Steel sheet having excellent formability and method for producing the same

IN606053BActive Publication Date: 2026-10-14JFE STEEL CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
IN2736MUM2011
Authority / Receiving Office
IN · IN
Patent Type
Patents
Current Assignee / Owner
Priority Date
2011-09-12
Filing Date
2011-09-28
Publication Date
2026-10-14
Estimated Expiration
2031-09-28
Patent Text Reader

Abstract

There is provided a steel sheet having excellent workability, which is capable of providing a good formability in actual press forming, wherein the steel has a chemical composition comprising C: not more than 0.01 mass%, Si: not more than 0.2 mass%, Mn: not more than 0.5 mass%, P: not more than 0.04 mass%, S: 0.001 to 0.03 mass%, N: not more than 0.01 mass%, Al: not more than 0.1 mass% and Ti: 0.02 to 0.1 mass% and the remainder being Fe and inevitable impurities, and Ti4 C2 S2 having an average particle size of not less than 10 nm is dispersed into steel at a volume ratio of 0.005 to 0.5%.
Need to check novelty before this filing date? Find Prior Art

Description

FORM 2 THE PATENTS ACT, 1970(39 of 1970) & The Patent Rules, 2003COMPLETE SPECIFICATION1. TITLE OF THE INVENTION:STEEL SHEET HAVING EXCELLENT FORMABILITY AND METHOD FOR PRODUCING THE SAME2. APPLICANT:Name: JFE STEEL CORPORATIONNationality: JapanAddress: 2-3, Uchisaiwai-cho 2-chome, Chiyoda-ku, Tokyo 100-0011 Japan.3. PREAMBLE TO THE DESCRIPTION:The following specification particularly describes the invention and the manner in which it is to be performed: [Technical Field]

[0001] This invention relates to a steel sheet having excellent formability suitable as a material for structural parts of automobile or for structural parts of houses, furniture, desks and the like and a method for producing the same.Moreover, the term “steel sheet” used herein means a cold-rolled and annealed steel sheet having a thickness of not more than 3 mm. [Background Art]

[0002] The steel sheets are used as a material for various structural parts because of good formability. Generally, two-dimensional sheet are press-formed into three-dimensional structural parts , which are joined to each other to form a further complicated three-dimensional structure.

[0003] Conventionally, a low carbon steel sheet containing about 0.03 mass% of C was used in such a steel sheet. In the low carbon steel sheet, the formability was improved by precipitating C as a coarse cementite. However, steel sheets having a better formability become to be required nowadays as the form of the structural parts becomes complicated. As a technique for improving the formability of such steel sheets, since the cementite causes the generation of cracks in the pressed parts of the low carbon steel sheet, it is attempted to reduce the cementite or form no cementite.

[0004] In Patent Document 1 is disclosed a technique wherein the formability and phosphate treatability of the steel sheet are improved by reducing C content to not more than 0.003 mass%, adding Ti and Nb, controlling S content and further determining a finish temperature in hot rolling process depending upon Mn, S, Nb and C contents.In this technique, excellent elongation and r-value can be obtained, though it is hard to say that the press formability is sufficient in the actual press forming.

[0005] In Patent Document 2 is disclosed a steel sheet having anti-secondary work brittleness improved by reducing C content to not more than 0.0025 mass% and refining ferrite grain diameter to not more than 15μm.In this technique, since the elongation of the sheet is low, the sufficient press formability can not be obtained in the actual press forming.

[0006] In Patent Document 3 is disclosed a method to obtain a steel sheet having excellent deep drawability by reducing C content to not more than 0.0030 mass% and adding an optimum amount of Ti depending upon C, N and S contents, and further starting hot rolling without cooling to room temperature after continuous casting and heating a rough rolled bar before finish rolling. In this technique, the r-value and resistance to anti-secondary work brittleness are improved, but the elongation is low and the sufficient press formability is not obtained in the actual press forming.

[0007] In Patent Document 4 is disclosed a steel sheet having good corrosion resistance and formability by reducing C content to not more than 0.0015 mass% and positively adding Al depending upon N content.In this technique, however, the improvement of elongation and r-value in a simple tensile test is achieved, but the satisfactory press formability can not be obtained in the actual press forming. [Prior Art Articles] [Patent Documents]

[0008] [Patent Document 1] Japanese Patent No. 2712986[Patent Document 2] Japanese Patent No. 3807177[Patent Document 3] Japanese Patent No. 3428318[Patent Document 4] Japanese Patent No. 3241429 [Summary of the Invention] [Problems to be solved by the Invention]

[0009] As mentioned above, it is difficult to provide the steel sheets having a good formability in the actual press forming by the conventional techniques.The invention is to advantageously solve the problems of the aforementioned conventional techniques and to provide a steel sheet having excellent press formability in the actual press forming as well as a method for producing the same. [Means for solving problems]

[0010] The elongation by the tensile test is generally used as an index for the press formability of the conventional steel sheet. This elongation means a plastic deformation quantity of a material fractured in the tensile test.However, when the fracture occurs, the products are not obtained. This means that the elongation is not sufficient index for the actual press forming.

[0011] The inventors have made examinations on the deformation behavior of the steel sheet in the actual press forming.Consequently, it has been found out that the formability in the actual press forming is controlled by work hardening behavior.Further, it has been found that it is important to have a high work hardening exponent in the range from 5% to 25%.

[0012] Now, the inventors have made further studies on various factors for providing such work hardening properties.As a result, the following knowledge is obtained:(1) the formability is improved by dispersing coarse Ti4 C2 S2 into steel; and(2) the formability is more improved by combining TiS with Ti4 C2 S2 .

[0013] The invention is accomplished based on the above knowledge, and the summary and construction thereof are as follows:1. A steel sheet having excellent formability, characterized in that the steel has a chemical composition comprising C: not more than 0.01 mass%, Si: not more than 0.2 mass%, Mn: not more than 0.5 mass%, P: not more than 0.04 mass%, S: 0.001 to 0.03 mass%, N: not more than 0.01 mass%, Al: not more than 0.1 mass% and Ti: 0.02 to 0.1 mass% and the remainder being Fe and inevitable impurities, and Ti4 C2 S2 having an average particle size of not less than 10 nm is dispersed into steel at a volume fraction of 0.005 to 0.5%.

[0014] 2. A steel sheet having excellent formability according to the item 1, wherein a part of Ti4 C2 S2 is replaced with a composite sulfide of TiS・Ti4 C2 S2 .

[0015] 3. A steel sheet having excellent formability according to the item 1 or 2, further comprising B: not more than 0.0030 mass%.

[0016] 4. A steel sheet having excellent formability according to any one of the items 1 to 3, further comprising Nb: not more than 0.01 mass%.

[0017] 5. A steel sheet having excellent formability according to any one of the items 1 to 4, further comprising not more than 1 mass% in total of one or more selected from the group consisting of Cu, Sn, Ni, Ca, Mg, Co, As, Cr, Sb, W, Mo, Pb, Ta, REM, V, Cs, Zr and Hf.

[0018] 6. A steel sheet having excellent formability according to any one of the items 1 to 5, wherein a coating layer is provided on the surface of the steel sheet.

[0019] 7. A method for producing a steel sheet as described in any one of the items 1 to 6 by subjecting a steel material having a chemical composition comprising C: not more than 0.01 mass%, Si: not more than 0.2 mass%, Mn: not more than 0.5 mass%, P: not more than 0.04 mass%, S: 0.001 to 0.03 mass%, N: not more than 0.01 mass%, Al: not more than 0.1 mass% and Ti: 0.02 to 0.1 mass% and the remainder being Fe and inevitable impurities to hot rolling, cooling, coiling, pickling, cold rolling and then continuous annealing to form a steel sheet, characterized in that a finish rolling temperature is not lower than 890°C and then the coiling temperature is above 600°C.

[0020] 8. A method for producing a steel sheet as described in the item 7 characterized in that coating treatment is carried out to the steel sheet. [Effect of the Invention]

[0021] According to the invention, it is possible to provide steel sheets havingexcellent press formability considerably improved than that of the conventional onesand to develop remarkable effects in industry.[Embodiments for carrying out the Invention]

[0022] The invention will be described in detail below.First, the reason why the chemical composition of the steel sheet in the invention is limited to the above range will be described. Moreover, % representing the following component means mass% unless otherwise specified.C: not more than 0.01%C is an essential element for generating Ti4 C2 S2 to increase the work hardening exponent of steel. In the invention, it is bonded to Ti and S to form a fine carbosulfide to thereby improve the work hardening exponent of the steel sheet. However, when C content exceeds 0.01%, steel is precipitation-strengthened by TiC and the work hardening exponent is lowered adversely. Therefore, the C content is not more than 0.01%. It is preferably not less than 0.0005% but not more than 0.005%, more preferably not less than 0.0005% but not more than 0.003%.

[0023] Si: not more than 0.2%Si is an element controlling a dislocation state to promote work hardening of ferrite. However, when Si content exceeds 0.2%, solid-solution strengthening of ferrite becomes remarkable, and the work hardening exponent lowers. Therefore, the Si content is not more than 0.2%. Preferably, it is not more than 0.05%.

[0024] Mn: not more than 0.5%Since Mn is a solid-solution strengthening element, it is desirable to be reduced likewise Si in the invention. In order to obtain excellent workability, the Mn content is not more than 0.5%. Preferably, it is not more than 0.30%.

[0025] P: not more than 0.04%Since P is a solid-solution strengthening element, it is desirable to be reduced in the invention. That is, when P content exceeds 0.04%, the solid-solution strengthening becomes remarkable, and the work hardening exponent lowers. Therefore, the P content is not more than 0.04%. Preferably, it is not more than 0.03%.

[0026] S: not less than 0.001% but not more than 0.03%In the invention, S is an important element bonding to Ti to form Ti4 C2 S2 to thereby attain the increase of the work hardening exponent. Therefore, at least 0.001% of S is included in the invention. On the other hand, when the S content exceeds 0.03%, fine TiS becomes large and MnS is precipitated, and hence the workability is deteriorated. In the invention, therefore, the S content is not more than 0.03%. Preferably, it is not more than 0.02%.

[0027] N: not more than 0.01%N forms TiN by bonding to Ti or forms AlN by bonding to Al. When N content exceeds 0.01%, these nitrides are dispersed into ferrite grains to deteriorate the work hardening exponent. Therefore, the N content is not more than 0.01%. Preferably, it is not more than 0.006%.

[0028] Al: not more than 0.1%Al is an element acting as a deoxidizer. In order to obtain this effect, Al is desirable to be included in an amount of not less than 0.001%. When the content exceeds 0.1%, the amount of oxidized inclusion is increased to inhibit the movement of dislocation and deteriorate the work hardening exponent. Therefore, the Al content is not more than 0.1%.

[0029] Ti: not less tan 0.02% but not more than 0.1%Ti is an important element in the invention. That is, Ti forms Ti4 C2 S2 in ferrite grains, whereby the work hardening exponent of the steel sheet is improved. However, when Ti content is less than 0.02%, the amount of Ti4 C2 S2 is too small and the movement of dislocation can not be controlled, and hence the work hardening exponent can not be increased sufficiently. On the other hand, when the Ti content exceeds 0.1%, fine TiC and TiS are precipitated to inhibit the movement of dislocation and deteriorate the work hardening exponent. Therefore, the Ti content is not less than 0.02% but not more than 0.1%.

[0030] Although the above is described with respect to the essential components, the following elements may be properly included in the invention, if necessary.B: not more than 0.0030%B is an element contributing to strengthen grain boundary scavenged by the formation of carbides. However, when B content exceeds 0.0030%, the work hardening exponent is deteriorated by solid-solution strengthening. Therefore, when B is included, the upper limit is 0.0030%.

[0031] Nb: not more than 0.01%Nb is bonded to C to suppress precipitation of cementite into ferrite and improve the formability. However, when it exceeds 0.01%, a greater amount of fine NbC is produced to increase yield strength and deteriorate the work hardening exponent by ferrite grain refinement and precipitation-strengthening. Therefore, the upper limit is 0.01%.

[0032] One or more selected from Cu, Sn, Ni, Ca, Mg, Co, As, Cr, Sb, W, Mo, Pb, Ta, REM, V, Cs, Zr and Hf: not more than 1% in totalCu, Sn, Ni, Ca, Mg, Co, As, Cr, Sb, W, Mo, Pb, Ta, REM, V, Cs, Zr and Hf are elements useful for improving the corrosion resistance, but if the total content exceeds 1%, there is caused a problem that the work hardening exponent is deteriorated by the increase of yield strength based on the solid-solution strengthening, so that the addition of these elements alone or in a combination of two or more is not more than 1%. Preferably, it is not more than 0.5%.Moreover, the components other than the above are Fe and inevitable impurities.

[0033] Although the above is described to the range of the chemical composition in the steel sheet, in order to obtain an expected effect in the invention, only the adjustment of the chemical composition to the above range is insufficient, and it is important that the kind, size and distribution state of carbosulfide precipitated into steel are controlled to the given ranges.in the invention, it is important to precipitate Ti4 C2S2 having an average particle size of not less than 10 nm. Also, a part of Ti4 C2 S2 may be replaced with a composite carbosulfide of TiS・Ti4 C2 S2 .

[0034] Average particle size of carbosulfide (Ti4 C2 S2 or composite carbosulfide of TiS・Ti4 C2S2 ): not less than 10 nmIn the invention, the size of the carbosulfide precipitating into steel is very important. When the average particle size of the carbosulfide is less than 10 nm, the movement of dislocation is suppressed and the work hardening exponent lowers. Therefore, the average particle size of the carbosulfide is not less than 10 nm. The upper limit of the average particle size of the carbosulfide is not particularly limited, but if it is too large, cracks become to easily generated at the interface between ferrite and carbosulfide and the lowering of the elongation becomes remarkable, so that the upper limit of the average particle size of the carbosulfide is preferable to be about 500 nm.Moreover, the average particle size of the aforementioned Ti-containing carbosulfide means an average particle size obtained by measuring individual particle sizes in 10 areas observed at 100000 magnifications through image analysing with circular approximation.

[0035] Volume fraction of carbosulfide: 0.005-0.5%When the amount of the carbosulfide satisfies 0.005% at a volume fraction, the improvement of the satisfactory work hardening exponent can not be attained, while when it exceeds 0.5%, the precipitation strengthening is caused to increase the strength and deteriorate the work hardening exponent, so that the volume fraction of the carbosulfide is within a range of 0.005% to 0.5% in the invention.Moreover, the volume fraction of the carbosulfide is determined by a replica method conducted in a common electron microscopy, wherein only the precipitates are taken out on a carbon support membrane and the size of each precipitate is measured by using a scanning electron microscope. A volume fraction of the precipitates is calculated by the way that the volume of carbides is divided by an amount of iron dissolved in the replica method.

[0036] The steel sheet of the invention may be provided coating layer on its surface. By forming the coating layer on the surface of the steel sheet is improved the corrosion resistance. As the coating are mentioned, for example, a galvanized coating, an alloyed galvanized coating, an electroplated zinc coating such as Zn-Ni alloy electroplated coating, and so on.

[0037] Next, the invention will be described with respect to the method for producing the steel sheet.In the invention, a slab obtained by a continuous casting is preferably used as a material, which is sequentially subjected to hot rolling, cooling on the run-out-table, coiling, pickling, cold rolling and continuous annealing to form a steel sheet.In the invention, the method of melting the steel material is not particularly limited, and all of the well-known methods using a converter, an induction furnace and an electric furnace and the like are adaptable. Also, the casting method is not particularly limited, but a continuous casting method is preferable. When the slab is hot-rolled, the slab may be reheated in a heating furnace and then subjected to hot rolling, or the slab may be heated for a short time in a heating furnace of not lower than 1250°C for temperature compensation just after casting.

[0038] The thus obtained steel material (slab) is subjected to hot rolling. The hot rolling may consist of rough rolling and finish rolling, or only finish rolling omitting rough rolling. In any case, a finish rolling temperature is important.Finish rolling temperature: not lower than 890°CWhen the finish rolling temperature is lower than 890°C, ferrite grains are extended to deteriorate the work hardening exponent. Therefore, the finish rolling temperature is not lower than 890°C. Moreover, the upper limit of the finish rolling temperature is not particularly limited, but is preferable to be about 1000°C.

[0039] Then, the hot rolled steel sheet is subjected to cooling on the run-out-table and coiling. In this case, the coiling temperature is important.Coiling temperature: higher than 600°CWhen the coiling temperature is not higher than 600°C, Ti4 C2S2 is not precipitated sufficiently, and hence the effect of the invention is not obtained. Therefore, the coiling temperature is higher than 600°C. It is preferably not lower than 620°C, more preferably 640°C. Moreover, the upper limit of the coiling temperature is preferable to be about 760°C.

[0040] Next, the steel sheet is subjected to pickling, cold rolling and continuous annealing, which may be conducted according to the conventionally known method because the conditions of the cold rolling and continuous annealing are not particularly limited.For example, it is preferable that a reduction in the cold rolling is about 40-95% and an annealing temperature in the continuous annealing is about 760-900°C.

[0041] Moreover, the cold rolled steel sheet produced as mentioned above may be subjected to a coating treatment to form a coating layer on the surface of the steel sheet. For example, the surface of the steel sheet may be subjected to a galvanizing treatment to form a galvanized coating, or may be subjected to an alloying treatment after the galvanizing treatment to form a zinc-iron alloyed layer. Besides, a coating layer may be formed by an electroplating such as Zn-Ni alloy or the like. [Examples]

[0042] Example 1A steel slab of 270mm in thickness having a chemical composition shown in Table 1 is prepared by continuous casting. Then, the slab is subjected to finish rolling at a temperature shown in Table 2 and thereafter coiled at a temperature shown in Table 2 to obtain a hot rolled steel sheet with a thickness of 2.8 mm. Next, the steel sheet is pickled to remove scales from the surface and subjected to cold rolling at a rolling reduction of 65% and continuous annealing at a temperature of 780-860°C. Moreover, a part of the steel sheet is dipped in a galvanizing bath (0.1% Al-Zn) of 480°C to form a zinc coating layer in the amount of 45 g / m2 (both surfaces) and thereafter subjected to an alloying treatment at 520°C to obtain an alloyed layer.

[0043] The tensile test is conducted by taking out a test specimen from the steel sheet obtained as mentioned above.Also, the type, average particle size and volume fraction of the carbosulfide are measured as follows.

[0044] (i) Observation of precipitatesA thin foil prepared from the cold rolled steel sheet is observed by a transmission electron microscope (TEM) and a scanning electron microscope (SEM) at 10000-260000 magnifications to determine the type of Ti-containing carbosulfide.Also, the average particle size and volume fraction of the Ti-containing carbosulfide are measured according to the aforementioned methods, respectively.

[0045] (ii) Tensile testA tensile test specimen of JIS No. 5 (JIS Z2201), in which a tension direction is parallel to the rolling direction, is taken out from the steel sheet and subjected to a tensile test according to a method defined in JIS Z2241 to measure a tensile strength. Also, n-value as a work hardening exponent is calculated in the strain range from 0.05 to 0.25.When the n-value is not less than 0.20, the press formability is said to be excellent.The thus obtained results are also shown in Table 2.

[0046] Table 1:Typeof steelABCDEFGHIJKLMN O PQ RST U V Chemic al compo sition ( Mn 0.22 0.22 0.22 0.22 0.22 0.35 0.35 0.35 0.35 0.35 0.15 0.21 0.210.21 0.19 0.190.19 0.190.430.41 0.21 0.18 mass %) Al0.0510.0510.0510.0510.0510.0550.0550.0550.0550.0550.0610.0610.0610.041 0.044 0.0440.044 0.0710.0620.059 0.045 0.051 Remarks C0.00090.00130.00270.00330.02170.00180.00180.00170.00160.00180.00350.00340.00340.0022 0.0028 0.00280.0027 0.00280.00210.0022 0.0018 0.0025 Si0.010.010.010.010.010.050.400.110.110.090.110.090.090.04 0.05 0.050.01 0.010.010.01 0.01 0.02 P0.0110.0110.0110.0110.0110.0110.0150.0150.0150.0210.0120.0080.0080.013 0.007 0.0090.009 0.0080.0090.014 0.011 0.018 S0.0130.0130.0130.0130.0120.0050.0050.0050.0050.0080.0080.0070.0080.008 0.016 0.0170.011 0.0190.0120.012 0.008 0.007 N0.00180.00210.00180.00190.00220.00350.00180.00210.00210.00210.00440.00380.00210.0014 0.0019 0.00320.0032 0.00250.00310.0021 0.0028 0.0028 Ti0.0450.0450.0430.0450.0440.0670.0670.0670.0670.0670.3130.0550.0550.00010.0410.0380.038 0.0490.0490.048 0.041 0.039 B Others - - Acceptable steel - - Acceptable steel - - Acceptable steel - - Acceptable steel - - Comparative steel - - Acceptable steel - - Comparative steel - Nb:0.008 Acceptable steel - - Acceptable steel 0.0003 - Acceptable steel 0.0002 - Comparative steel 0.0003 - Acceptable steel 0.0005 Cu:0.02, Ni:0.04, Sn:0.0010 Acceptable steel - - Comparative steel - Mo:0.02, Cr:0.07 Acceptable steel - As:0.0011, Sb:0.006, Hf:0.0021 Acceptable steel - Co:0.0071, Ca:0.0020 Acceptable steel - V:0.01, Mg:0.0021, W:0.0018 Acceptable steel - Zr:0.09, REM:0.0022, Cs:0.0021 Acceptable steel - Pb:0.007, Ta:0.09 Acceptable steel - Acceptable steel 0.0004 Acceptable steel

[0047] Table 2:No. Type of Hot rolling conditions Carbosulfide precipitated MechanTS(MPa)302 299 308 321 398 303 345 300 311 309 355 301 299 301 298 301 303 298 301 303 305 311 ical properties Remarks steel Finish rolling temperature (°C) Coilingtemperature(°C) Average particle size (nm) Volume fraction (%) Ratio of precipitated carbosulfides every type (%) Work hardening exponent, n-value Ti4C2 S2 Composite carbosulfide of TiS・Ti4C2 S2 1 A 920 660 21 0.02 62 38 0.26 Invention Example2 B 920 660 22 0.03 61 39 0.26 Invention Example3 C 920 660 25 0.05 62 38 0.26 Invention Example4 D 920 660 25 0.07 62 38 0.26 Invention Example5 E 920 590 5 0.43 85 15 0.16 Comparative Example6 F 910 680 31 0.04 100 0 0.23 Invention Example7 G 910 680 33 0.04 100 0 0.19 Comparative Example8 H 910 680 32 0.03 100 0 0.23 Invention Example9 I 910 680 34 0.03 100 0 0.23 Invention Example10 J 910 620 33 0.04 41 59 0.24 Invention Example11 K 820 620 5 0.21 31 69 0.18 Comparative Example12 L 940 620 33 0.19 32 68 0.26 Invention Example13 M 940 700 36 0.22 67 33 0.26 Invention Example14 N 930 700 - - - - 0.18 Comparative Example15 O 930 670 41 0.06 58 42 0.26 Invention Example16 P 890 670 44 0.06 54 46 0.26 Invention Example17 Q 890 670 42 0.05 48 52 0.27 Invention Example18 R 900 670 43 0.06 49 51 0.27 Invention Example19 S 900 670 44 0.04 65 35 0.26 Invention Example20 T 920 670 31 0.04 66 34 0.26 Invention Example21 U 840 640 8 0.04 100 0 0.19 Comparative Example22 V 930 500 7 0.05 100 0 0.18 Comparative Example

[0048] As seen from Table 2, all of the steel sheets obtained according to the invention have the n-value of not less than 0.20 and are excellent in the press formability.

Claims

We claim:

1. A steel sheet having excellent formability, characterized in that the steel has a chemical composition comprising C: not more than 0.01 mass%, Si: not more than 0.2 mass%, Mn: not more than 0.5 mass%, P: not more than 0.04 mass%, S: 0.001 to 0.03 mass%, N: not more than 0.01 mass%, Al: not more than 0.1 mass% and Ti: 0.02 to 0.1 mass% and the remainder being Fe and inevitable impurities, and Ti4 C2 S2 having an average particle size of not less than 10 nm is dispersed into steel at a volume fraction of 0.005 to 0.5%.

2. A steel sheet having excellent formability according to claim 1, wherein a part of Ti4 C2 S2 is replaced with a composite sulfide of TiS・Ti4 C2 S2 .

3. A steel sheet having excellent formability according to claim 1 or 2, further comprising B: not more than 0.0030 mass%.

4. A steel sheet having excellent formability according to any one of claims 1 to 3, further comprising Nb: not more than 0.01 mass%.

5. A steel sheet having excellent formability according to any one of claims 1 to 4, further comprising not more than 1 mass% in total of one or more selected from the group consisting of Cu, Sn, Ni, Ca, Mg, Co, As, Cr, Sb, W, Mo, Pb, Ta, REM, V, Cs, Zr and Hf.

6. A steel sheet having excellent formability according to any one of claims 1 to 5, wherein a coating layer is provided on the surface of the steel sheet.

7. A method for producing a steel sheet as described in any one of claims 1 to 6 by subjecting a steel material having a chemical composition comprising C: not more than 0.01 mass%, Si: not more than 0.2 mass%, Mn: not more than 0.5 mass%, P: not more than 0.04 mass%, S: 0.001 to 0.03 mass%, N: not more than 0.01 mass%, Al: not more than 0.1 mass% and Ti: 0.02 to 0.1 mass% and the remainder being Fe and inevitable impurities to hot rolling, cooling, coiling, pickling, cold rolling and then continuous annealing to form a steel sheet, characterized in that a finish rolling temperature is not lower than 890°C and then the coiling temperature is above 600°C.

8. A method for producing a steel sheet according to claim 7 characterized in that coating treatment is carried out to the steel sheet.