A zif-67 / mxene composite based on schottky junction and a preparation method and application thereof

By forming Schottky junctions by in-situ growth of ZIF-67 crystals on two-dimensional MXene materials, the problems of poor conductivity and easy aggregation of ZIF-67 materials are solved, achieving efficient photothermal and chemical dynamic synergistic antibacterial and wound healing effects, which has broad prospects for biomedical applications.

CN123078639APending Publication Date: 2026-11-13YANGTZE UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611237138.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-14
Publication Date
2026-11-13

AI Technical Summary

Technical Problem

Existing ZIF-67 materials suffer from poor conductivity, easy aggregation, and masking of active sites, which limits their application in the biomedical field.

Method used

By employing an electrostatic self-assembly and in-situ growth strategy, ZIF-67 crystals were uniformly grown in situ on the surface of a two-dimensional MXene material to form a Schottky junction heterostructure, thereby reducing the interfacial electron transfer resistance. Furthermore, the aggregation of ZIF-67 crystals was restricted by MXene, exposing more catalytic active sites.

Benefits of technology

The conductivity and catalytic efficiency of the ZIF-67/MXene composite material were significantly improved, realizing the functions of photothermal and chemodynamic synergistic antibacterial and wound healing promotion, and demonstrating good biocompatibility and clinical application potential.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123078639A_ABST
    Figure CN123078639A_ABST
Patent Text Reader

Abstract

This invention discloses a ZIF-67 / MXene composite material based on a Schottky junction, its preparation method, and its applications, belonging to the field of biomedical materials technology. This invention utilizes the abundant endogenous functional groups on the two-dimensional MXene surface as "anchoring sites" for metal ions, inducing the in-situ uniform nucleation and growth of ZIF-67 crystals between MXene layers and on the surface, forming a Schottky junction heterostructure with a clean interface. This effectively reduces the Schottky barrier, significantly lowers the interfacial electron transfer resistance, and substantially improves the conductivity of the ZIF-67 / MXene composite material. Simultaneously, this composite material possesses more catalytically active sites, significantly enhancing reaction efficiency. Furthermore, this ZIF-67 / MXene composite material exhibits photothermal and chemokinetic synergistic antibacterial properties and promotes wound healing, thus showing promising application prospects in the field of biomedical materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of biomedical materials technology, specifically relating to a ZIF-67 / MXene composite material based on a Schottky junction, its preparation method, and its application. Background Technology

[0002] Bacterial infections of skin wounds, especially those caused by multidrug-resistant bacteria such as methicillin-resistant Staphylococcus aureus (MRSA), pose a significant challenge in clinical treatment. While traditional antibiotic therapy is widespread, long-term use leads to increased bacterial resistance and makes it difficult to disrupt bacterial biofilms, resulting in delayed wound healing and even serious complications such as sepsis. Therefore, developing novel non-invasive treatment strategies that do not rely on antibiotics, such as photothermal therapy (PTT), photodynamic therapy (PDT), and chemokinetic therapy (CDT), has become a current research focus.

[0003] Metal-organic frameworks (MOFs), especially ZIF-67, are widely used as precursors for constructing multifunctional materials due to their tunable microporous structure, high porosity, and large specific surface area. ZIF-67 is rich in nitrogen as an active center, and its cobalt (Co) content can serve as a catalytic center for chemokinetic therapy, generating hydroxyl radicals (·OH) to kill bacteria through a Fenton-like reaction. However, directly applying ZIF-67 to the biomedical field still faces the following major technical drawbacks: 1) Poor conductivity: Most MOFs (including ZIF-67) are essentially semiconductors or insulators with poor electronic conductivity. In catalytic reactions requiring electron transfer (such as the Fenton reaction producing ROS), the high electron transport impedance limits their catalytic rate and therapeutic efficiency. 2) Prone aggregation and masking of active sites: Nanoscale MOF particles have high surface energy in physiological environments, making them highly prone to aggregation. This leads to a reduction in effective specific surface area and masking of catalytic active sites, significantly reducing their bactericidal effect.

[0004] In view of this, there is an urgent need to develop a ZIF-67 / MXene composite material with tight interfacial bonding, smooth electron transport, and the ability to achieve a "balance between efficient sterilization and healing promotion" through specific concentration control, so as to solve the shortcomings of the existing technology. Summary of the Invention

[0005] The purpose of this invention is to provide a ZIF-67 / MXene composite material based on a Schottky junction, its preparation method, and its applications. This addresses the problems of poor conductivity, easy aggregation, and masking of active sites in existing ZIF-67 materials.

[0006] In a first aspect, the present invention provides a method for preparing a ZIF-67 / MXene composite material based on a Schottky junction, comprising the following steps: mixing Ti3AlC2 powder, lithium fluoride, and an acid solution and reacting the mixture; subjecting the resulting product to ultrasonic treatment; and then washing, centrifuging, and freeze-drying to obtain Ti3C2T x Powder; Ti3C2T x The powder was dispersed in an organic solvent, then cobalt salt was added, and after ultrasonic treatment, a first solution was obtained; 2-methylimidazole was dissolved in an organic solvent to obtain a second solution; the first solution was added to the second solution and allowed to stand for reaction. After the reaction was completed, the ZIF-67 / MXene composite material was obtained by filtration, washing, and freeze-drying.

[0007] In this invention, the inventors discovered that, based on an electrostatic self-assembly and in-situ growth strategy, a two-dimensional MXene (Ti3C2T) can be grown... x The abundant endogenous functional groups (-F, -OH, -O, etc.) on the surface of the material serve as "anchoring sites" for metal ions, inducing the in-situ uniform nucleation and growth of ZIF-67 crystals in the interlayer and on the surface of MXene. This results in the formation of a Schottky junction heterostructure with a clean interface, effectively reducing the Schottky barrier, significantly lowering the interfacial electron transfer resistance, and substantially improving the conductivity of the ZIF-67 / MXene composite material. Simultaneously, MXene, acting as a "two-dimensional planar support," restricts the excessive growth and aggregation of ZIF-67 crystals, reducing the size of ZIF-67 particles and ensuring their uniform distribution, thereby exposing more catalytically active sites and significantly improving reaction efficiency. Furthermore, this ZIF-67 / MXene composite material exhibits photothermal and chemodynamic synergistic antibacterial properties and promotes wound healing.

[0008] In some embodiments, in the step of reacting Ti3AlC2 powder, lithium fluoride and acid solution, the mass ratio of Ti3AlC2 powder to lithium fluoride is 1:(1-2), and the mass-volume ratio of Ti3AlC2 powder to acid solution is 1g:(15-25mL).

[0009] In some embodiments, in the step of reacting Ti3AlC2 powder, lithium fluoride and acid solution, the concentration of the acid solution is 7-12M and the acid solution includes hydrochloric acid; the reaction specifically includes: reacting at room temperature for 10-15 hours.

[0010] In some embodiments, after mixing Ti3AlC2 powder, lithium fluoride and acid solution and reacting, the resulting product is ultrasonically treated, and then washed, centrifuged and freeze-dried. The ultrasonic treatment time is 6-12 hours. The washing specifically includes washing until the pH of the supernatant is 5-6.

[0011] In some embodiments, during the step of obtaining the first solution, Ti3C2T in the first solution x The concentration of the powder is 2-3 mg / mL, and the concentration of the cobalt salt is 0.01-0.04 mmol / mL.

[0012] In some embodiments, in the step of obtaining the first solution, the organic solvent includes methanol; the cobalt salt includes cobalt nitrate hexahydrate; and the ultrasonic treatment time is 5-15 min.

[0013] In some embodiments, in the step of obtaining the second solution, the concentration of 2-methylimidazole in the second solution is 0.1-0.3 mmol / mL; the organic solvent includes methanol.

[0014] In some embodiments, in the step of adding the first solution to the second solution and then allowing the reaction to stand, the volume ratio of the first solution to the second solution is (0.5-1.5):(0.5-1.5); and the standing reaction time is 20-30 hours.

[0015] In a second aspect, the present invention provides a ZIF-67 / MXene composite material based on a Schottky junction, which is prepared by any of the above preparation methods.

[0016] In a third aspect, the present invention provides the application of the ZIF-67 / MXene composite material based on the Schottky junction as described above in at least one of the following: A1) preparing a drug with photothermal and chemodynamic synergistic antibacterial properties; A2) preparing a drug that promotes wound healing.

[0017] The beneficial effects of this invention are: unlike the prior art, this invention is based on an electrostatic self-assembly and in-situ growth strategy, utilizing two-dimensional MXene (Ti3C2T) x The abundant endogenous functional groups (-F, -OH, -O, etc.) on the surface of the ZIF-67 / MXene composite material serve as "anchoring sites" for metal ions, inducing the uniform in-situ nucleation and growth of ZIF-67 crystals within the MXene interlayer and on the surface. This results in a Schottky junction heterostructure with a clean interface, effectively reducing the Schottky barrier, significantly lowering the interfacial electron transfer resistance, and substantially improving the conductivity of the ZIF-67 / MXene composite. Simultaneously, MXene, acting as a "two-dimensional planar support," restricts the excessive growth and aggregation of ZIF-67 crystals, reducing the particle size and ensuring uniform distribution of ZIF-67 particles. This exposes more catalytically active sites, significantly enhancing reaction efficiency. Furthermore, this ZIF-67 / MXene composite exhibits photothermal and chemodynamic synergistic antibacterial properties and promotes wound healing, thus demonstrating promising applications in the field of biomedical materials. Attached Figure Description

[0018] Figure 1The ZIF-67 / MXene composite material and Ti3C2T in this invention x SEM results of powder materials and ZIF-67 materials, where (a) is Ti3C2T x SEM images of powder materials, (b) is an enlarged view of the area within the dashed box in (a), (c) is an SEM image of ZIF-67 material, (d) is an enlarged view of the area within the dashed box in (c), (e) is an SEM image of ZIF-67 / MXene composite material, and (f) is an enlarged view of the area within the dashed box in (e). Figure 2 The images show the TEM and elemental distribution results of the ZIF-67 / MXene composite material and the ZIF-67 material in this invention. Among them, (a) is the TEM image of the ZIF-67 material, (c) is the HAAD-STEM image of the ZIF-67 material, (df) are the TEM elemental mapping images of Co, O, and N of the ZIF-67 material, (b) is the TEM image of the ZIF-67 / MXene composite material, (g) is the HAAD-STEM image of the ZIF-67 / MXene composite material, and (hl) are the TEM elemental mapping images of Co, O, N, C, and Ti of the ZIF-67 / MXene composite material. Figure 3 The ZIF-67 / MXene composite material and Ti3C2T in this invention x XRD patterns of powder materials and ZIF-67 materials; Figure 4 The ZIF-67 / MXene composite material and Ti3C2T in this invention x XPS results for powder materials and ZIF-67 materials, where (a) shows the ZIF-67 / MXene composite material and Ti3C2T. x Full scan XPS spectra of powder material and ZIF-67 material, (bf) are XPS spectra after peak fitting of C1s, Ti 2p, O 1s, Co 2p and N1 2p, respectively; Figure 5 The results of the cytotoxicity test of the ZIF-67 / MXene composite material in Example 2 of this invention; Figure 6 The scratch test results are for the ZIF-67 / MXene composite material in Example 2 of this invention; Figure 7 The results of antibacterial activity of Staphylococcus aureus ATCC43300 in vitro under different treatment groups in Example 3 of the present invention are shown. (a) shows the results of fluorescence liveness and deadness staining of the strain after treatment with different treatment groups, and (b) shows the results of scanning electron microscopy observation of the strain after treatment with different treatment groups. Figure 8The in vivo evaluation results of the synergistic antibacterial and wound healing effects in Example 4 of this invention include: (a) a schematic diagram of establishing an infected skin defect model and subsequent treatment; (b) schematic diagrams of wound closure on days 0, 3, and 7 in different treatment groups; (c) representative digital photographs of infected wounds on days 7 in different treatment groups; (d) results of weight changes in mice during treatment in different treatment groups; (e) results of wound healing rates on day 7 in different treatment groups; and (f) results of 808nm laser (0.84W / cm²) treatment in different treatment groups. 2 Real-time infrared thermographs of mice irradiated for 10 minutes. Data are expressed as mean ± SD (n=3, p <0.05); Figure 9 The above are the immunofluorescence analysis results of angiogenesis, cell proliferation, and tissue remodeling in mouse wound tissue on day 7 in Example 4 of this invention. (ac) represents representative immunofluorescence images of CD31 (angiogenesis marker), Ki67 (proliferation marker), and TGF-β (tissue remodeling factor), respectively. Target protein staining is red (CY3), and reverse staining of cell nuclei is blue (DAPI). Scale bar: 100 μm. (df) represents the quantitative analysis results of the average fluorescence intensity or percentage of positive cells for CD31, Ki67, and TGF-β. Data are expressed as mean ± SD (n=3, ...). p <0.05); Figure 10 This is a representative H&E staining image of the major organs (heart, liver, spleen, lung and kidney) of mice in the control group and MXM / H2O2+NIR group on day 7 in Example 4 of this invention. Detailed Implementation

[0019] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0020] Experimental methods not specified in the examples are generally performed under conventional conditions and as described in the manual, or as recommended by the manufacturer. Unless otherwise specified, the general equipment, materials, reagents, etc. used are commercially available.

[0021] Currently, existing ZIF-67 materials suffer from problems such as poor conductivity, easy aggregation, and masking of active sites.

[0022] To address the problems of poor conductivity, easy aggregation, and masking of active sites in existing ZIF-67 materials, this invention provides a ZIF-67 / MXene composite material based on a Schottky junction, its preparation method, and its application.

[0023] In a first aspect, the present invention provides a method for preparing a ZIF-67 / MXene composite material based on a Schottky junction, comprising the following steps: mixing Ti3AlC2 powder, lithium fluoride, and an acid solution and reacting the mixture; subjecting the resulting product to ultrasonic treatment; and then washing, centrifuging, and freeze-drying to obtain Ti3C2T x Powder; Ti3C2T x The powder was dispersed in an organic solvent, then cobalt salt was added, and after ultrasonic treatment, a first solution was obtained; 2-methylimidazole was dissolved in an organic solvent to obtain a second solution; the first solution was added to the second solution and allowed to stand for reaction. After the reaction was completed, the ZIF-67 / MXene composite material was obtained by filtration, washing, and freeze-drying.

[0024] In the preparation method of ZIF-67 / MXene composite material provided by this invention, ZIF-67 (semiconductor) is directly grown on Ti3C2T through fine design of the micro-interface. x Significant electron transfer (negative shift of Co 2p binding energy) occurs between the surface of the material (metal-like conductor) and the MXene nanosheets, forming a built-in electric field. This direct contact effectively reduces the Schottky barrier and greatly reduces the interfacial electron transfer resistance, thus endowing the material with excellent overall conductivity. Simultaneously, ZIF-67 is tightly anchored to the MXene nanosheets through Ti-O chemical bonds. This chemical bonding ensures that the material does not disintegrate or detach in complex physiological environments. Furthermore, the MXene nanosheets, acting as a "two-dimensional planar support," limit the excessive growth and aggregation of ZIF-67 crystals. The size of the composite ZIF-67 particles is significantly reduced from the pure sample's 700-1000 nm to a smaller size with uniform distribution. This size effect exposes more catalytically active sites, significantly improving reaction efficiency. In addition, this ZIF-67 / MXene composite material exhibits photothermal, chemodynamic, and synergistic antibacterial functions as well as wound healing promotion.

[0025] In some embodiments, in the step of reacting Ti3AlC2 powder, lithium fluoride and acid solution, the mass ratio of Ti3AlC2 powder to lithium fluoride is 1:(1-2), and the mass-volume ratio of Ti3AlC2 powder to acid solution is 1g:(15-25mL).

[0026] In this invention, by controlling the amounts of Ti3AlC2 powder, lithium fluoride, and acid solution within a specific range, the aluminum (Al) atomic layer in the MAX phase can be effectively etched and removed.

[0027] In some embodiments, in the step of reacting Ti3AlC2 powder, lithium fluoride and acid solution, the concentration of the acid solution is 7-12M and the acid solution includes hydrochloric acid; the reaction specifically includes: reacting at room temperature for 10-15 hours.

[0028] Understandably, the concentration and type of acid solution, as well as the reaction time, can be routinely adjusted according to actual usage needs, as long as a high-performance Ti3C2T can be obtained. x Powder is acceptable. For example, in this invention, the concentration of the acid solution is preferably 7-12M, and the acid solution preferably includes hydrochloric acid; the reaction specifically includes: at room temperature, the reaction preferably lasts for 10-15 hours.

[0029] In some embodiments, after mixing Ti3AlC2 powder, lithium fluoride and acid solution and reacting, the resulting product is ultrasonically treated, and then washed, centrifuged and freeze-dried. The ultrasonic treatment time is 6-12 hours. The washing specifically includes washing until the pH of the supernatant is 5-6.

[0030] In this invention, by controlling the ultrasonic treatment time and cleaning parameters within a specific range, a multilayer structure can be exfoliated into fewer nanosheets, thereby preparing accordion-shaped or sheet-like Ti3C2T. x powder.

[0031] In some embodiments, during the step of obtaining the first solution, Ti3C2T in the first solution x The concentration of the powder is 2-3 mg / mL, and the concentration of the cobalt salt is 0.01-0.04 mmol / mL.

[0032] In this invention, by controlling Ti3C2T x Within a specific range, the concentrations of powder and cobalt salt can enable Ti3C2T x Negatively charged functional groups (-F, -OH, -O, etc.) on the powder surface adsorb positively charged Co. 2+ Ions provide better nucleation sites for the growth of ZIF-67 crystals.

[0033] In some embodiments, in the step of obtaining the first solution, the organic solvent includes methanol; the cobalt salt includes cobalt nitrate hexahydrate; and the ultrasonic treatment time is 5-15 min.

[0034] It is understandable that the types of organic solvents, cobalt salts, and ultrasonic treatment time can be adjusted according to actual usage needs, as long as a ZIF-67 material with good performance can be obtained. For example, in the step of obtaining the first solution in this invention, the organic solvent preferably includes methanol; the cobalt salt preferably includes cobalt nitrate hexahydrate; and the ultrasonic treatment time is preferably 5-15 minutes.

[0035] In some embodiments, in the step of obtaining the second solution, the concentration of 2-methylimidazole in the second solution is 0.1-0.3 mmol / mL; the organic solvent includes methanol.

[0036] It is understood that the concentration of 2-methylimidazole and the type of organic solvent can be routinely adjusted according to actual usage needs, as long as a ZIF-67 material with good performance can be obtained. For example, in this invention, the concentration of 2-methylimidazole in the second solution is preferably 0.1-0.3 mmol / mL; the organic solvent preferably includes methanol.

[0037] In some embodiments, in the step of adding the first solution to the second solution and then allowing the reaction to stand, the volume ratio of the first solution to the second solution is (0.5-1.5):(0.5-1.5); and the standing reaction time is 20-30 hours.

[0038] In this invention, by controlling the volume ratio of the first solution and the second solution and the standing reaction time within a specific range, ZIF-67 can be uniformly grown on MXene material, thereby significantly improving the performance of ZIF-67 / MXene composite material.

[0039] In a second aspect, the present invention provides a ZIF-67 / MXene composite material based on a Schottky junction, which is prepared by any of the above preparation methods.

[0040] In some implementations, the specific surface area of ​​the ZIF-67 / MXene composite material is 470-480 m². 2 / g, pore volume 0.1-0.3cm 3 / g.

[0041] The ZIF-67 / MXene composite material provided by this invention has an extremely high specific surface area and abundant microporous structure, thus providing more open active sites and greatly improving the substrate contact efficiency of catalytic reactions.

[0042] In a third aspect, the present invention provides the application of the ZIF-67 / MXene composite material based on the Schottky junction as described above in at least one of the following: A1) preparing a drug with photothermal and chemodynamic synergistic antibacterial properties; A2) preparing a drug that promotes wound healing.

[0043] In the application provided by this invention, the ZIF-67 / MXene composite material has the functions of photothermal and chemokinetic synergistic antibacterial and wound healing promotion; wherein, the dual driving mechanism of "photothermal-chemokinetic" of the ZIF-67 / MXene composite material is as follows: 1) Photothermal therapy (PTT) mechanism: Utilizing the excellent photothermal conversion performance of MXene, the composite material can be rapidly heated to about 50°C under irradiation with 808nm near-infrared light (NIR). This local thermal effect can not only directly destroy the bacterial cell membrane structure (thermal ablation), but more importantly, it serves as an energy trigger source. 2) Mechanism of Heat-assisted Chemokinetic Therapy (CDT): Co ions released by ZIF-67 act as catalysts for Fenton-like reactions, converting H2O2 in the microenvironment into highly toxic hydroxyl radicals (·OH). The heat energy generated by photothermal activity (50℃) significantly accelerates the kinetic rate of the ZIF-67-mediated Fenton-like reaction. This thermodynamic drive enables explosive ROS generation even when the H2O2 concentration in the wound microenvironment is low, achieving a more thorough bactericidal effect than single CDT or single PTT, and without relying on oxygen (superior to photodynamic PDT).

[0044] Furthermore, after effectively clearing wound infection, the ZIF-67 / MXene composite material can actively regulate the regenerative microenvironment at a specific concentration (preferably 40 μg / mL). The specific mechanisms are as follows: 1) It significantly upregulates CD31 expression, promotes the formation of a dense microvascular network by vascular endothelial cells, improves blood supply to the affected area, and thus promotes angiogenesis; 2) It significantly increases the proportion of Ki67 positive cells, reverses cell cycle arrest caused by infection, promotes fibroblast proliferation and migration, and thus activates cell proliferation; 3) It upregulates TGF-β expression, promotes collagen synthesis and orderly deposition, makes the structure of new tissue closer to normal skin, effectively reduces scar formation, and thus optimizes tissue remodeling.

[0045] In addition, this ZIF-67 / MXene composite material exerts a strong bactericidal effect while having no toxic side effects on the body, and has extremely high potential for clinical translation.

[0046] The following are some specific embodiments. It should be noted that the embodiments described below are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention.

[0047] Example 1: Preparation of ZIF-67 / MXene composite material based on Schottky junction This embodiment provides a method for preparing ZIF-67 / MXene composite material.

[0048] Specifically, it includes the following steps: S1. 0.125 g Ti3AlC2 powder, 0.2 g lithium fluoride, and 2.5 mL 9 M hydrochloric acid were mixed and reacted with magnetic stirring at room temperature for 12 h. The resulting product was then sonicated for 10 h. Subsequently, the product was repeatedly washed by centrifugation with deionized water until the pH of the supernatant was 5.5. The precipitate was collected by differential centrifugation and freeze-dried to obtain accordion-shaped or lamellar Ti3C2T x powder.

[0049] S2. Take 100 mg of the Ti3C2T prepared in step S1. x The powder was dispersed in 40 mL of methanol and sonicated until completely dispersed; then 1 mmol of cobalt nitrate hexahydrate (Co(NO3)2·6H2O) was added and sonicated for another 10 min to obtain the first solution.

[0050] S3. Dissolve 8 mmol of 2-methylimidazole in 40 mL of methanol and stir for 20 minutes until completely dissolved to obtain the second solution.

[0051] S4. Under magnetic stirring, the first solution prepared in step S2 is added to the second solution prepared in step S3, and the mixture is stirred continuously for 30 min. Then, the mixture is allowed to stand for 24 h. After the reaction is completed, the precipitate is collected by filtration, washed with methanol to remove unreacted raw materials, and finally freeze-dried to obtain the ZIF-67 / MXene composite material.

[0052] Comparative Example 1 In this comparative example, a Ti3C2T is provided. x For the specific preparation of the powder material, please refer to step S1 of Example 1.

[0053] Comparative Example 2 In this comparative example, a ZIF-67 material is provided, the specific preparation of which is described in steps S2-S4 of Example 1, except that Ti3C2T is not added in step S2. x The powder is used to obtain ZIF-67 material in step S4.

[0054] Performance testing The ZIF-67 / MXene composite material prepared in Example 1 and the Ti3C2T composite material prepared in Comparative Example 1 were compared. x The powder material and the ZIF-67 material prepared in Comparative Example 2 were subjected to SEM testing, and the results are as follows: Figure 1 As shown.

[0055] from Figure 1 As can be seen from this, Ti3C2T x Powder materials ( Figure 1 (a and 1b) have a layered structure, and the ZIF-67 material ( Figure 1c) and 1d) exhibit a regular rhombic dodecahedral structure with a particle size of approximately 700-1000 nm; while the ZIF-67 nanoparticles in the composite material are uniformly distributed in Ti3C2T x The surface and interlayer structure are layered, and the ZIF-67 particle size is significantly reduced, with no obvious agglomeration. Figure 1 (e and 1f); This indicates that MXene, acting as a carrier and binder, effectively limited the excessive growth of ZIF-67 crystals and prevented interparticle aggregation.

[0056] Furthermore, the specific surface area and pore volume of the ZIF-67 / MXene composite material prepared in Example 1 were tested. The results showed that the specific surface area of ​​the ZIF-67 / MXene composite material was 474.661 m². 2 / g, pore volume is 0.159cm³ 3 / g.

[0057] Furthermore, TEM and elemental distribution tests were performed on the ZIF-67 / MXene composite material prepared in Example 1 and the ZIF-67 material prepared in Comparative Example 2. The results are as follows: Figure 2 As shown.

[0058] from Figure 2 As can be seen, ZIF-67 material exhibits a regular rhombic dodecahedral structure and contains Co, O, and N elements. Figure 2 a, 2c, 2d, 2e, 2f); while in the ZIF-67 / MXene composite material, elements such as Co, O, N, C, and Ti are uniformly distributed ( Figure 2 (b, 2g, 2h, 2i, 2j, 2k, 2l) The results further demonstrate that the ZIF-67 / MXene composite material was successfully synthesized.

[0059] Furthermore, the ZIF-67 / MXene composite material prepared in Example 1 and the Ti3C2T composite material prepared in Comparative Example 1 were compared. x The powder material and the ZIF-67 material prepared in Comparative Example 2 were subjected to XRD tests, and the results are as follows: Figure 3 As shown.

[0060] from Figure 3 It can be seen that the ZIF-67 / MXene composite material contains both Ti3C2T. x The characteristic peaks of the powder material and the ZIF-67 material further indicate that the ZIF-67 / MXene composite material was successfully synthesized.

[0061] Furthermore, the ZIF-67 / MXene composite material prepared in Example 1 and the Ti3C2T composite material prepared in Comparative Example 1 were compared. xXPS tests were performed on the powder material and the ZIF-67 material prepared in Comparative Example 2. The results are as follows: Figure 4 As shown.

[0062] from Figure 4 As can be seen from the data, in the Ti 2p XPS spectrum, the Ti-O bond binding energy peak intensity of the composite material is significantly increased compared to pure MXene, indicating that ZIF-67 has undergone chemical bonding with MXene through Ti-O bonds; in the Co 2p XPS spectrum, compared to pure ZIF-67, the Co binding energy in the composite material shifts to a higher energy region (positive shift), or in other words, the Co 2p binding energy of ZIF-67 shows a negative shift relative to the composite material. Figure 4 (a, 4b, 4c, 4d, 4e, 4f); The results show that electrons transferred from ZIF-67 (semiconductor) to the more electronegative Ti3C2T. x On (metal-like conductors), this electron transfer confirms the formation of a Schottky junction, which effectively reduces the interfacial electron transport resistance and enhances the conductivity and catalytic activity of the material.

[0063] Example 2: Biocompatibility and Cell Migration Promotion Properties of ZIF-67 / MXene Composite Material In this embodiment, the aim is to determine the biocompatibility and cell migration-promoting properties of the ZIF-67 / MXene composite material.

[0064] 2.1 Cytotoxicity test The toxicity of ZIF-67 / MXene composite materials at different concentrations (0, 10, 20, 50, 100, 200, 500, 1000, 2000 μg / mL) to L929 mouse fibroblasts after 24 h of culture was detected using the CCK-8 assay. The results are as follows: Figure 5 As shown.

[0065] from Figure 5 As can be seen, the cell survival rate of the ZIF-67 / MXene composite material is above 80% in the concentration range of 0-50 μg / mL, indicating that the ZIF-67 / MXene composite material has low toxicity and good biocompatibility.

[0066] 2.2 Cell migration experiment The optimal healing-promoting concentration of the ZIF-67 / MXene composite material was determined through scratch testing.

[0067] Specifically, it includes the following steps: 1) Take L929 cells that are in the logarithmic growth phase and are in good growth condition, and use 5 × 10⁻⁶ cells per cell. 5 Cells / well were seeded into 6-well cell culture plates and incubated overnight at 37°C in a 5% CO2 incubator. 2) The cells were treated according to the following grouping: Group 1: Blank control group (Control); Group 2: Low concentration treatment group (20 μg / mL ZIF-67 / MXene composite material); Group 3: Medium concentration treatment group (100 μg / mL ZIF-67 / MXene composite material); Group 4: High concentration treatment group (500 μg / mL ZIF-67 / MXene composite material); Group 5: Blank control group + NIR; Group 6: Low concentration treatment group (20 μg / mL ZIF-67 / MXene composite material) + NIR; Group 7: Medium concentration treatment group (100 μg / mL ZIF-67 / MXene composite material) + NIR; Group 8: High-concentration treatment group (500 μg / mL ZIF-67 / MXene composite material) + NIR; The irradiation dose for NIR was: 808 nm laser (1.25 W / cm²). 2 Irradiate for 10 minutes and co-treat with cells for 24 hours.

[0068] 3) After the required time for cell processing, trypsin digests and collects the cells separately; 4) Using a ruler, draw even horizontal lines across the holes on the back of the 6-hole board with a marker pen. 5) With 1×10 6 Cells / well were seeded into 6-well cell culture plates and incubated overnight at 37°C and 5% CO2 saturated humidity. 6) Once the cell density reaches 90% or more, spread the cells to cover the bottom of the 6-well plate. Use a pipette tip to align with a ruler and make a vertical cut along the horizontal line on the back of the plate. The pipette tip should be vertical and not tilted. 7) Wash cells three times with PBS to remove any skimmed cells, add serum-free medium, and take a 0h photograph. Incubate at 37℃ in a 5% CO2 incubator, take a photograph after 24 hours, and calculate migration ability. The results are as follows: Figure 6 As shown.

[0069] from Figure 6 As can be seen, the ZIF-67 / MXene composite material exhibits the best healing-promoting effect when its concentration is 20 μg / mL.

[0070] Example 3: In vitro anti-infection application test of ZIF-67 / MXene composite material In this embodiment, the antibacterial effect of ZIF-67 / MXene composite material against Staphylococcus aureus ATCC43300 under different treatment conditions was tested.

[0071] Specifically, the following grouped experiments were conducted: Group 1: Normal flora control group (Control); Group 2: H2O2 treatment group (H2O2); Group 3: ZIF-67 / MXene composite material treatment group (MXM); Group 4: H2O2+ZIF-67 / MXene composite material treatment group (MXM / H2O2); Group 5: Normal bacteria control group + NIR laser irradiation treatment group; Group 6: H2O2 treatment + NIR laser irradiation treatment group; Group 7: ZIF-67 / MXene composite material treatment + NIR laser irradiation treatment group; Group 8: H2O2 treatment + ZIF-67 / MXene composite material treatment + NIR laser irradiation treatment group; In the above different treatment groups, the final bacterial concentration was 1×10⁻⁶. 8 CFU / ml, final H2O2 concentration of 100 μM, final ZIF-67 / MXene composite material concentration of 20 μg / ml; NIR laser treatment conditions: treatment distance 5 cm, spot diameter 16 mm; after drug addition, the NIR laser-treated group was first laser-treated for 10 min, then incubated at 37℃ for 4 h, followed by fluorescence staining and scanning electron microscopy observation. The results are as follows: Figure 7 As shown.

[0072] from Figure 7 As can be seen, the survival status of Staphylococcus aureus changed significantly after combined treatment with ZIF-67 / MXene composite material, H2O2, and NIR. Specifically, the number of viable bacteria labeled with SYTO 9 green fluorescent markers decreased significantly, while the number of dead bacteria labeled with PI red fluorescent markers increased significantly. In the Merge image, red signals dominated. Compared with the untreated control group, the proportion of viable bacteria in the combined treatment group decreased significantly, while the proportion of dead bacteria increased significantly, indicating that this combined treatment strategy has a strong killing effect on Staphylococcus aureus. Figure 7 a); The ZIF-67 / MXene composite material combined with H2O2 and NIR laser irradiation (i.e., photothermal-chemokinetic synergistic therapy) can severely disrupt the cell wall / membrane structure of Staphylococcus aureus, leading to bacterial lysis and death. The bactericidal effect of the combined treatment group was significantly better than any single combination treatment, consistent with the results of live and dead staining, further verifying the high efficiency of this composite material in synergistic antibacterial activity. Figure 7 b).

[0073] Example 4: In vivo anti-infection and wound healing application tests of ZIF-67 / MXene composite material In this embodiment, using mouse skin infection as a model, the anti-infection and wound healing effects of the ZIF-67 / MXene composite material were studied.

[0074] Specifically, it includes the following steps (see experimental diagram). Figure 8 a): 1) Model construction and treatment grouping A full-thickness skin defect model with a diameter of 2 cm was established on the mouse back, and the mouse was inoculated with MRSA bacterial solution (100 μL, 1×10⁻⁶). 8 An infection model was constructed using CFU / mL; then the mice were randomly divided into the following eight groups: Group 1: Control Group; Group 2: H2O2 treatment group (H2O2); Group 3: ZIF-67 / MXene composite material treatment group (MXM); Group 4: H2O2 treatment + ZIF-67 / MXene composite material treatment group (MXM / H2O2); Group 5: Control group + NIR laser irradiation treatment group; Group 6: ZIF-67 / MXene composite material treatment + NIR laser irradiation treatment group; Group 7: H2O2 treatment + ZIF-67 / MXene composite material treatment + NIR laser irradiation treatment group; Group 8: ZIF-67 / MXene composite material treatment + H2O2 treatment + NIR laser irradiation treatment group (synergistic treatment group).

[0075] 2) Treatment process In the different treatment groups mentioned above, 50 μL of H2O2 (1.5 mM) was dripped and applied to the mouse wounds; 50 μL of ZIF-67 / MXene composite material (20 μg / ml) was added. For the NIR laser irradiation treatment group, an 808 nm laser with a power density of 0.84 W / cm² was used. 2 The irradiation time is 10 minutes.

[0076] Test results as follows Figure 8 As shown.

[0077] from Figure 8 As can be seen, under NIR laser irradiation, the wound surface temperature in the synergistic treatment group rapidly rose to approximately 50°C within 10 minutes, while the control group showed no significant temperature increase. Figure 8f); The healing rate on day 7 showed that under NIR laser irradiation, the healing rate of the synergistic treatment group reached 81.5%, significantly higher than that of the control group and the single treatment group; furthermore, the synergistic treatment group formed dry scabs on day 3 with no purulent exudation; and the newly formed epidermis was smooth on day 7 with no obvious scars. Figure 8 b, 8c, 8e); In addition, in each treatment group, the control group mice showed weight fluctuations or growth retardation, which was likely attributed to systemic stress and inflammation caused by persistent infection. In contrast, under NIR laser irradiation, the mice in the synergistic treatment group showed stable weight gain, comparable to the growth trend of healthy mice. Figure 8 (d) This result indicates that the systemic toxicity caused by the ZIF-67 / MXene composite material is negligible and can effectively reduce the physiological burden caused by infection, demonstrating good biosafety.

[0078] Furthermore, immunofluorescence assays were performed on mice in different treatment groups 7 days after the above treatment, and the results are as follows: Figure 9 As shown.

[0079] from Figure 9 As can be seen, compared with the control group and other treatment groups, the expression of CD31 (angiogenesis marker), Ki67 (proliferation marker), and TGF-β (tissue remodeling factor) was significantly enhanced in the synergistic treatment group under NIR laser irradiation. Figure 9 (a, 9b, 9c, 9d, 9e, 9f) The results show that the ZIF-67 / MXene composite material promotes wound healing by promoting angiogenesis, cell proliferation, and optimizing tissue remodeling.

[0080] Furthermore, H&E staining was performed on different tissues of mice in different treatment groups 7 days after the above treatment, and the results are as follows: Figure 10 As shown.

[0081] from Figure 10 As can be seen, compared with the control group, the pathological abnormalities or inflammatory lesions in the synergistic treatment group under NIR laser irradiation are negligible, indicating that the composite material has good biocompatibility.

[0082] In summary, this invention is based on an electrostatic self-assembly and in-situ growth strategy, utilizing two-dimensional MXene (Ti3C2T). xThe abundant endogenous functional groups (-F, -OH, -O, etc.) on the surface of the material serve as "anchoring sites" for metal ions, inducing ZIF-67 crystals to nucleate and grow uniformly in situ between and on the surface of MXene layers. This results in the formation of a Schottky junction heterostructure with a clean interface, effectively reducing the Schottky barrier, significantly lowering the interfacial electron transfer resistance, and substantially improving the conductivity of the ZIF-67 / MXene composite material. In addition, this ZIF-67 / MXene composite material exhibits photothermal, chemodynamic, and synergistic antibacterial properties as well as the ability to promote wound healing.

[0083] It should be noted that all the above embodiments belong to the same inventive concept, and the descriptions of each embodiment have different focuses. Where the description in a particular embodiment is not detailed, please refer to the description in other embodiments.

[0084] The embodiments described above are merely illustrative of implementation methods of the present invention, and while the descriptions are specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this invention patent should be determined by the appended claims.

Claims

1. A method for preparing ZIF-67 / MXene composite material based on Schottky junction, characterized in that, Includes the following steps: Ti3AlC2 powder, lithium fluoride, and acid solution were mixed and reacted. The resulting product was ultrasonically treated, then washed, centrifuged, and freeze-dried to obtain Ti3C2T. x powder; The Ti3C2T x The powder was dispersed in an organic solvent, then cobalt salt was added, and after ultrasonic treatment, the first solution was obtained; 2-Methylimidazole was dissolved in an organic solvent to obtain a second solution; After the first solution was added to the second solution, the mixture was allowed to stand for reaction. After the reaction was completed, the mixture was filtered, washed, and freeze-dried to obtain the ZIF-67 / MXene composite material.

2. The preparation method according to claim 1, characterized in that, In the step of reacting Ti3AlC2 powder, lithium fluoride and acid solution, the mass ratio of Ti3AlC2 powder to lithium fluoride is 1:(1-2), and the mass-volume ratio of Ti3AlC2 powder to acid solution is 1g:(15-25mL).

3. The preparation method according to claim 1, characterized in that, In the step of reacting Ti3AlC2 powder, lithium fluoride and acid solution, the concentration of the acid solution is 7-12M, and the acid solution includes hydrochloric acid; The reaction specifically includes: reacting at room temperature for 10-15 hours.

4. The preparation method according to claim 1, characterized in that, In the process of mixing Ti3AlC2 powder, lithium fluoride and acid solution and reacting them, the resulting product is subjected to ultrasonic treatment, followed by washing, centrifugation and freeze drying. The ultrasonic treatment time is 6-12 hours. The cleaning process specifically includes cleaning until the pH of the supernatant is 5-6.

5. The preparation method according to claim 1, characterized in that, In the step of obtaining the first solution, the Ti3C2T in the first solution... x The concentration of the powder is 2-3 mg / mL, and the concentration of the cobalt salt is 0.01-0.04 mmol / mL.

6. The preparation method according to claim 1, characterized in that, In the step of obtaining the first solution, the organic solvent includes methanol; Cobalt salts include cobalt nitrate hexahydrate; The ultrasonic treatment time is 5-15 minutes.

7. The preparation method according to claim 1, characterized in that, In the step of obtaining the second solution, the concentration of 2-methylimidazole in the second solution is 0.1-0.3 mmol / mL; Organic solvents include methanol.

8. The preparation method according to claim 1, characterized in that, In the step of adding the first solution to the second solution and allowing the reaction to stand, the volume ratio of the first solution to the second solution is (0.5-1.5):(0.5-1.5). The static reaction time is 20-30 hours.

9. A ZIF-67 / MXene composite material based on a Schottky junction, characterized in that, It is prepared by the preparation method according to any one of claims 1-8.

10. The use of the ZIF-67 / MXene composite material based on a Schottky junction as described in claim 9 in at least one of the following: A1) Preparation of drugs with synergistic photothermal and chemodynamic antibacterial effects; A2) Prepare drugs that promote wound healing.