ng / g, 5 mL of the solution is pipetted into a 50 mL or 100 mL volumetric flask, and 2.5 mL or 5 mL of aqua regia is added respectively. The solution is then diluted to the mark with water, shaken well, and used as a new test solution.
[0047] As a further improvement of the present invention, the formula for calculating the rhodium content in a high-impurity material sample is as follows: in, w i This refers to the rhodium content; r 1 The mass concentration of rhodium in the test solution is determined from the standard solution. r 2 The mass concentration of rhodium in the blank solution is determined by comparing it with the standard solution. V 1 This represents the volume of the solution after heating and digestion. V 2 This refers to the total volume of the test solution; V 3 m1 represents the volume of the test solution after dilution; m2 represents the mass of the sample containing high levels of impurities.
[0048] In this embodiment, the rhodium content in the high-impurity material sample is calculated using data obtained by ICP-MS determination. The calculation method is simple and the results are highly accurate.
[0049] The following are some specific embodiments. It should be noted that the embodiments described below are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention. Where specific techniques or conditions are not specified in the embodiments, they shall be performed in accordance with the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all conventional products that can be obtained commercially.
[0050] I. Preparation Method Example 1 This embodiment provides a method for determining the rhodium content in high-impurity materials, including the following steps: Accurately weigh 10.00g of high-impurity material sample, add 10g of basic nickel carbonate, 1.5g of sublimed sulfur, 30g of sodium carbonate, 10g of borax, 7g of ferrous sulfide and 5g of silicon dioxide into a refractory clay crucible, mix thoroughly and evenly, and cover with a 10mm layer of covering agent to obtain a refractory clay crucible with complete ingredients. The prepared refractory clay crucible was placed in a fire assay furnace with an initial temperature of 950°C and heated to 1100°C at a rate of 5°C / min. After the temperature stabilized, it was held for 20 minutes until the high impurity material was fully melted and the rhodium element was completely enriched in the nickel matte phase. After melting, the refractory clay crucible was quickly removed, poured into a cast iron mold, cooled and separated to obtain the nickel matte. The nickel matte was completely immersed in a 2% sodium chloride aqueous solution and soaked in a constant temperature water bath at 90°C for 3 hours to completely crack and loosen the hard nickel matte. Add concentrated hydrochloric acid to the loose nickel matte, place it on a hot plate and heat it at 150°C to leach. Heat until no more bubbles are produced to fully remove the base metal matrix such as nickel, copper, and iron. After leaching, cool and filter, remove the filtrate, and obtain rhodium-enriched residue. The rhodium enrichment residue was digested with 10 mL of aqua regia at 120 °C for 3 h. After digestion, it was cooled to room temperature and diluted to 100 mL with ultrapure water. The signal intensity of rhodium in the test solution was measured using ICP-MS with optimized instrument parameters. The rhodium content in the high-impurity material sample was calculated by combining the standard curve.
[0051] Example 2 The only difference between this embodiment and Example 1 is that the concentration of the sodium chloride aqueous solution is changed to 1%. The remaining steps and parameters are roughly the same as in Example 1, and will not be repeated here.
[0052] Example 3 The only difference between this embodiment and Example 1 is that the concentration of the sodium chloride aqueous solution is changed to 3%. The remaining steps and parameters are roughly the same as in Example 1, and will not be repeated here.
[0053] Example 4 The only difference between this embodiment and Embodiment 1 is that the constant temperature soaking temperature is changed to 80°C. The remaining steps and parameters are roughly the same as in Embodiment 1, and will not be repeated here.
[0054] Example 5 The only difference between this embodiment and Embodiment 1 is that the constant temperature soaking temperature is changed to 100°C. The remaining steps and parameters are roughly the same as in Embodiment 1, and will not be repeated here.
[0055] Example 6 The only difference between this embodiment and Embodiment 1 is that the high-impurity material used comes from other production workshops, the raw materials are different, and the impurity content is also different. The remaining steps and parameters are roughly the same as in Embodiment 1, and will not be repeated here.
[0056] Example 7 The only difference between this embodiment and Example 1 is that the rhodium content in the high-impurity material sample used is 1099.2 ng / g. The remaining steps and parameters are roughly the same as in Example 1, and will not be repeated here.
[0057] Example 8 The only difference between this embodiment and Embodiment 1 is that the high-impurity material sample used is replaced with a standard substance (GBW07291). The remaining steps and parameters are roughly the same as in Embodiment 1, and will not be repeated here.
[0058] Example 9 The only difference between this embodiment and Embodiment 1 is that the high-impurity material sample used is replaced with a standard substance (GBW07293). The remaining steps and parameters are roughly the same as in Embodiment 1, and will not be repeated here.
[0059] Example 10 The only difference between this embodiment and Example 1 is that the high-impurity material sample used is replaced with a standard substance (GBW07294). The remaining steps and parameters are roughly the same as in Example 1, and will not be repeated here.
[0060] Comparative Example 1 The only difference between this comparative example and Example 1 is that the high-impurity material sample used is replaced with a standard substance (GBW07291), and the method of breaking the loose nickel matte is the conventional mechanical breaking method. The remaining steps and parameters are roughly the same as in Example 1, and will not be repeated here.
[0061] Comparative Example 2 The only difference between this comparative example and Example 1 is that the high-impurity material sample used is replaced with a standard substance (GBW07293), and the method of breaking the loose nickel matte is the conventional mechanical breaking method. The remaining steps and parameters are roughly the same as in Example 1, and will not be repeated here.
[0062] Comparative Example 3 The only difference between this comparative example and Example 1 is that the high-impurity material sample used is replaced with a standard substance (GBW07294), and the method of breaking the loose nickel matte is the conventional mechanical breaking method. The remaining steps and parameters are roughly the same as in Example 1, and will not be repeated here.
[0063] Comparative Example 4 The only difference between this comparative example and Example 1 is that the concentration of the sodium chloride aqueous solution is changed to 0.5%. The remaining steps and parameters are roughly the same as in Example 1, and will not be repeated here.
[0064] Comparative Example 5 The only difference between this comparative example and Example 1 is that the concentration of the sodium chloride aqueous solution is changed to 4%. The remaining steps and parameters are roughly the same as in Example 1, and will not be repeated here.
[0065] Comparative Example 6 The only difference between this comparative example and Example 1 is that the constant temperature soaking temperature is changed to 70°C. The remaining steps and parameters are roughly the same as in Example 1, and will not be repeated here.
[0066] II. Testing Methods Calculate the rhodium content using the following formula, and calculate the relative standard deviation after multiple measurements; III. Results Analysis Table 1. Impurity content in Examples 1 and 6 Table 2, Rhodium content of Examples 1-10 Table 3. Relative standard deviations of Examples 1-10 As shown in Tables 2 and 3, the concentrations of the sodium chloride aqueous solution used in Examples 1-3 were different, but all were within feasible ranges. The appropriate concentration of sodium chloride was just right to break down the nickel matte, resulting in good stability of the measured rhodium content and its relative standard deviation. Examples 4 and 5 involved changing the temperature of the constant-temperature soaking, both of which were within feasible ranges, resulting in good matte-breaking effect and good stability of the results. The high-impurity material used in Example 6 came from another production workshop, and the measured results showed good stability. The rhodium grade in the high-impurity material sample used in Example 7 was 109%. The rhodium content obtained by the test was 9.2 ng / g, and the relative standard deviation of the repeated tests was small, indicating that the method of the present invention has high accuracy and precision. The samples used in Examples 8-10 were three standard test samples, and the rhodium content in the three standard samples were (4.3±0.8) ng / g, (22±3) ng / g, and (1.1±0.2) ng / g, respectively. The data obtained by the three tests all met the content range of the standard samples, and the relative standard deviation was small, further indicating that the method of the present invention has high accuracy and precision.
[0067] Table 4. Rhodium content of Comparative Examples 1-6 Table 5. Relative standard deviations of comparative examples 1-6 As shown in Tables 4 and 5, the average values of the nickel matte buckles obtained from the tests on the three standard samples in Comparative Examples 1-3, using conventional mechanical crushing methods, differed significantly from the standard values of the samples and also from the values obtained in the examples. The relative standard deviations calculated from the parallel tests were also large. This is because conventional mechanical crushing easily leads to cross-contamination of the samples, loss of fine rhodium particles, and incomplete crushing. The nickel matte buckle core remains dense, resulting in incomplete dissolution of the matrix during hydrochloric acid leaching. The rhodium is encapsulated and sealed within the dense matrix, ultimately leading to significantly lower test results. The parallel samples showed poor precision and accuracy. Comparative Example 4 used a sodium chloride aqueous solution with a concentration of 0.5%. Due to the low sodium chloride concentration, it failed to break down the sample and could not be measured. Comparative Example 5 used a sodium chloride aqueous solution with a concentration of 4%. Although the sodium chloride concentration was high enough to break down the sample, the excessive sodium chloride affected the measurement results, resulting in lower values. Comparative Example 6 used a constant temperature soaking temperature of 70℃. The constant temperature soaking temperature was too low, resulting in poor breaking down of the sample. The broken sample contained fine particles, which affected the subsequent dissolution of the sample and led to lower measurement results.
[0068] Therefore, the method for determining the rhodium content in high-impurity materials of the present invention uses a low-concentration sodium chloride system, which plays a role in activating and breaking the film and inducing grain boundary corrosion. It leaves no large amount of salt residue, does not change the occurrence state of rhodium, and is fully compatible with subsequent hydrochloric acid leaching, aqua regia digestion, and ICP-MS precise determination process. It completely solves the problem of rhodium determination failure and data distortion caused by the failure of nickel buckle water in high-impurity materials, and ensures the accuracy and stability of trace rhodium content determination in high-impurity materials.
[0069] It should be noted that this application is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same structure and effect as the technical concept within the scope of this application are included in the technical scope of this application. Various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing embodiments by combining some of the constituent elements, are also included in the scope of this application without departing from the spirit of this application.
[0070] Furthermore, although this application has been described with reference to preferred embodiments, various modifications can be made thereto and components can be replaced with equivalents without departing from the scope of this application. In particular, the technical features mentioned in the various embodiments can be combined in any manner, provided there is no structural conflict. This application is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.
Claims
1. A method for determining the rhodium content in high-impurity materials, characterized in that, include: Weigh the sample of high-impurity material into a crucible, add the molten ingredients, and obtain the crucible with the prepared ingredients; The crucible containing the prepared ingredients is melted and subjected to a first cooling treatment to obtain nickel matte. The nickel matte was immersed in a sodium chloride aqueous solution and soaked at a constant temperature to obtain loose nickel matte; the mass fraction of sodium chloride in the sodium chloride aqueous solution was 1%~3%, and the constant temperature soaking temperature was 80℃~100℃; The loose nickel matte was immersed in hydrochloric acid solution for leaching, and then subjected to a second cooling treatment to obtain rhodium-enriched residue. The rhodium-enriched residue was heated and digested with aqua regia, and after a third cooling treatment, the rhodium content in the high-impurity material sample was determined by ICP-MS.
2. The method for determining the rhodium content in a high-impurity material according to claim 1, characterized in that, The impurities in the high-impurity material sample include at least one of sulfur, copper, iron, and organic matter; and / or, The mass of the high-impurity material sample is 5.00g~10.00g.
3. The method for determining the rhodium content in a high-impurity material according to claim 1, characterized in that, The addition of molten materials includes: adding basic nickel carbonate, sublimed sulfur, sodium carbonate, borax, ferrous sulfide, and silicon dioxide, mixing thoroughly, and then covering the surface with a covering agent; wherein the mass of the basic nickel carbonate is 10g~20g; and / or, The sublimed sulfur has a mass of 1g to 2g; and / or, The sodium carbonate is 30g to 40g in mass; and / or, The borax has a mass of 10g~15g; and / or, The ferrous sulfide has a mass of 0 g to 12 g; and / or, The mass of the silicon dioxide is 0g~10g; and / or, The covering agent contains sodium carbonate and borax, wherein the mass ratio of sodium carbonate to borax is 1.8-2.2:1; and / or, The thickness of the covering agent is 8mm to 12mm.
4. The method for determining the rhodium content in a high-impurity material according to claim 1, characterized in that, The melting process includes: placing the prepared refractory clay crucible in a fire test furnace and heating it to a constant temperature for melting; Wherein, the initial temperature of the fire assay furnace is 940℃~960℃; and / or, The heating rate is 5°C / min to 10°C / min; and / or, The constant temperature is 1050℃~1100℃; and / or, The melting time is 20 min to 30 min.
5. The method for determining the rhodium content in a high-impurity material according to claim 1, characterized in that, The first cooling process includes: after the melting is completed, pouring the mixture into a cast iron mold, cooling, and separating it.
6. The method for determining the rhodium content in a high-impurity material according to claim 1, characterized in that, The constant temperature soaking time is 2h~4h.
7. The method for determining the rhodium content in a high-impurity material according to claim 1, characterized in that, The concentration of the hydrochloric acid solution is 11.5 mol / L to 12.5 mol / L; and / or, The immersion temperature is 145℃~155℃; and / or, The heating and digestion temperature is 110℃~130℃; and / or, The heating and digestion time is 2h to 4h.
8. The method for determining the rhodium content in a high-impurity material according to claim 1, characterized in that, The second cooling process includes: after the leaching is completed, cooling and filtering are performed to remove the filtrate and obtain the rhodium-enriched residue; the third cooling process includes: after the heating digestion is completed, cooling to room temperature and making up to a final volume with ultrapure water.
9. The method for determining the rhodium content in a high-impurity material according to claim 1, characterized in that, The ICP-MS determination includes: after heating and digestion, transferring the solution to a volumetric flask and making up to volume to obtain a test solution; taking a rhodium standard solution and determining it to plot a standard curve; adding an indium internal standard solution to the blank solution, standard solution, and test solution, determining the rhodium element intensity in the test solution and blank solution, and determining the mass concentration of rhodium on the standard curve.
10. The method for determining the rhodium content in a high-impurity material according to claim 9, characterized in that, The formula for calculating the rhodium content in the high-impurity material sample is as follows: Among them, the w i The content of rhodium; the ρ 1 The mass concentration of rhodium in the test solution was determined from the standard solution; ρ 2 The mass concentration of rhodium in the blank solution was determined by comparing it with the standard solution; V 1 The volume of the solution after heating and digestion; V 2 The total volume of the test solution; V 3 The volume of the test solution after dilution is given; m1 is the mass of the sample containing high levels of impurities.